Anionic polymer suitable for river sludge dehydration and preparation method thereof

The anionic polymer addresses poor dehydration effects in river sludge by forming high molecular weight polymers with calcium ions and cyclodextrin structures, improving flocculation and dehydration efficiency and reducing moisture content in filter cakes.

CN118620133BActive Publication Date: 2024-12-03DONGYING BEILU BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103025.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing river sludge dehydration methods face challenges with poor dehydration effects, high moisture content in filter cakes, and substandard discharge of sludge residual water, particularly for sludges with high organic matter and fine particle content.

Method used

An anionic polymer is prepared through copolymerization of propylene sulfonic acid, vinyl sulfonic acid, acrylamide, acrylic acid, and allyl-β-cyclodextrin, incorporating a conditioning agent with calcium ions and polyvinyl alcohol fiber to enhance flocculation and dehydration, forming a high molecular weight polymer with multiple adsorption groups and a cyclodextrin structure for improved floc binding and drainage.

Benefits of technology

The anionic polymer effectively destabilizes suspended matter, reduces viscosity, facilitates floc sinking and filtration, and significantly decreases moisture content in the filter cake, enhancing dehydration efficiency and preventing filter mesh clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to an anionic polymer suitable for river silt dehydration and a preparation method thereof, and belongs to the technical field of polymer compound synthesis. The method is as follows: propylene sulfonic acid, vinyl sulfonic acid, calcium chloride and water are mixed, and the mixed system pH obtained is adjusted to 5~6 with calcium hydroxide, and then nitrogen is passed through to deoxygenate, and then a chain transfer agent, an oxidant and a reducing agent are added to react to obtain a conditioning agent; acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, a conditioning agent, a surfactant and water are mixed, and the mixed solution pH obtained is adjusted to 6~6.5 with calcium hydroxide, and then nitrogen is passed through to deoxygenate, and then a chain transfer agent, a co-initiator, an oxidant and a reducing agent are added to react, and then granulated, dried, ground and sieved to obtain the anionic polymer. The anionic polymer prepared by the present invention has a good dehydration effect, can make the filtrate clear, and the moisture content of the filter cake is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer compound synthesis, and in particular to an anionic polymer suitable for river sludge dehydration and a preparation method thereof. Background Art

[0002] Bottom mud dredging is an important means of controlling endogenous pollution in black and odorous water bodies, and can effectively reduce the total amount of pollutants in the water environment. However, the large amount of sludge produced by bottom mud dredging often has the characteristics of a large proportion of fine particles, high water content, rich organic matter content, and high viscosity, which makes it difficult to dehydrate and dry naturally and difficult to dispose of efficiently. The plate and frame filter press dewatering process relies on mechanical pressurization, which can significantly increase the mud-water separation rate and improve the degree of sludge drying. It is currently widely used in water environment governance projects in my country. Before plate and frame filter press dewatering, the sludge needs to be flocculated to destroy the stable colloidal state of the sludge, promote the discharge of water between the sludge particles, and thus reduce the dehydration resistance.

[0003] Domestic research on dredged sludge mainly focuses on sludge reduction and harmless disposal technology, and sludge dehydration is one of the key steps in sludge reduction treatment technology. In order to improve the dehydration and solidification disposal efficiency of lake and river dredged sludge, a variety of sludge treatment agents have been developed. Ma Tao et al. used FeCl3, alum, polyaluminium chloride (PAC) and polyacrylamide (PAM) to treat river sludge in the "Experimental Study on Optimization of Dehydration Agents for River Sediments of Different Mud Types" and found that the polymer flocculant PAM had the best effect.

[0004] After the dredged sludge is solidified, the water content is required to be reduced to a certain range (usually 40%) to facilitate external disposal or resource utilization. Due to the large volume of sludge dewatering tailwater, it is often discharged into the surrounding natural water bodies. The tailwater quality needs to meet the corresponding discharge standards and not pollute the receiving water bodies. Therefore, when selecting river sludge treatment agents, not only the dehydration effect needs to be considered, but also the water quality of sludge dewatering tailwater and the operating cost of the plate and frame filter press should be considered. Chinese patent application 201010578166.3 discloses a sludge filter bag dewatering method with the addition of a coagulant, wherein the dewatering method is to add a suitable coagulant to the sludge, and then the sludge enters the filter bag for rapid flocculation and precipitation, and the clarified water is pressed out by gravity or water pump pressure, thereby dewatering the sludge; the coagulant is an organic polymer coagulant polyacrylamide; the sludge filter bag dewatering method has a good dewatering effect on sludge with low organic matter content, coarse sludge particles and good water permeability, but the filter bag dewatering method has a long construction period, and requires a large amount of space to be occupied for a long time to stack filter bags, and the treatment of difficult-to-filter sludge in rivers with high mud content and high organic matter content often causes the filter bag aperture to be blocked, resulting in the phenomenon that the sludge cannot be dewatered for a long time.

[0005] In summary, it is very necessary to research and develop an anionic polymer suitable for river sludge dehydration with good dehydration effect, clear filtrate and low filter cake moisture content and a preparation method thereof. Summary of the invention

[0006] In order to solve one or more technical problems existing in the prior art of river sludge dehydration process, such as poor dehydration effect, high moisture content of filter cake, and substandard discharge of sludge residual water, the present invention provides an anionic polymer suitable for river sludge dehydration and a preparation method thereof.

[0007] In a first aspect, the present invention provides a method for preparing an anionic polymer suitable for dehydrating river sludge, the preparation method comprising the following steps:

[0008] (1) Propylene sulfonic acid, vinyl sulfonic acid, calcium chloride and water are uniformly mixed to obtain a mixed system, and then the pH of the mixed system is adjusted to 5-6 with calcium hydroxide, and then nitrogen is passed through the mixed system to remove oxygen, and then a chain transfer agent, an oxidant and a reducing agent are added to react to obtain a conditioning agent;

[0009] (2) acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, a conditioner, a surfactant and water are uniformly mixed to obtain a mixed solution, and then the pH of the mixed solution is adjusted to 6-6.5 with calcium hydroxide, and then nitrogen is passed to remove oxygen, and then a chain transfer agent, a co-initiator, an oxidant and a reducing agent are added to react to obtain a polymer block;

[0010] (3) The polymer blocks are granulated, dried, ground and sieved in sequence to obtain an anionic polymer suitable for river sludge dehydration.

[0011] Preferably, in step (1), the mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is (1.5-2.5):1:(6-8); the amount of calcium hydroxide used is 60-65% of the sum of the mass amounts of propylene sulfonic acid and vinyl sulfonic acid; and / or the amount of calcium chloride used is 35-45% of the sum of the mass amounts of propylene sulfonic acid and vinyl sulfonic acid.

[0012] Preferably, the mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is 2:1:7.

[0013] Preferably, in step (1): the chain transfer agent is dodecyl mercaptan; the oxidizing agent is potassium persulfate; and / or the reducing agent is sodium bisulfite.

[0014] Preferably, in step (1), the amount of the chain transfer agent is 0.2-0.4% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; the amount of the oxidant is 0.3-0.5% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; and / or the amount of the reducing agent is 0.1-0.3% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

[0015] Preferably, in step (1): the initiation temperature of the reaction is 2-5°C; and / or the molecular weight of the conditioning agent is 30,000-100,000.

[0016] Preferably, in step (2): the surfactant is sodium fatty alcohol polyoxyethylene ether sulfate; the chain transfer agent is sodium hypophosphite; the co-initiator is tetramethylethylenediamine; the oxidant is potassium persulfate; and / or the reducing agent is sodium bisulfite.

[0017] Preferably, in step (2), the raw materials used include, by weight, 50-100 parts of acrylamide, 60-120 parts of acrylic acid, 30-50 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10-20 parts of water-soluble polyvinyl alcohol fiber, 10-20 parts of allyl-β-cyclodextrin, 200-400 parts of a conditioner, 3-6 parts of a surfactant, 31-62 parts of calcium hydroxide, 222-606 parts of water, 0.005-0.01 parts of a chain transfer agent, 0.5-2 parts of a co-initiator, 0.005-0.01 parts of an oxidant, and 0.005-0.01 parts of a reducing agent.

[0018] Preferably, in step (2), the initiation temperature of the reaction is 5-10° C.; in step (1) and / or step (2), the time for nitrogen deoxygenation is 20-40 min.

[0019] In a second aspect, the present invention provides an anionic polymer suitable for river sludge dehydration, which is prepared by the preparation method described in the first aspect of the present invention.

[0020] Compared with the prior art, the present invention has at least the following beneficial effects:

[0021] (1) The present invention polymerizes acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid and allyl-β-cyclodextrin through a copolymerization process to form a high molecular anionic polymer having multiple adsorption groups. At the same time, a conditioning agent is introduced into the anionic polymer, so that the anionic polymer has great electrical neutralization ability and sweeping ability when dehydrating river silt, and can quickly destabilize suspended matter to form flocs.

[0022] (2) The conditioning agent in the present invention is a low molecular weight polymer with a high charge. When it is introduced into an anionic polymer, it can quickly break the original equilibrium structure in the sludge and destabilize the sludge suspended matter. At the same time, the conditioning agent contains a large amount of calcium ions. A large amount of divalent electrolyte ions can accelerate the destabilization of the colloid. At the same time, it can act as a coagulant for the colloidal particles in the wastewater and can serve as a particle core weighting agent to accelerate the sedimentation of the suspended matter.

[0023] (3) Although the water-soluble polyvinyl alcohol fiber introduced in the present invention does not participate in the copolymerization reaction, the abundant hydroxyl groups on its surface can interact with polymers, nanoparticles and other small molecules, and play a role of interweaving and entanglement in the polymer chain network. It can act as a skeleton monomer and interweave and entangle with the molecular chains, so that the network structure of the anionic polymer is interspersed with polyvinyl alcohol fibers. The polyvinyl alcohol fiber is like a large skeleton supporting the spatial structure of the copolymer molecular chains. During flocculation, the large skeleton structure can penetrate the entire floc structure and connect different flocs. During the filter press process, a skeleton drainage channel can be constructed, thereby reducing the dehydration resistance and facilitating the removal of free water.

[0024] (4) The anionic polymer prepared by the present invention introduces a cyclodextrin structure into its molecular chain. The structure is a cavity structure with a hydrophobic cavity inside and a hydrophilic surface outside. It also has abundant hydroxyl groups and can achieve floc adsorption through van der Waals force, hydrogen bond Coulomb force and hydrophilic / hydrophobic force, thereby enhancing the binding ability of the anionic polymer and the floc, making the floc compact and more conducive to dehydration.

[0025] (5) The anionic polymer prepared by the present invention has a good dehydration effect. After flocculation and dehydration, the viscosity of the flocs and the supernatant can be reduced, which is conducive to the sinking of the flocs, the clarification of the filtrate, and the compaction of the flocs, which greatly reduces the sludge specific resistance and is not easy to clog the filter mesh. During compression dehydration, there are skeleton channels between the flocs, which helps to increase the filtration speed and can greatly reduce the moisture content of the filter cake. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] In a first aspect, the present invention provides a method for preparing an anionic polymer (abbreviated as anionic polymer) suitable for dehydration of river sludge, the preparation method comprising the following steps:

[0028] (1) Propylene sulfonic acid, vinyl sulfonic acid, calcium chloride and water are uniformly mixed to obtain a mixed system, and then the pH of the mixed system is adjusted to 5-6 with calcium hydroxide, and then nitrogen is passed to remove oxygen, and then a chain transfer agent, an oxidant and a reducing agent are added to react to obtain a conditioning agent; in the present invention, calcium ions are introduced into the conditioning agent, and a high content of divalent ions can promote the destabilization of colloidal particles, and at the same time has the effects of sterilization, replacement of toxic and harmful substances, and promotion of sedimentation;

[0029] (2) acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, a conditioner, a surfactant and water are uniformly mixed to obtain a mixed solution, and then the pH of the mixed solution is adjusted to 6-6.5 with calcium hydroxide, and then nitrogen is passed through the mixed solution to remove oxygen, and then a chain transfer agent, a co-initiator, an oxidant and a reducing agent are added to react to obtain a polymer block; in the present invention, unless otherwise specified, the various substances used can be products that can be directly purchased on the market or synthesized by existing methods; (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid is also introduced into the copolymerization process of the present invention. In addition to the carboxyl group, the (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid monomer can also introduce a sulfonyl structure and a benzimidazole structure. The sulfonyl structure and the benzimidazole structure have strong hydrophilicity and ionicity, and can form adsorption with the microparticles, which is beneficial to enhancing the rigid structure and net capture sweeping area of ​​the anionic polymer;

[0030] (3) The polymer block is granulated, dried, ground and sieved in sequence to obtain an anionic polymer suitable for river sludge dehydration. The present invention does not specifically limit the conditions for the granulation, drying, grinding and sieving, and conventional conditions can be used.

[0031] The invention polymerizes acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid and allyl-β-cyclodextrin through a copolymerization process to form a high molecular anionic polymer with multiple adsorption groups. At the same time, a conditioning agent is introduced into the anionic polymer, so that the anionic polymer has great electrical neutralization ability and sweeping ability when dewatering river sludge, and can quickly destabilize suspended matter to form flocs. The conditioning agent in the invention is a low molecular weight polymer with high charge. When the conditioning agent is introduced into the anionic polymer, the original equilibrium structure in the sludge can be quickly broken to destabilize the sludge suspended matter. At the same time, the conditioning agent contains a large amount of calcium ions and a large amount of divalent electrolyte ions, which can accelerate the destabilization of the colloid. At the same time, the conditioning agent can play a coagulant role on the colloidal particles in the wastewater and can be used as a particle core weighting agent to accelerate the sedimentation of the suspended matter. The water-soluble polyvinyl alcohol fiber of the skeleton monomer introduced in the invention can be intertwined with the molecular chain, so that the network structure of the anionic polymer is interspersed with polyvinyl alcohol. Fiber, polyvinyl alcohol fiber is similar to a large skeleton supporting the spatial structure of connecting copolymer molecular chains. During flocculation, the large skeleton structure can penetrate the entire floc structure and connect different flocs. During the filter pressing process, a skeleton drainage channel can be constructed, thereby reducing the dehydration resistance and facilitating the removal of free water. The anionic polymer prepared by the present invention introduces a cyclodextrin structure into its molecular chain. The structure is a cavity structure with a hydrophobic cavity inside and a hydrophilic surface outside. It also has abundant hydroxyl groups, and can achieve floc adsorption through van der Waals force, hydrogen bond Coulomb force and hydrophilic / hydrophobic force, enhance the binding ability of the anionic polymer and the floc, make the floc compact, and be more conducive to dehydration. The anionic polymer prepared by the present invention has a good dehydration effect. After flocculation and dehydration, the viscosity of the floc and the supernatant can be low, which is conducive to the sinking of the floc, the clarification of the filtrate, the compactness of the floc, the significant reduction of the sludge specific resistance, and the difficulty in clogging the filter mesh. During compression dehydration, there are skeleton channels between the flocs, which helps to increase the filtration speed and can significantly reduce the moisture content of the filter cake.

[0032] According to some preferred embodiments, in step (1), the mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is (1.5-2.5):1:(6-8) (e.g., 1.5:1:6, 1.5:1:7, 1.5:1:8, 2:1:6, 2:1:7, 2:1:8, 2.5:1:6, 2.5:1:7 or 2.5:1:8); in the present invention, preferably, the mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is (1.5-2.5):1:(6-8). The conditioning agent formed in this way can make the anionic polymer have It has better electrical neutralization ability and sweeping ability, can quickly form flocs during river sludge dehydration, and quickly destabilize and settle suspended matter; the amount of calcium hydroxide is 60-65% (for example, 60%, 61%, 62%, 63%, 64% or 65%) of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; and / or the amount of calcium chloride is 35-45% (for example, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44% or 45%) of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

[0033] According to some preferred embodiments, the mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is 2:1:7.

[0034] According to some preferred embodiments, in step (1): the chain transfer agent is dodecyl mercaptan; in the present invention, dodecyl mercaptan refers to n-dodecyl mercaptan; the oxidant is potassium persulfate; and / or the reducing agent is sodium bisulfite.

[0035] According to some preferred embodiments, in step (1): the amount of the chain transfer agent is 0.2-0.4% (e.g., 0.2%, 0.25%, 0.3%, 0.35% or 0.4%) of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; the amount of the oxidant is 0.3-0.5% (e.g., 0.3%, 0.35%, 0.4%, 0.45% or 0.5%) of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; and / or the amount of the reducing agent is 0.1-0.3% (e.g., 0.1%, 0.15%, 0.2%, 0.25% or 0.3%) of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

[0036] According to some preferred embodiments, in step (1): the initiation temperature of the reaction is 2-5°C (e.g., 2°C, 3°C, 4°C or 5°C); in step (1) of the present invention, after the reaction is initiated at 2-5°C, the temperature of the reaction system will naturally rise until the temperature of the reaction system naturally rises to the peak temperature. After the temperature of the reaction system remains unchanged, the reaction ends; in step (1) of the present invention, the peak temperature of the reaction is, for example, 60-63°C.

[0037] According to some preferred embodiments, in step (1): the molecular weight of the conditioning agent is 30,000 to 100,000; the present invention finds that the conditioning agent with a molecular weight in the range of 30,000 to 100,000 has a moderate chain length, which can effectively balance the reaction speed and bridging ability of the polymer to the particles. The conditioning agent with a suitable molecular weight can enable the anionic polymer to more effectively neutralize the charge on the surface of the particles when treating suspended particles, and can form an effective bridge between the suspended particles, thereby improving the sweeping ability, thereby facilitating the aggregation of the dispersed suspended particles into flocs, thereby improving the flocculation and sedimentation effects; in the present invention, the molecular weight of the conditioning agent is measured according to the test method 5.2 in the standard GB / T31246-2014.

[0038] According to some specific embodiments, the preparation of the conditioning agent adopts the following raw materials: propylene sulfonic acid, vinyl sulfonic acid, calcium hydroxide, calcium chloride and water; the preparation method is: add propylene sulfonic acid, vinyl sulfonic acid, calcium chloride and water into a reaction kettle, mix them thoroughly to obtain a mixed system, add calcium hydroxide to adjust the pH of the mixed system, adjust the temperature of the mixed system to 2~5°C, blow nitrogen to deoxygenate for 30 minutes, add a chain transfer agent, an oxidant and a reducing agent to initiate a reaction (polymerization reaction) to obtain the conditioning agent.

[0039] According to some preferred embodiments, in step (2): the surfactant is sodium fatty alcohol polyoxyethylene ether sulfate; in the present invention, the sodium fatty alcohol polyoxyethylene ether sulfate is, for example, C10~C16 sodium fatty alcohol polyoxyethylene ether sulfate, and in some specific embodiments, the sodium fatty alcohol polyoxyethylene ether sulfate is, for example, sodium dodecyl alcohol polyoxyethylene ether sulfate; the chain transfer agent is sodium hypophosphite; the co-initiator is tetramethylethylenediamine; in the present invention, the co-initiator tetramethylethylenediamine helps potassium persulfate to generate free radicals; the oxidant is potassium persulfate; and / or the reducing agent is sodium bisulfite.

[0040] In the present invention, “and / or” appearing between multiple technical features means that these technical features are connected in an “and / or” relationship, indicating that it can be any one of these technical features, or a combination of any two or more of these technical features.

[0041] According to some preferred embodiments, in step (2), the raw materials used include 50-100 parts (e.g., 50, 60, 70, 80, 90 or 100 parts) of acrylamide, 60-120 parts (e.g., 60, 70, 80, 90, 100, 110 or 120 parts) of acrylic acid, 30-50 parts (e.g., 30, 35, 40, 45 or 50 parts) of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10-20 parts (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 parts) of water-soluble polyvinyl alcohol fiber, and 10-20 parts (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 parts) of allyl-β-cyclodextrin. , 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 parts), a conditioning agent 200-400 parts (for example, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390 or 400 parts), a surfactant 3-6 parts (for example, 3, 4, 5 or 6 parts), calcium hydroxide 31-62 parts (for example, 31, 35, 38, 40, 42, 45, 48, 50, 52, 55, 58, 60 or 62 parts), water 222-606 parts (for example, 222, 250, 30 0, 350, 400, 450, 500, 550, 600 or 606 parts), chain transfer agent 0.005-0.01 parts (for example, 0.005, 0.006, 0.007, 0.008, 0.009 or 0.01 parts), co-initiator 0.5-2 parts (for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2 parts), oxidant 0.005-0.01 parts (for example, 0.005, 0.006, 0.007, 0.008, 0.009 or 0.01 parts), reducing agent 0.005-0.01 parts (For example, 0.005, 0.006, 0.007, 0.008, 0.009 or 0.01 parts); In the present invention, preferably, the mass ratio of the amount of acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin and conditioning agent is (50-100): (60-120): (30-50): (10-20): (10-20): (200-400), which is more conducive to obtaining the anionic polymer suitable for river sludge dehydration, which can achieve better dehydration effect, lower filtrate turbidity and lower filter cake moisture content when dehydrating river sludge. In the present invention, "parts" all refer to "parts by weight". In specific embodiments and comparative examples, the units of parts by weight can be unified as weight units such as "g" or "kg".

[0042] According to some preferred embodiments, in step (2), the initiation temperature of the reaction is 5-10°C (e.g., 5°C, 6°C, 7°C, 8°C, 9°C or 10°C); in the present invention, after the reaction is initiated at 5-10°C, the temperature of the reaction system will naturally rise until the reaction system naturally rises to the peak temperature. After the temperature of the reaction system remains unchanged, the reaction ends.

[0043] According to some preferred embodiments, in step (1) and / or step (2), the time for nitrogen deoxygenation is 20 to 40 minutes.

[0044] According to some specific embodiments, the preparation of the anionic polymer suitable for river sludge dehydration adopts the following raw materials in parts by weight: 50-100 parts of acrylamide, 60-120 parts of acrylic acid, 30-50 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10-20 parts of backbone monomer (water-soluble polyvinyl alcohol fiber), 10-20 parts of allyl-β-cyclodextrin, 200-400 parts of conditioning agent, 3-6 parts of surfactant, 31-62 parts of calcium hydroxide, 222-606 parts of water, 0.005-0.01 parts of chain transfer agent, 0.5-2 parts of co-initiator, 0.005-0.01 parts of oxidant, and 0.01 parts of reducing agent. .005-0.01 parts; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, a conditioner, a surfactant and water are mixed uniformly to obtain a mixed solution, the pH of the mixed solution is adjusted to 6.0-6.5 with calcium hydroxide, and the temperature of the mixed solution is adjusted to 5-10°C, and nitrogen is blown for deoxygenation for 30 minutes, and a chain transfer agent, a co-initiator, an oxidant and a reductant are added to initiate the reaction to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer (abbreviated as anionic polymer) suitable for river sludge dehydration.

[0045] In a second aspect, the present invention provides an anionic polymer suitable for river sludge dehydration, which is prepared by the preparation method described in the first aspect of the present invention.

[0046] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.

[0047] In the present invention, the preparation of conditioning agent A is:

[0048] Add 20 parts of propylene sulfonic acid, 10 parts of vinyl sulfonic acid, 12 parts of calcium chloride and 70 parts of water into the reactor, mix them thoroughly to obtain a mixed system, add 18 parts of calcium hydroxide and adjust the pH of the mixed system to 5.5, adjust the temperature of the mixed system to 5°C (initiating temperature), blow nitrogen to deoxygenate for 30 minutes, add 0.09 parts of dodecyl mercaptan, 0.12 parts of potassium persulfate and 0.06 parts of sodium bisulfite and react to obtain a conditioner A with a molecular weight of 63,000.

[0049] In the present invention, the preparation of conditioning agent B is:

[0050] Add 20 parts of propylene sulfonic acid, 10 parts of vinyl sulfonic acid, 12 parts of calcium chloride and 70 parts of water into the reactor, mix them thoroughly to obtain a mixed system, add 18 parts of calcium hydroxide and adjust the pH of the mixed system to 5.5, adjust the temperature of the mixed system to 5°C (initiating temperature), blow nitrogen to deoxygenate for 30 minutes, add 0.8 parts of dodecyl mercaptan, 0.12 parts of potassium persulfate and 0.06 parts of sodium bisulfite and react to obtain a conditioner B with a molecular weight of 9,000.

[0051] In the present invention, the preparation of conditioning agent C is:

[0052] Add 20 parts of propylene sulfonic acid, 10 parts of vinyl sulfonic acid, 12 parts of calcium chloride and 70 parts of water into a reactor, mix them thoroughly to obtain a mixed system, add 18 parts of calcium hydroxide and adjust the pH of the mixed system to 5.5, adjust the temperature of the mixed system to 5°C (initiating temperature), blow nitrogen to deoxygenate for 30 minutes, add 0.005 parts of dodecyl mercaptan, 0.12 parts of potassium persulfate and 0.06 parts of sodium bisulfite and react to obtain a conditioning agent C with a molecular weight of 570,000.

[0053] In the present invention, the preparation of conditioning agent D is:

[0054] 20 parts of propylene sulfonic acid, 10 parts of vinyl sulfonic acid and 70 parts of water were added to a reactor and mixed thoroughly to obtain a mixed system. After adding 10 parts of sodium hydroxide, the pH of the mixed system was adjusted to 5.5. After adjusting the temperature of the mixed system to 5°C (initiating temperature), nitrogen was blown for deoxygenation for 30 minutes. After adding 0.09 parts of dodecyl mercaptan, 0.12 parts of potassium persulfate and 0.06 parts of sodium bisulfite, a reaction was carried out to obtain a conditioning agent D.

[0055] Example 1

[0056] The present embodiment provides a method for preparing an anionic polymer suitable for dehydrating river sludge; the raw materials used in the preparation of the anionic polymer suitable for dehydrating river sludge are: 50 parts of acrylamide, 60 parts of acrylic acid, 30 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10 parts of water-soluble polyvinyl alcohol fiber, 10 parts of allyl-β-cyclodextrin, 200 parts of conditioning agent A, 3 parts of fatty alcohol polyoxyethylene ether sodium sulfate (dodecyl alcohol polyoxyethylene ether sodium sulfate), 31 parts of calcium hydroxide, 606 parts of water, 0.005 parts of sodium hypophosphite, 0.5 parts of tetramethylethylenediamine, 0.005 parts of potassium persulfate and 0.005 parts of sodium bisulfite; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, conditioning agent A, dodecyl alcohol polyoxyethylene ether sodium sulfate Alkyl alcohol polyoxyethylene ether sodium sulfate and water are uniformly mixed to obtain a mixed solution, the pH of the mixed solution is adjusted to 6.0 with calcium hydroxide, and the temperature of the mixed solution is adjusted to 5°C (initiating temperature), and then nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, tetramethylethylenediamine, potassium persulfate and sodium bisulfite are added to react to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer (abbreviated as anionic polymer) suitable for river sludge dehydration.

[0057] Example 2

[0058] The present embodiment provides a method for preparing an anionic polymer suitable for dehydrating river sludge; the raw materials used in the preparation of the anionic polymer suitable for dehydrating river sludge are: 75 parts of acrylamide, 90 parts of acrylic acid, 40 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 15 parts of water-soluble polyvinyl alcohol fiber, 15 parts of allyl-β-cyclodextrin, 300 parts of conditioning agent A, 4.5 parts of fatty alcohol polyoxyethylene ether sodium sulfate (dodecyl alcohol polyoxyethylene ether sodium sulfate), 46 parts of calcium hydroxide, 429 parts of water, 0.008 parts of sodium hypophosphite, 1 part of tetramethylethylenediamine, 0.008 parts of potassium persulfate and 0.008 parts of sodium bisulfite; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, conditioning agent A, dodecyl alcohol polyoxyethylene ether sodium sulfate, 46 parts of calcium hydroxide, 429 parts of water, 0.008 parts of sodium hypophosphite, 1 part of tetramethylethylenediamine, 0.008 parts of potassium persulfate and 0.008 parts of sodium bisulfite. Alkyl alcohol polyoxyethylene ether sodium sulfate and water are uniformly mixed to obtain a mixed solution, the pH of the mixed solution is adjusted to 6.2 with calcium hydroxide, and the temperature of the mixed solution is adjusted to 8°C (initiating temperature), and then nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, tetramethylethylenediamine, potassium persulfate and sodium bisulfite are added to react to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer (abbreviated as anionic polymer) suitable for river sludge dehydration.

[0059] Example 3

[0060] The present embodiment provides a method for preparing an anionic polymer suitable for dehydrating river sludge; the raw materials used in the preparation of the anionic polymer suitable for dehydrating river sludge are: 100 parts of acrylamide, 120 parts of acrylic acid, 50 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 20 parts of water-soluble polyvinyl alcohol fiber, 20 parts of allyl-β-cyclodextrin, 400 parts of conditioning agent A, 6 parts of fatty alcohol polyoxyethylene ether sodium sulfate (dodecyl alcohol polyoxyethylene ether sodium sulfate), 62 parts of calcium hydroxide, 222 parts of water, 0.01 parts of sodium hypophosphite, 2 parts of tetramethylethylenediamine, 0.01 parts of potassium persulfate and 0.01 parts of sodium bisulfite; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, conditioning agent A, dodecyl alcohol Sodium polyoxyethylene ether sulfate and water are mixed evenly to obtain a mixed solution, the pH of the mixed solution is adjusted to 6.5 with calcium hydroxide, and the temperature of the mixed solution is adjusted to 10°C (initiating temperature), and then nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, tetramethylethylenediamine, potassium persulfate and sodium bisulfite are added to react to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer (abbreviated as anionic polymer) suitable for river sludge dehydration.

[0061] Example 4

[0062] The present embodiment provides a method for preparing an anionic polymer suitable for dehydrating river sludge; the raw materials used in the preparation of the anionic polymer suitable for dehydrating river sludge are: 90 parts of acrylamide, 60 parts of acrylic acid, 20 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 5 parts of water-soluble polyvinyl alcohol fiber, 5 parts of allyl-β-cyclodextrin, 180 parts of conditioning agent A, 3 parts of fatty alcohol polyoxyethylene ether sodium sulfate (dodecyl alcohol polyoxyethylene ether sodium sulfate), 31 parts of calcium hydroxide, 606 parts of water, 0.005 parts of sodium hypophosphite, 0.5 parts of tetramethylethylenediamine, 0.005 parts of potassium persulfate and 0.005 parts of sodium bisulfite; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, conditioning agent A, Sodium dodecyl alcohol polyoxyethylene ether sulfate and water are mixed evenly to obtain a mixed solution, the pH of the mixed solution is adjusted with calcium hydroxide, and the temperature of the mixed solution is adjusted to 5°C (initiating temperature), and then nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, tetramethylethylenediamine, potassium persulfate and sodium bisulfite are added to react to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer (abbreviated as anionic polymer) suitable for river sludge dehydration.

[0063] Example 5

[0064] Example 5 is substantially the same as Example 1, except that:

[0065] In the preparation of anionic polymers, the experiment was conducted using Conditioner B instead of Conditioner A.

[0066] Example 6

[0067] Embodiment 6 is substantially the same as Embodiment 1, except that:

[0068] In the preparation of anionic polymers, the experiment was conducted using Conditioner C instead of Conditioner A.

[0069] Comparative Example 1

[0070] Comparative Example 1 is substantially the same as Example 1, except that:

[0071] The raw materials for preparing the anionic polymer do not contain the conditioning agent A, and the conditioning agent A is not added during the preparation of the anionic polymer.

[0072] Comparative Example 2

[0073] Comparative Example 2 is substantially the same as Example 1, except that:

[0074] In the preparation of anionic polymers, a 25 wt% calcium chloride aqueous solution was used to replace the conditioning agent A for the experiment.

[0075] Comparative Example 3

[0076] This comparative example provides a method for preparing an anionic polymer; the raw materials used in the preparation of the anionic polymer are: 50 parts of acrylamide, 60 parts of acrylic acid, 30 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10 parts of water-soluble polyvinyl alcohol fiber, 10 parts of allyl-β-cyclodextrin, and a conditioning agent D 200 parts, sodium polyoxyethylene fatty alcohol ether sulfate (sodium polyoxyethylene lauryl alcohol ether sulfate) 3 parts, 606 parts of water, 0.005 parts of sodium hypophosphite, 0.5 parts of tetramethylethylenediamine, 0.005 parts of potassium persulfate and 0.005 parts of sodium bisulfite; the preparation method is: acrylamide, acrylic acid, (2-allylsulfonyl-benzimidazole-1-yl)-acetic acid, water-soluble polyvinyl alcohol fiber, allyl-β-cyclodextrin, conditioner D, sodium polyoxyethylene lauryl alcohol ether sulfate and water are uniformly mixed to obtain a mixed solution, the pH of the mixed solution is adjusted to 6.0 with sodium hydroxide, and the temperature of the mixed solution is adjusted to 5°C (initiating temperature), nitrogen is blown for deoxygenation for 30 minutes, sodium hypophosphite, tetramethylethylenediamine, potassium persulfate and sodium bisulfite are added and reacted to obtain a polymer block, and the polymer block is granulated, dried, ground and sieved to obtain an anionic polymer.

[0077] Comparative Example 4

[0078] Comparative Example 4 is substantially the same as Example 1, except that:

[0079] The raw materials for preparing the anionic polymer do not contain water-soluble polyvinyl alcohol fibers, and no water-soluble polyvinyl alcohol fibers are added during the process of preparing the anionic polymer.

[0080] Comparative Example 5

[0081] Comparative Example 5 is substantially the same as Example 1, except that:

[0082] The raw materials for preparing the anionic polymer do not contain allyl-β-cyclodextrin, and no allyl-β-cyclodextrin is added during the process of preparing the anionic polymer.

[0083] Comparative Example 6

[0084] Comparative Example 6 is substantially the same as Example 1, except that:

[0085] The raw materials for preparing the anionic polymer do not contain (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, and (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid is not added during the preparation of the anionic polymer.

[0086] The present invention conducts comparative performance evaluation on the anionic polymers prepared in various embodiments and comparative examples.

[0087] River sludge was used to prepare a sludge slurry with a moisture content of 90%. 1 mL of anionic polymer aqueous solution with a concentration of 1000 ppm was added to 100 mL of sludge slurry. After stirring at a slow speed of 50 r / min for 1 min, the sludge was poured into a measuring cylinder for sedimentation. After sedimentation for 10 min, the tail water and the lower settled sludge were collected separately, and the turbidity removal rate of the tail water and the sludge specific resistance of the settled sludge were determined. The results are shown in Table 1.

[0088] The sludge resistance before flocculation (sludge with 90% water content) is 7.9×10 12 cm / g, which is difficult to filter sludge.

[0089] A small plate and frame filter press was used to carry out the sludge plate and frame filter press experiment, which mainly includes a mud mixing tank, a feed pump, an air compressor, a filter press, a squeeze pump, and a squeeze water tank. During the experiment, 200L of river sludge was first deposited in the mud mixing tank, and then an anionic polymer aqueous solution was added according to the dosage of the agent (1mL of an anionic polymer aqueous solution with a concentration of 1000ppm was added for every 100mL of river sludge) and stirred for 5min. After flocculation, the feed pump was turned on and the sludge slurry was pumped into the filter chamber of the filter press. During the feeding process, the pressure was stabilized at 0.5MPa, and the flow rate of the sludge dewatering tail water at the drainage outlet was monitored at the same time. After the feeding was completed, the feed pump was turned off, the squeeze pump was turned on, and the squeeze dehydration was carried out at a pressure of 1.0MPa. The squeezing stage was maintained for 10min. After the squeezing was completed, the filter plate was loosened, the solidified mud cake (filter cake) was taken out, and the moisture content of the filter cake was measured. The results are shown in Table 1.

[0090] Table 1

[0091]

[0092] It can be seen from the experimental data in Table 1 that the anionic polymer prepared by the present invention can destabilize the suspended particles of river sludge by introducing the conditioning agent A to form a tight floc, and the anionic polymer prepared by the present invention can connect the flocs together under the action of charge neutralization, adsorption bridging and sweeping through the synergy of various adsorption groups, so that the flocs are rigid and the adhesion between the flocs is weak. At the same time, under the action of the skeleton monomer, a skeleton channel is established, and under the joint action of calcium ions, the anionic polymer of the present invention can significantly reduce the sludge specific resistance when the river sludge is dehydrated, which helps to improve the filtration speed and significantly reduce the moisture content of the filter cake. The anionic polymers prepared by some preferred embodiments of the present invention can control the turbidity removal rate to more than 95% and the sludge specific resistance to 3×10 11 cm / g, the difficult-to-filter sludge is transformed into easy-to-filter sludge, the moisture content of the filter cake is controlled within 35%, and the moisture content of the mud cake is greatly reduced.

[0093] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing anionic polymers suitable for dehydrating river sludge, It is characterized in that The preparation method comprises the following steps: (1) Propylene sulfonic acid, vinyl sulfonic acid, calcium chloride and water are uniformly mixed to obtain a mixed system, and then the pH of the mixed system is adjusted to 5-6 with calcium hydroxide, and then nitrogen is passed through the mixed system to remove oxygen, and then a chain transfer agent, an oxidant and a reducing agent are added to react to obtain a conditioning agent; in step (1), the chain transfer agent is dodecyl mercaptan, the oxidant is potassium persulfate, and the reducing agent is sodium bisulfite; the molecular weight of the conditioning agent is 30,000-100,000; (2) By weight, 50-100 parts of acrylamide, 60-120 parts of acrylic acid, 30-50 parts of (2-allylsulfonyl-benzimidazol-1-yl)-acetic acid, 10-20 parts of water-soluble polyvinyl alcohol fiber, 10-20 parts of allyl-β-cyclodextrin, 200-400 parts of a conditioning agent, 3-6 parts of a surfactant and 222-606 parts of water are mixed uniformly to obtain a mixed solution, and then 31-62 parts of calcium hydroxide are used to adjust the pH of the mixed solution to After 6 to 6.5, nitrogen is passed to remove oxygen, and then 0.005 to 0.01 parts of a chain transfer agent, 0.5 to 2 parts of a co-initiator, 0.005 to 0.01 parts of an oxidant and 0.005 to 0.01 parts of a reducing agent are added to react to obtain a polymer block; in step (2), the surfactant is sodium fatty alcohol polyoxyethylene ether sulfate, the chain transfer agent is sodium hypophosphite, the co-initiator is tetramethylethylenediamine, the oxidant is potassium persulfate, and the reducing agent is sodium bisulfite; (3) The polymer blocks are granulated, dried, ground and sieved in sequence to obtain an anionic polymer suitable for river sludge dehydration.

2. The preparation method according to claim 1, It is characterized in that In step (1): The mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is (1.5-2.5):1:(6-8); The amount of calcium hydroxide used is 60-65% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; And / or the amount of calcium chloride is 35-45% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

3. The preparation method according to claim 2, Features: The mass ratio of propylene sulfonic acid, vinyl sulfonic acid and water is 2:1:

7.

4. The preparation method according to claim 1, It is characterized in that In step (1): The amount of the chain transfer agent is 0.2-0.4% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

5. The preparation method according to claim 1, It is characterized in that In step (1): The amount of the oxidant is 0.3-0.5% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid; And / or the amount of the reducing agent is 0.1-0.3% of the sum of the mass amounts of the propylene sulfonic acid and the vinyl sulfonic acid.

6. The preparation method according to claim 1, It is characterized in that In step (1): The initiation temperature of the reaction is 2-5°C.

7. The preparation method according to claim 1, Features: In step (2), the initiation temperature of the reaction is 5-10°C.

8. The preparation method according to claim 1, Features: In step (1) and / or step (2), the time for nitrogen deoxygenation is 20 to 40 minutes.

9. An anionic polymer suitable for river sludge dehydration obtained by the preparation method according to any one of claims 1 to 8.