Ultra-high performance composite material and preparation method thereof
By using cement, magnetic fly ash microbeads, modified magnetic mineral particles, bamboo fibers and seaweed extracts in composite materials, combined with the use of fiber webs, the problem of insufficient mechanical properties of existing concrete materials is solved, and the problem of achieving the goal of achieving Ultra-high performance composite materials with high compression, tensile and flexural strength.
Patent Information
- Application Number
- CN202411090296.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Existing concrete materials have shortcomings in the compressive strength, tensile strength and impact resistance of national defense doors and civil defense doors, resulting in low mechanical properties.
Using an ultra-high performance composite material, including cement, magnetic fly ash microbeads, modified magnetic mineral particles, bamboo fibers, seaweed extracts and fiber webs, the compressive strength of the material is improved through specific preparation methods. Tensile strength and flexural strength.
The mechanical properties of composite materials are significantly improved, including flexural strength, compressive strength and tensile strength, extend the service life, and enhance fire-proof and flame-retardant performance, solving the problem of lower performance in the prior art.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to an ultra-high performance composite material and a preparation method thereof. Background Art
[0002] Civil defense doors are the doors at the entrances and exits of people's defense projects and are civil defense protection equipment. National defense doors are similar to civil defense doors, but there are certain differences in specific thickness and structure; both are mainly reinforced concrete composite structures and steel structures, which have a certain role in preventing shock waves and effectively ensure the safety and stability of the interior of the civil defense space.
[0003] At present, when preparing national defense doors and civil defense doors, concrete is often filled in the steel structure, and the concrete is prepared by taking advantage of its good durability and excellent comprehensive performance to facilitate the stable use of national defense doors and civil defense doors. However, due to the limitations of existing concrete materials, civil defense doors are still lacking in mechanical properties such as compressive strength, tensile strength and impact resistance. Therefore, an ultra-high performance composite material is urgently needed to solve the above problems. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide an ultra-high performance composite material and a preparation method thereof, which has excellent mechanical properties such as compressive strength, flexural strength, tensile strength, corrosion resistance, and high toughness, and effectively solves the problem of low compressive strength and tensile strength in the existing technical materials.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: an ultra-high performance composite material is provided, comprising the following components in parts by weight: 22-27 parts of cement, 5-7 parts of magnetic fly ash microbeads, 5-7 parts of slag powder, 2-5 parts of modified magnetic mineral particles, 40-43 parts of sand, 0.4-2 parts of bamboo fiber, 0.5-2 parts of seaweed extract, 0.9-1.3 parts of water reducer, 0.02-0.04 parts of defoamer, 1-60 parts of fiber mesh and 0.3-2 parts of water.
[0006] Furthermore, the ultra-high performance composite material includes the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand, 0.6 parts of bamboo fiber, 1.2 parts of seaweed extract, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0007] Furthermore, magnetic fly ash microspheres are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, then baking soda solution is added and spherical granulation is performed, and after drying, the mixture is calcined at 100-120°C, 500-600°C and 1000-1100°C for 20-40 minutes respectively, and after cooling, the mixture is magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0008] Further, the concentration of the baking soda solution is 3 wt %, and the amount of baking soda added is 20 wt % of the fly ash.
[0009] Furthermore, modified magnetic mineral particles are prepared by the following method: mixing ferroferric oxide magnetic nanoparticles with water, ethanol and ammonia water, adding tetraethyl orthosilicate and placing in a constant temperature water bath at room temperature to obtain an intermediate product; then mixing the intermediate product with ethanol and ammonia water, stirring in a water bath at room temperature; then adding a silane surface modifier and an organic solvent and stirring for 24 hours, and magnetic separation to obtain modified magnetic mineral particles.
[0010] Furthermore, the mass volume ratio of ferrosoferric oxide magnetic nanoparticles, tetraethyl orthosilicate, water, ethanol and ammonia water is 200 mg: 200 μL: 10-30 mL: 180-200 mL: 4-6 mL.
[0011] Furthermore, the mass volume ratio of ferrosoferric oxide magnetic nanoparticles and tetraethyl orthosilicate is 200 mg:200 μL.
[0012] Furthermore, the volume ratio of ethanol and ammonia water to the silane surface modifier and the organic solvent added for the second time was 50:0.5:4:2.
[0013] Furthermore, the silane surface modifier is KH-550, KH-560 or KH570; and the organic solvent is dichloromethane.
[0014] Furthermore, the seaweed extract is prepared by the following method: crushing the seaweed and placing it in water at a solid-liquid ratio of 1:30, extracting at 100°C for 2 hours, and filtering to obtain a filtrate and a residue; placing the residue in 90-95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extracting at 100-300W and 80°C for 0.5h, filtering to obtain a filtrate; combining the filtrates, and then successively concentrating and drying to obtain a seaweed extract.
[0015] Furthermore, the average particle size of the modified magnetic mineral particles is less than 3µm and the specific surface area is greater than 3000m 2 / kg, activity index is greater than 100%.
[0016] Furthermore, the fiber mesh is a metal fiber mesh, an inorganic non-metal fiber mesh or an organic fiber mesh.
[0017] Furthermore, the metal fiber mesh is a steel fiber mesh; the inorganic non-metal fiber mesh is at least one of a basalt fiber mesh, a carbon fiber mesh and a glass fiber mesh; and the organic fiber mesh is at least one of an ultra-high molecular weight polyethylene fiber mesh and a Kevlar fiber mesh.
[0018] Furthermore, the fiber web is a two-dimensional fiber web and / or a three-dimensional fiber web; the shape of the fiber filaments in the fiber web is at least one of a straight line, a wave, a spiral, a twist, and a convex point.
[0019] Furthermore, the diameter of the fiber filaments in the fiber net is ≤2 mm, the tensile strength of the fiber filaments is ≥500 MPa, and the fiber mesh spacing is ≤30 mm.
[0020] Furthermore, the specific surface area of slag powder is greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0021] Furthermore, the particle size of the magnetic fly ash microbeads is 0.07-0.2 mm.
[0022] Furthermore, the sand is at least one of river sand, machine-made sand and quartz sand; and the sand particle size is less than 4 mm.
[0023] Furthermore, the bamboo fiber has a length of 2-4 cm and a diameter of 0.2-0.4 mm.
[0024] Furthermore, the water reducing agent is a polycarboxylic acid water reducing agent with a water reducing rate of ≥30%, including powder or liquid.
[0025] The present invention also provides a method for preparing the ultra-high performance composite material, comprising the following steps:
[0026] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0027] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0028] The present invention has the following beneficial effects:
[0029] 1. The present invention uses a fiber mesh in the composite material, which connects and reinforces cementitious components such as cement, slag powder and sand, thereby improving the integrity of the composite material and enhancing the flexural strength and tensile strength of the composite material; and magnetic substances such as magnetic fly ash microbeads and modified magnetic mineral particles are added to the cementitious material in contact with the fiber mesh, and the magnetic substances are adsorbed on the ultra-high strength steel fiber mesh, which enhances the pull-out force of each fiber filament of the steel fiber mesh, and further enhances the compressive strength, compressive strength and flexural strength and other properties of the composite material.
[0030] 2. The present invention modifies the magnetic mineral particles. The surface of the ferroferric oxide magnetic nanoparticles is coated with silicon dioxide, and then a silane surface modifier is added for modification. The obtained modified magnetic mineral particles have better stability and dispersibility. When used in the composite material of the present invention, uniform dispersion can be achieved, and problems such as agglomeration of magnetic substances directly added in the composite material can be avoided; the strength and other mechanical properties of the composite material are effectively improved.
[0031] 3. In the magnetic fly ash microbeads, iron oxide and ferric oxide contained in fly ash are both used as magnetic materials, and baking soda will decompose to produce carbon dioxide gas during staged calcination, so that the magnetic fly ash microbeads will produce a large number of pores while filling the magnetic material, increasing the roughness and specific surface area of the microbeads, thereby increasing the contact area between the microbeads and other components in the composite material. Even bamboo fibers can be partially interspersed in the pores of the microbeads, enhancing the bonding force between the magnetic fly ash microbeads and other components, thereby enhancing the mechanical properties of the composite material such as compressive strength.
[0032] 4. The addition of bamboo fiber enhances the bonding with cement, slag powder, sand and other cementitious materials in the composite material, and the bonding between the components is tighter, which can greatly improve the bending and tensile properties of the composite material and extend the service life of the composite material. The use of seaweed extract promotes the dispersion of bamboo fiber in the composite material and the bonding with the components, enhances the structural strength, and also makes the composite material have better fire retardant properties, improving the comprehensive performance of the composite material. DETAILED DESCRIPTION
[0033] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0034] Example 1
[0035] An ultra-high performance composite material comprises the following components in parts by weight: 22 parts of cement, 5 parts of magnetic fly ash microbeads, 5 parts of slag powder, 2 parts of modified magnetic mineral particles, 40 parts of sand (river sand), 0.4 parts of bamboo fiber, 0.5 parts of seaweed extract, 0.9 parts of water reducer, 0.02 parts of defoamer, 3 parts of fiber mesh (steel fiber mesh) and 0.3 parts of water.
[0036] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 500°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0037] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 200 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of a silane surface modifier (KH-550) and 2 mL of an organic solvent (dichloromethane) were added and stirred for 24 h, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0038] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0039] The fiber diameter in the fiber mesh is 1mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 2mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The bamboo fiber is 3cm long and 0.3mm in diameter. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0040] The method for preparing the ultra-high performance composite material comprises the following steps:
[0041] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0042] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0043] Example 2
[0044] An ultra-high performance composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand (river sand), 0.6 parts of bamboo fiber, 1.2 parts of seaweed extract, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0045] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 550°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0046] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 190 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0047] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0048] The fiber diameter in the fiber mesh is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 5mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The bamboo fiber length is 3cm and the diameter is 0.3mm. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0049] The method for preparing the ultra-high performance composite material comprises the following steps:
[0050] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0051] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0052] Example 3
[0053] An ultra-high performance composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 4 parts of modified magnetic mineral particles, 43 parts of sand (quartz sand), 0.7 parts of bamboo fiber, 1 part of seaweed extract, 1.2 parts of water reducer, 0.03 parts of defoamer, 9 parts of fiber mesh (steel fiber mesh) and 1 part of water.
[0054] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 600°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0055] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 190 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0056] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0057] The fiber diameter in the fiber mesh is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 4mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The bamboo fiber length is 3cm and the diameter is 0.3mm. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0058] The method for preparing the ultra-high performance composite material comprises the following steps:
[0059] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0060] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0061] Example 4
[0062] An ultra-high performance composite material comprises the following components in parts by weight: 27 parts of cement, 7 parts of magnetic fly ash microbeads, 7 parts of slag powder, 5 parts of modified magnetic mineral particles, 43 parts of sand (machine-made sand), 2 parts of bamboo fiber, 2 parts of seaweed extract, 1.3 parts of water reducer, 0.04 parts of defoamer, 15 parts of fiber mesh (steel fiber mesh) and 2 parts of water.
[0063] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 600°C and 1100°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0064] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 30 mL of water, 200 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0065] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0066] The fiber diameter in the fiber mesh is 1.5mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 15mm. The particle size of the magnetic fly ash microbeads is 0.2mm. The bamboo fiber is 3cm long and 0.3mm in diameter. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0067] The method for preparing the ultra-high performance composite material comprises the following steps:
[0068] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0069] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0070] Comparative Example 1
[0071] A composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand (river sand), 0.6 parts of bamboo fiber, 1.2 parts of seaweed extract, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0072] Among them, the modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 190 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water, and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0073] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0074] The fiber diameter in the fiber net is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 5mm. The bamboo fiber length is 3cm and the diameter is 0.3mm. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0075] The method for preparing the composite material comprises the following steps:
[0076] (1) Cement, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water are added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0077] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0078] Comparative Example 2
[0079] A composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 42 parts of sand (river sand), 0.6 parts of bamboo fiber, 1.2 parts of seaweed extract, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0080] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 550°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0081] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0082] The fiber diameter in the fiber mesh is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 5mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The bamboo fiber length is 3cm and the diameter is 0.3mm. The specific surface area of slag powder is greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0083] The method for preparing the composite material comprises the following steps:
[0084] (1) Cement, magnetic fly ash microbeads, sand, bamboo fiber, seaweed extract, water reducing agent and defoaming agent are stirred and mixed, and then four fifths of water is added and stirred until it becomes viscous, and then the remaining water is added and stirred to obtain a mixed material;
[0085] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0086] Comparative Example 3
[0087] A composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand (river sand), 0.6 parts of bamboo fiber, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0088] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 550°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0089] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 190 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0090] The fiber diameter in the fiber mesh is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 5mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The bamboo fiber length is 3cm and the diameter is 0.3mm. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0091] The method for preparing the composite material comprises the following steps:
[0092] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0093] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0094] Comparative Example 4
[0095] A composite material comprises the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand (river sand), 1.2 parts of seaweed extract, 1.1 parts of water reducing agent, 0.03 parts of defoaming agent, 10 parts of fiber mesh and 1 part of water.
[0096] Among them, magnetic fly ash microbeads are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, and then 3wt% baking soda solution is added and spherical granulation is performed, the amount of baking soda added is 20wt% of the fly ash, and after drying, they are calcined at 110°C, 550°C and 1000°C for 30 minutes respectively, and after cooling, they are magnetized in a magnetic field to obtain magnetic fly ash microspheres.
[0097] The modified magnetic mineral particles were prepared by the following method: 200 mg of ferroferric oxide magnetic nanoparticles were mixed with 20 mL of water, 190 mL of ethanol and 5 mL of ammonia water, 200 μL of tetraethyl orthosilicate was added and the mixture was kept in a constant temperature water bath at room temperature to obtain an intermediate product; the intermediate product was then mixed with 50 mL of ethanol and 0.5 mL of ammonia water and stirred in a water bath at room temperature; 4 mL of silane surface modifier (KH-550) and 2 mL of organic solvent (dichloromethane) were added and stirred for 24 hours, and magnetic separation was performed to obtain modified magnetic mineral particles.
[0098] The seaweed extract is prepared by the following method: crush the seaweed and place it in water at a solid-liquid ratio of 1:30, extract it at 100°C for 2 hours, and filter to obtain a filtrate and a residue; place the residue in 95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extract it at 200W and 80°C for 0.5h, filter to obtain a filtrate; combine the filtrates, and then concentrate and dry them in turn to obtain the seaweed extract.
[0099] The fiber diameter in the fiber mesh is 1.2mm, the tensile strength of the fiber is ≥500MPa, and the fiber mesh spacing is 5mm. The particle size of the magnetic fly ash microbeads is 0.1mm. The average particle size of the modified magnetic mineral particles is less than 3µm, and the specific surface area is greater than 3000m 2 / kg, activity index greater than 100%. Slag powder specific surface area greater than 800m 2 / kg, D90≤15µm, activity index greater than 120%.
[0100] The method for preparing the composite material comprises the following steps:
[0101] (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material;
[0102] (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
[0103] The composite materials obtained in Examples 1-4 and Comparative Examples 1-4 are now subjected to mechanical property tests, with reference to the test standard: GB / T 50081. The results are shown in Table 1.
[0104] Table 1 Mechanical properties test results
[0105]
[0106] As can be seen from Table 1, the flexural strength, compressive strength, initial crack tensile strength and ultimate tensile strength of the ultra-high performance composite materials of Examples 1-4 are all higher than those of Comparative Examples 1-4; that is, the ultra-high performance composite materials of the present invention have excellent mechanical properties, effectively solving the problem of poor compressive strength and tensile strength in the prior art. And the composite materials of Comparative Examples 1-4 illustrate that the magnetic fly ash microbeads, modified magnetic mineral particles, bamboo fiber and seaweed extract in the ultra-high performance composite materials of the present invention all play an important role, and the combination of the several effectively enhances the compressive strength, compressive strength and flexural strength and other properties of the composite materials.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An ultra-high performance composite material, characterized in that: It is made of the following components in parts by weight: 22-27 parts of cement, 5-7 parts of magnetic fly ash microbeads, 5-7 parts of slag powder, 2-5 parts of modified magnetic mineral particles, 40-43 parts of sand, 0.4-2 parts of bamboo fiber, 0.5-2 parts of seaweed extract, 0.9-1.3 parts of water reducer, 0.02-0.04 parts of defoamer, 1-60 parts of fiber mesh and 0.3-2 parts of water; the fiber mesh is a metal fiber mesh; The magnetic fly ash microspheres are prepared by the following method: fly ash, clay powder, carbon powder and iron oxide powder are mixed in a mass ratio of 70:25:20:8, then baking soda solution is added and spherical granulation is performed, and after drying, the mixture is calcined at 100-120° C., 500-600° C. and 1000-1100° C. for 20-40 min, respectively, and after cooling, magnetized in a magnetic field to obtain magnetic fly ash microspheres; The modified magnetic mineral particles are prepared by the following method: mixing ferroferric oxide magnetic nanoparticles with water, ethanol and ammonia water, adding tetraethyl orthosilicate and then placing in a constant temperature water bath at room temperature to obtain an intermediate product; then mixing the intermediate product with ethanol and ammonia water, stirring in a water bath at room temperature; then adding a silane surface modifier and an organic solvent and stirring for 24 hours, and magnetically separating to obtain the modified magnetic mineral particles; The seaweed extract is prepared by the following method: crushing the seaweed and placing it in water at a solid-liquid ratio of 1:30, extracting at 100°C for 2h, filtering to obtain a filtrate and a filter residue; placing the filter residue in 90-95vt% ethanol at a solid-liquid ratio of 1:1, ultrasonically extracting at 100-300W and 80°C for 0.5h, filtering to obtain a filtrate; combining the filtrates, and then sequentially concentrating and drying to obtain the seaweed extract.
2. The ultra-high performance composite material according to claim 1, characterized in that: It is made of the following components in parts by weight: 25 parts of cement, 6 parts of magnetic fly ash microbeads, 6 parts of slag powder, 3 parts of modified magnetic mineral particles, 42 parts of sand, 0.6 parts of bamboo fiber, 1.2 parts of seaweed extract, 1.1 parts of water reducer, 0.03 parts of defoamer, 10 parts of fiber mesh and 1 part of water.
3. The ultra-high performance composite material according to claim 1 or 2, characterized in that: The modified magnetic mineral particles have an average particle size of less than 3 μm and a specific surface area of more than 3000 m 2 / kg, activity index is greater than 100%.
4. The ultra-high performance composite material according to claim 1 or 2, characterized in that: The fiber web is a two-dimensional fiber web and / or a three-dimensional fiber web; the shape of the fiber filaments in the fiber web is at least one of a straight line, a wave, a spiral, a twist, and a convex point.
5. The ultra-high performance composite material according to claim 1 or 2, characterized in that: The fiber diameter in the fiber net is ≤2 mm, the tensile strength of the fiber net is ≥500 MPa, and the fiber mesh spacing is ≤30 mm.
6. The method for preparing the ultra-high performance composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Cement, magnetic fly ash microbeads, modified magnetic mineral particles, sand, bamboo fiber, seaweed extract, water reducer and defoamer are mixed and then four fifths of water is added and stirred until a viscous state is reached, and then the remaining water is added and stirred to obtain a mixed material; (2) pouring the mixed material obtained in step (1) into a mold tooling equipped with a fiber mesh, and then removing the mold after curing to obtain an ultra-high performance composite material.
Citation Information
Patent Citations
High crack-resistant performance modified polyester synthetic fiber concrete and preparation method thereof
CN101077834A
Carbon nano-tube fiber cement-based material and preparation thereof
CN101274831A
Antimagnetic veneer
CN103159445A
Extraction method for algal polysaccharide
CN103739726A
Reinforced cement based composite material with fiber woven mesh and preparation method of reinforced cement based composite material
CN103964795A
Cited By
Cement-based composite material civil air defense door machining tool and machining process thereof
CN119928062A
Integrated cementing material special for ultra-high performance concrete and preparation method
CN120736858A