A kind of anti-ultraviolet polyurethane film and preparation method thereof

By connecting the quaternary ammonium salt-containing siloxane monomer with TiO2 surface and preparing diol quaternary ammonium salt-modified TiO2, the aging problem of polyurethane film under ultraviolet light and heat and the problem of insufficient antibacterial performance is solved. , achieving efficient anti-ultraviolet and antibacterial effects, broadening its application areas.

CN118620262BActive Publication Date: 2024-11-19佛山市奥川顺新材料实业有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411087739.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing polyurethane films are prone to aging and degradation under ultraviolet light and heat, and have poor antibacterial performance, making it difficult to meet the needs of packaging materials for antibacterial and ultraviolet resistance.

Method used

The quaternary ammonium salt group-containing silicone monomer forms a bond with the surface of TiO2 to improve its binding force with polyurethane molecules. The quaternary ammonium salt-modified TiO2 of diol is prepared through ultrasonic reaction and polymerization technology to achieve its uniformity. Dispersing and chain extenders act to enhance antibacterial and UV resistance.

Benefits of technology

It significantly improves the anti-ultraviolet and antibacterial properties of polyurethane films, enhances its application potential in the packaging field, and improves the ultraviolet light absorption and bacterial killing capabilities through uniform dispersion and chain extender action.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_8
    Figure SMS_8
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane films, and discloses an anti-ultraviolet polyurethane film and a preparation method thereof. When diol quaternary ammonium salt-modified TiO2 is irradiated with ultraviolet light, its valence band electrons can obtain energy, absorb ultraviolet light in the medium-wave and long-wave regions, and the absorption and scattering of ultraviolet light constitute a shielding effect on ultraviolet light, weaken the damage of ultraviolet light to polyurethane molecules, and improve the anti-ultraviolet performance of the polyurethane film; the positively charged diol quaternary ammonium salt-modified TiO2 is easy to adhere to negatively charged bacteria through electrostatic interaction and adsorb on the surface of the bacteria, which can effectively change the permeability of the cell wall, finally rupture the bacteria, and achieve the antibacterial effect; at the same time, it can be used as a chain extender to participate in the synthesis of polyurethane, form a protective layer on the surface of the polyurethane, reduce the water vapor permeability coefficient, improve the barrier performance of the polyurethane film, and broaden its application in the fields of packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane films, in particular to an anti-ultraviolet polyurethane film and a preparation method thereof. Background Art

[0002] The packaging film industry has been involved in various fields, requiring films to have higher performance. Due to its alternating structure of hard segments and soft segments, the ratio of its hard and soft segments can be adjusted to regulate the performance of polyurethane, thereby achieving the selection and control of performance. Therefore, polyurethane has excellent comprehensive performance, but ordinary polyurethane materials are prone to aging, degradation and yellowing under the action of light and heat, especially ultraviolet light, which affects both product performance and appearance. At the same time, with the improvement of living standards, people pay great attention to the safety performance of daily necessities, food packaging and medical packaging materials, which requires film materials to have certain antibacterial properties, but the antibacterial properties of polyurethane are poor. Therefore, the preparation of an antibacterial and UV-resistant polyurethane film material to meet the requirements of various fields has become a hot topic of current research.

[0003] TiO 2 As a low-cost, environmentally friendly and non-toxic metal oxide, TiO has high exciton binding energy and large bandgap, showing good potential for absorbing, reflecting and refracting ultraviolet radiation, thus playing a role in resisting ultraviolet radiation. 2 The high hydrophilicity and polarity make it easy to aggregate, have low dispersibility, and be intolerant to acid and alkali, resulting in poor usability. It is also difficult to disperse evenly in waterborne polyurethane. The particles tend to aggregate to form secondary particles, which easily become stress concentration points. In the prior art, high-speed stirring and ultrasonic dispersion are often used to temporarily disperse the nanoparticles evenly. However, the interaction force between the nanoparticles is much stronger than the interaction force between the nanoparticles and the polyurethane polymer. Silane coupling agents are also used to modify them organically, which can reduce the TiO 2 's surface energy, connecting the organic phase and the inorganic phase, but did not improve the antibacterial properties of the polyurethane film.

[0004] The present invention aims to synthesize a siloxane monomer containing a quaternary ammonium salt group and react with TiO 2 The surface hydroxyl groups form bonds to eliminate TiO 2 The high energy potential on the surface increases the binding force between the polyurethane molecules and significantly improves the antibacterial properties of polyurethane. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an anti-ultraviolet polyurethane film and a preparation method thereof, which significantly improves the anti-ultraviolet and antibacterial properties of the polyurethane film and broadens the application field of the polyurethane film.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing an anti-ultraviolet polyurethane film comprises the following steps:

[0008] Step (1), under nitrogen atmosphere, add nano-TiO 2 , ethanol and deionized water, dispersed evenly, added with the structural formula The dimethoxy quaternary ammonium salt siloxane monomer is prepared, and the pH value of the system is adjusted to 3-5 with glacial acetic acid, and an ultrasonic reaction is performed. After the reaction is completed, the product is filtered, washed, and dried under reduced pressure to obtain a dimethoxy quaternary ammonium salt-modified TiO 2 .

[0009] Step (2), under nitrogen atmosphere, add dimethoxy quaternary ammonium salt modified TiO 2 and dichloromethane, mixed evenly, added boron tribromide, reacted at 0-20°C for 12-24h, filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt modified TiO 2 .

[0010] Step (3), under nitrogen atmosphere, add polytetrahydrofuran diol to the reaction flask, vacuum dehydrate at 110-120°C for 1-3h, cool to 50-65°C, add isophorone isocyanate, dimethylol propionic acid and dibutyltin dilaurate, react at 75-90°C for 2-5h, then add diol quaternary ammonium salt modified TiO 2 , continue the reaction for 0.5-1h, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0011] Furthermore, in step (1), the nano-TiO 2 The ratio of ethanol, deionized water, and dimethoxy quaternary ammonium salt siloxane monomer is 1g: (3-5) mL: (10-15) mL: (0.02-0.05) g.

[0012] Furthermore, in step (1), the ultrasonic reaction temperature is 40-60°C, the power is 50-80 Hz, and the time is 30-60 min.

[0013] Furthermore, in step (2), the dimethoxy quaternary ammonium salt modifies TiO 2 The ratio of dichloromethane and boron tribromide is 1g: (30-45) mL: (8-10) g.

[0014] Furthermore, in step (3), polytetramethylene glycol, isophorone isocyanate, dimethylol propionic acid, dibutyltin dilaurate, and diol quaternary ammonium salt modified TiO 2The ratio is 100g: (50-70)g: (6-9)g: (3-5)g: (2-10)g.

[0015] Furthermore, the preparation method of the dimethoxy quaternary ammonium salt siloxane monomer in step (1) comprises the following steps:

[0016] Step S1, under a nitrogen atmosphere, add diethylaminomethyltriethoxysilane and acetonitrile to a reaction flask, stir evenly, add 3-bromopropylene, stir to react, after the reaction is completed, freeze crystallize, filter, wash, and dry to obtain an olefin quaternary ammonium salt siloxane monomer.

[0017] Step S2, under a nitrogen atmosphere, add alkenyl quaternary ammonium salt siloxane monomer and methanol to a reaction flask, stir evenly, add bis-(4-methoxybenzyl)-amine, react at 40-60° C. for 5-10 h, concentrate under reduced pressure, and obtain dimethoxy quaternary ammonium salt siloxane monomer after drying.

[0018] Furthermore, in step S1, the ratio of diethylaminomethyltriethoxysilane, acetonitrile, and 3-bromopropylene is 1 g: (10-20) mL: (0.52-0.65) g.

[0019] Furthermore, in step S1, the reaction temperature is 60-80° C., and the reaction time is 16-32 h.

[0020] Furthermore, in step S2, the ratio of the alkenyl quaternary ammonium salt siloxane monomer, methanol, and bis-(4-methoxybenzyl)-amine is 1 g: (15-30) mL: (1.3-1.5) g.

[0021] By adopting the above technical solution, the beneficial effects of the present invention are:

[0022] The invention firstly reacts diethylaminomethyltriethoxysilane with 3-bromopropylene to obtain an alkenyl quaternary ammonium salt siloxane monomer, and then reacts the monomer with bis-(4-methoxybenzyl)-amine to obtain a dimethoxy quaternary ammonium salt siloxane monomer. Then, the siloxy groups on the surface of the dimethoxy quaternary ammonium salt siloxane monomer react with nano-TiO 2 Chemical bonding is generated to obtain dimethoxy quaternary ammonium salt modified TiO 2 , and then add boron tribromide to remove the methoxy group to obtain diol quaternary ammonium salt modified TiO 2 Finally, polytetramethylene glycol and isophorone isocyanate were used as polymerization monomers, and diol quaternary ammonium salt modified TiO 2 It is a chain extender, and after polymerization to form a film, an anti-ultraviolet polyurethane film is obtained.

[0023] Modified TiO 2 It can be evenly dispersed in the polyurethane matrix and can stably absorb ultraviolet light.2 When exposed to ultraviolet light, the electrons in the valence band can gain energy and jump to the conduction band to form photogenerated electrons. The photogenerated electrons capture oxygen in the air to generate superoxide radicals, which can oxidize organic pollutants to generate carbon dioxide and water. Therefore, nano-TiO 2 It has good absorption of ultraviolet light; at the same time, nano-TiO 2 The small particle size can absorb ultraviolet light in the medium and long wave regions. The absorption and scattering of ultraviolet light constitute a shielding effect on ultraviolet light, weakening the damage of ultraviolet light to polyurethane molecules and improving the anti-ultraviolet performance of polyurethane film.

[0024] Positively charged diol quaternary ammonium salt modified TiO 2 It has good uniform dispersion and can easily adhere to negatively charged bacteria through electrostatic interaction. It can be adsorbed on the surface of bacteria and can effectively change the permeability of the cell wall, eventually causing the bacteria to rupture, resulting in the inactivity of enzymes in the bacteria or protein denaturation, thus achieving an antibacterial effect. 2 The nano-rough surface can further enhance the adhesion of bacteria, leading to physical destruction of the bacterial cell membrane. 2 Hydroxyl radicals can be generated to enhance the antibacterial activity and adhesion to bacteria, causing chemical damage that can quickly destroy bacterial cell components, leading to protein or gene leakage in the cells, thereby achieving the purpose of killing bacteria; in addition, diol quaternary ammonium salt-modified TiO 2 It can be used as a chain extender in the synthesis of polyurethane to form a protective layer on its surface, which reduces the water vapor permeability coefficient, improves the barrier properties of the polyurethane film, and broadens its application in packaging and other fields. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] (1) Under nitrogen atmosphere, add 80 g of diethylaminomethyltriethoxysilane and 1200 mL of acetonitrile to a reaction flask, stir evenly, then add 49.6 g of 3-bromopropylene, react at 70 °C for 24 h, freeze crystallize, filter, wash, and dry to obtain an olefin quaternary ammonium salt siloxane monomer. The preparation reaction formula is as follows:

[0028] .

[0029] (2) Under nitrogen atmosphere, add 75 g of alkenyl quaternary ammonium salt siloxane monomer and 1800 mL of methanol to the reaction flask, stir evenly, add 105 g of bis-(4-methoxybenzyl)-amine, react at 50° C. for 8 h, concentrate under reduced pressure, and dry to obtain dimethoxy quaternary ammonium salt siloxane monomer. The preparation reaction formula is as follows:

[0030] .

[0031] (3) Under nitrogen atmosphere, add 65g of nano-TiO 2 , 260 mL of ethanol and 780 mL of deionized water, after being evenly dispersed, 1.95 g of dimethoxy quaternary ammonium salt siloxane monomer was added, the pH of the system was adjusted to 4 with glacial acetic acid, and ultrasonic reaction was performed at a temperature of 50 ° C and a power of 70 Hz for 50 min. After filtering, washing and drying under reduced pressure, dimethoxy quaternary ammonium salt-modified TiO 2 .

[0032] (4) Under nitrogen atmosphere, add 50 g of dimethoxy quaternary ammonium salt-modified TiO 2 and 2000 mL of dichloromethane, mixed evenly, added 9.5 g of boron tribromide, reacted at 10 ° C for 16 h, filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt modified TiO 2 .

[0033] (5) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 115 °C for 2 h, cooled to 55 °C, 60 g of isophorone isocyanate, 8 g of dimethylol propionic acid and 5 g of dibutyltin dilaurate were added, and reacted at 85 °C for 4 h. Then 2 g of diol quaternary ammonium salt-modified TiO 2 , continue the reaction for 1 hour, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0034] Example 2

[0035] (1) Under nitrogen atmosphere, 55 g of diethylaminomethyltriethoxysilane and 550 mL of acetonitrile were added to a reaction flask. After stirring, 28.6 g of 3-bromopropylene was added. The mixture was reacted at 80 °C for 16 h. The mixture was frozen and crystallized. After filtering and washing, the olefinic ammonium salt siloxane monomer was obtained after drying.

[0036] (2) Under a nitrogen atmosphere, 52 g of alkenyl quaternary ammonium salt siloxane monomer and 780 mL of methanol were added to a reaction flask. After stirring evenly, 67.6 g of bis-(4-methoxybenzyl)-amine was added and reacted at 60° C. for 5 h. The mixture was concentrated under reduced pressure and dried to obtain a dimethoxy quaternary ammonium salt siloxane monomer.

[0037] (3) Under nitrogen atmosphere, add 45g of nano-TiO 2 , 135 mL of ethanol and 450 mL of deionized water, after being evenly dispersed, 0.9 g of dimethoxy quaternary ammonium salt siloxane monomer was added, the pH of the system was adjusted to 5 with glacial acetic acid, and ultrasonic reaction was carried out at a temperature of 60 ° C and a power of 80 Hz for 30 min. After filtering, washing and drying under reduced pressure, dimethoxy quaternary ammonium salt-modified TiO 2 .

[0038] (4) Under nitrogen atmosphere, 40 g of dimethoxy quaternary ammonium salt-modified TiO2 and 1200 mL of dichloromethane were added to the reaction flask. After mixing evenly, 320 g of boron tribromide was added. The mixture was reacted at 20 °C for 12 h. The mixture was filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt-modified TiO2. 2 .

[0039] (5) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 120 °C for 1 h, cooled to 65 °C, 50 g of isophorone isocyanate, 6 g of dimethylol propionic acid and 3 g of dibutyltin dilaurate were added, and reacted at 90 °C for 2 h. Then 4 g of diol quaternary ammonium salt-modified TiO 2 , continue the reaction for 0.5h, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0040] Example 3

[0041] (1) Under nitrogen atmosphere, 35 g of diethylaminomethyltriethoxysilane and 700 mL of acetonitrile were added to a reaction flask. After stirring, 22.75 g of 3-bromopropylene was added. The mixture was reacted at 60 °C for 32 h. The mixture was frozen and crystallized. After filtering and washing, the quaternary ammonium siloxane monomer was obtained after drying.

[0042] (2) Under nitrogen atmosphere, 30 g of alkenyl quaternary ammonium salt siloxane monomer and 900 mL of methanol were added to a reaction flask. After stirring evenly, 45 g of bis-(4-methoxybenzyl)-amine was added. The mixture was reacted at 40° C. for 10 h. The mixture was concentrated under reduced pressure and dried to obtain dimethoxy quaternary ammonium salt siloxane monomer.

[0043] (3) Under nitrogen atmosphere, add 25 g of nano-TiO 2 , 125 mL of ethanol and 375 mL of deionized water, after being evenly dispersed, 1.25 g of dimethoxy quaternary ammonium salt siloxane monomer was added, the pH of the system was adjusted to 3 with glacial acetic acid, and ultrasonic reaction was carried out at a temperature of 40 ° C and a power of 50 Hz for 60 min. After filtering, washing and drying under reduced pressure, dimethoxy quaternary ammonium salt-modified TiO 2 .

[0044] (4) Under nitrogen atmosphere, add 20 g of dimethoxy quaternary ammonium salt-modified TiO 2 and 900 mL of dichloromethane, mixed evenly, added 200 g of boron tribromide, reacted at 0 ° C for 24 h, filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt modified TiO 2 .

[0045] (5) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 110 °C for 3 h, cooled to 50 °C, 70 g of isophorone isocyanate, 9 g of dimethylol propionic acid and 5 g of dibutyltin dilaurate were added, and reacted at 75 °C for 5 h. Then 6 g of diol quaternary ammonium salt-modified TiO 2 , continue the reaction for 1 hour, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0046] Example 4

[0047] (1) Under nitrogen atmosphere, 30 g of diethylaminomethyltriethoxysilane and 480 mL of acetonitrile were added to a reaction flask. After stirring, 17.4 g of 3-bromopropylene was added. The mixture was reacted at 75 °C for 30 h. The mixture was frozen and crystallized. The mixture was filtered, washed, and dried to obtain an olefin quaternary ammonium salt siloxane monomer.

[0048] (2) Under a nitrogen atmosphere, 28 g of alkenyl quaternary ammonium salt siloxane monomer and 560 mL of methanol were added to a reaction flask. After stirring evenly, 40.6 g of bis-(4-methoxybenzyl)-amine was added. The mixture was reacted at 45 °C for 9 h. The mixture was concentrated under reduced pressure and dried to obtain a dimethoxy quaternary ammonium salt siloxane monomer.

[0049] (3) Under nitrogen atmosphere, add 22g of nano-TiO 2 , 85 mL of ethanol and 285 mL of deionized water, after being evenly dispersed, 0.77 g of dimethoxy quaternary ammonium salt siloxane monomer was added, the pH of the system was adjusted to 5 with glacial acetic acid, and ultrasonic reaction was carried out at a temperature of 50 ° C and a power of 60 Hz for 50 min. After filtering, washing and drying under reduced pressure, dimethoxy quaternary ammonium salt-modified TiO 2 .

[0050] (4) Under nitrogen atmosphere, add 20 g of dimethoxy quaternary ammonium salt-modified TiO 2 and 840 mL of dichloromethane, mixed evenly, added 185 g of boron tribromide, reacted at 5 ° C for 15 h, filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt modified TiO 2 .

[0051] (5) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 120 °C for 2 h, cooled to 60 °C, 55 g of isophorone isocyanate, 8 g of dimethylol propionic acid and 4 g of dibutyltin dilaurate were added, and reacted at 85 °C for 3 h. Then 8 g of diol quaternary ammonium salt-modified TiO 2 , continue the reaction for 1 hour, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0052] Example 5

[0053] (1) Under nitrogen atmosphere, add 25 g of diethylaminomethyltriethoxysilane and 400 mL of acetonitrile to a reaction flask, stir evenly, add 14.5 g of 3-bromopropylene, react at 65 °C for 25 h, freeze crystallize, filter, wash, and dry to obtain an olefin quaternary ammonium salt siloxane monomer.

[0054] (2) Under a nitrogen atmosphere, 18 g of alkenyl quaternary ammonium salt siloxane monomer and 330 mL of methanol were added to a reaction flask. After stirring evenly, 26.1 g of bis-(4-methoxybenzyl)-amine was added and reacted at 45° C. for 10 h. The mixture was concentrated under reduced pressure and dried to obtain a dimethoxy quaternary ammonium salt siloxane monomer.

[0055] (3) Under nitrogen atmosphere, add 15 g of nano-TiO 2 , 70 mL of ethanol and 210 mL of deionized water, after being evenly dispersed, 0.54 g of dimethoxy quaternary ammonium salt siloxane monomer was added, the pH of the system was adjusted to 5 with glacial acetic acid, and ultrasonic reaction was carried out at a temperature of 60 ° C and a power of 70 Hz for 45 min. After filtering, washing and drying under reduced pressure, dimethoxy quaternary ammonium salt-modified TiO 2 .

[0056] (4) Under nitrogen atmosphere, add 10 g of dimethoxy quaternary ammonium salt-modified TiO 2 and 350 mL of dichloromethane, mixed evenly, added 85 g of boron tribromide, reacted at 0 ° C for 16 h, filtered, washed with ethanol, and dried to obtain diol quaternary ammonium salt modified TiO 2 .

[0057] (5) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 120 °C for 3 h, cooled to 60 °C, 65 g of isophorone isocyanate, 7 g of dimethylol propionic acid and 5 g of dibutyltin dilaurate were added, and reacted at 90 °C for 5 h. Then 10 g of diol quaternary ammonium salt-modified TiO 2 , continue the reaction for 1 hour, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

[0058] Comparative Example 1

[0059] (1) Under nitrogen atmosphere, 50 g of dimethoxy quaternary ammonium salt siloxane monomer (prepared in Example 1) and 2000 mL of dichloromethane were added to a reaction flask, mixed evenly, and then 9.5 g of boron tribromide was added. The mixture was reacted at 10° C. for 16 h, filtered, washed with ethanol, and dried to obtain a diol quaternary ammonium salt chain extender (structural formula: ).

[0060] (2) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 115 °C for 2 h, cooled to 55 °C, 60 g of isophorone isocyanate, 8 g of dimethylol propionic acid and 5 g of dibutyltin dilaurate were added, and the reaction was carried out at 85 °C for 4 h. Then 2 g of diol quaternary ammonium salt chain extender was added and the reaction was continued for 1 h. Triethylamine was added for neutralization, and the mixture was poured into a glass mold and allowed to stand for degassing and naturally dried in the shade to form a polyurethane film.

[0061] Comparative Example 2

[0062] (1) Under nitrogen atmosphere, add 75 g of KH570 (CAS No. 2530-85-0) and 1800 mL of methanol to a reaction flask, stir evenly, add 105 g of bis-(4-methoxybenzyl)-amine, react at 50 °C for 8 h, concentrate under reduced pressure, and dry to obtain a dimethoxysiloxane monomer (structural formula: ).

[0063] (2) Under nitrogen atmosphere, add 65g of nano-TiO 2 , 260 mL of ethanol and 780 mL of deionized water, after being evenly dispersed, 1.95 g of dimethoxysiloxane monomer was added, the pH of the system was adjusted to 4 with glacial acetic acid, and ultrasonic reaction was carried out at a temperature of 50 ° C and a power of 70 Hz for 50 min. After filtering, washing and drying under reduced pressure, dimethoxy-modified TiO 2 .

[0064] (3) Under nitrogen atmosphere, add 50 g of dimethoxy-modified TiO 2 and 2000 mL of dichloromethane, mixed evenly, added 9.5 g of boron tribromide, reacted at 10 ° C for 16 h, filtered, washed with ethanol, and dried to obtain diol-modified TiO 2 .

[0065] (4) Under nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 115 °C for 2 h, cooled to 55 °C, 60 g of isophorone isocyanate, 8 g of dimethylol propionic acid and 5 g of dibutyltin dilaurate were added, and reacted at 85 °C for 4 h. Then 2 g of diol-modified TiO 2, continue the reaction for 1 hour, add triethylamine to neutralize, pour into a glass mold, let stand to degas, and dry naturally in the shade to form a polyurethane film.

[0066] Comparative Example 3

[0067] Under a nitrogen atmosphere, 100 g of polytetrahydrofuran diol was added to the reaction flask, vacuum dehydrated at 115 ° C for 2 h, cooled to 55 ° C, 60 g of isophorone isocyanate, 8 g of dimethylolpropionic acid and 5 g of dibutyltin dilaurate were added, and the mixture was reacted at 85 ° C for 4 h. Triethylamine was added for neutralization, and the mixture was poured into a glass mold, allowed to stand for degassing, and naturally dried in the shade to form a polyurethane film.

[0068] Antibacterial performance test: mainly test bacteria (Escherichia coli and Salmonella), the bacteria are placed in the culture medium with beef extract peptone agar, cultured at 37°C for 24 hours, eluted with sterile saline, and made into a concentration of 10 7 CFU / mL of bacterial suspension; the cultured bacterial suspension was coated on the surface of the culture medium with a diameter of 10 cm using a coating rod, the prepared polyurethane film was cut into the size of the sample to be tested with a diameter of 1 cm and placed in the center of the culture medium, and cultured at a constant temperature of 37°C overnight, and the diameter of the inhibition zone was measured by the cross method, and the average value was taken.

[0069]

[0070] From the test results in the above table, it can be seen that with the modification of TiO 2 With the increase of the content, the antibacterial property of the polyurethane film is gradually enhanced. In Example 5, the diameter of the inhibition zone for Escherichia coli reaches 88.39 mm, and the diameter of the inhibition zone for Staphylococcus aureus reaches 82.31 mm, which has good antibacterial property; this is because on the one hand, the positively charged diol quaternary ammonium salt modified TiO 2 It has good uniform dispersion and can easily adhere to negatively charged bacteria through electrostatic interaction and adsorb on the surface of bacteria, which can effectively change the permeability of the cell wall, eventually causing the bacteria to rupture, resulting in the inactivity of enzymes in the bacteria or protein denaturation, thus achieving an antibacterial effect. On the other hand, diol quaternary ammonium salt-modified TiO 2 The nano-rough surface can further enhance the adhesion of bacteria, leading to physical destruction of the bacterial cell membrane. 2 Hydroxyl radicals can be generated to enhance antibacterial activity and adhesion to bacteria, causing chemical damage that can quickly destroy bacterial cell components, leading to leakage of intracellular proteins or genes, thereby achieving the purpose of killing bacteria.

[0071] Comparative Example 1 contains quaternary ammonium salt antibacterial ingredients, but does not contain nano-TiO 2 , has certain antibacterial properties; Comparative Example 2 contains nano-TiO2 , but does not contain quaternary ammonium salt and has poor antibacterial performance; Comparative Example 3 does not contain any antibacterial ingredients and has no antibacterial performance.

[0072] Anti-ultraviolet performance test: the prepared polyurethane film was cut into rectangular specimens of 150mm×10mm in size, and the tensile strength test was carried out using a universal testing machine. The tensile speed was 200mm / min, the test temperature was 23℃, the relative humidity was 50%RH, and the average value was taken after 5 measurements. The polyurethane film was then placed in an ultraviolet accelerated aging box and irradiated with a 200W mercury light source for 360h for a tensile strength test.

[0073]

[0074] From the test results in the above table, it can be seen that with the modification of TiO 2 With the increase of TiO content, the anti-ultraviolet performance of polyurethane film is gradually enhanced. This is because the modified TiO 2 It can be evenly dispersed in the polyurethane matrix and can stably absorb ultraviolet light. 2 When exposed to ultraviolet light, the electrons in the valence band can gain energy and jump to the conduction band to form photogenerated electrons. The photogenerated electrons capture oxygen in the air to generate superoxide radicals, which can oxidize organic pollutants to generate carbon dioxide and water. Therefore, nano-TiO 2 It has good absorption of ultraviolet light; at the same time, nano-TiO 2 The small particle size can absorb ultraviolet light in the medium and long wave regions. The absorption and scattering of ultraviolet light constitute a shielding effect on ultraviolet light, weakening the damage of ultraviolet light to polyurethane molecules and improving the anti-ultraviolet performance of polyurethane film.

[0075] Comparative Examples 1 and 3 do not contain TiO 2 After 360 hours of UV irradiation, the tensile strength of the polyurethane film decreased significantly and it did not have anti-UV properties.

[0076] Water vapor transmission coefficient test: refer to GB / T 1037-88 for testing, the experimental temperature is 23℃, the humidity is 50%RH.

[0077]

[0078] The water vapor permeability coefficient can reflect the barrier ability of the film to water vapor. The lower the coefficient, the lower the water absorption rate of the material and the better the barrier performance. From the test results in the above table, it can be seen that with the modification of TiO 2 With the increase of content, the water vapor permeability coefficient of polyurethane film gradually decreased, and the barrier performance was significantly enhanced. This is because the diol quaternary ammonium salt modified TiO 2It can be used as a chain extender in the synthesis of polyurethane to form a protective layer on its surface, which reduces the water vapor permeability coefficient, improves the barrier properties of the polyurethane film, and broadens its application in packaging and other fields.

[0079] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.

Claims

1. A method for preparing an anti-ultraviolet polyurethane film, characterized in that: The preparation method comprises the following steps: Step (1), under nitrogen atmosphere, add nano-TiO2, ethanol and deionized water to a reaction flask, and after uniform dispersion, add The dimethoxy quaternary ammonium salt siloxane monomer is used to adjust the system pH to 3-5 with glacial acetic acid, and ultrasonic reaction is carried out. After the reaction is completed, the dimethoxy quaternary ammonium salt modified TiO2 is obtained after filtering, washing, and drying under reduced pressure; Step (2), under a nitrogen atmosphere, add dimethoxy quaternary ammonium salt-modified TiO2 and dichloromethane to a reaction flask, mix well, add boron tribromide, react at 0-20° C. for 12-24 h, filter, wash with ethanol, and dry to obtain diol quaternary ammonium salt-modified TiO2; Step (3), under nitrogen atmosphere, add polytetrahydrofuran diol to the reaction flask, vacuum dehydrate at 110-120° C. for 1-3 h, cool to 50-65° C., add isophorone isocyanate, dimethylol propionic acid and dibutyltin dilaurate, react at 75-90° C. for 2-5 h, then add diol quaternary ammonium salt-modified TiO2, continue to react for 0.5-1 h, add triethylamine for neutralization, pour into a glass mold, stand for degassing, and naturally dry in the shade to form a film to obtain an anti-ultraviolet polyurethane film.

2. The method for preparing the anti-ultraviolet polyurethane film according to claim 1, characterized in that: In the step (1), the ratio of nano-TiO2, ethanol, deionized water, and dimethoxy quaternary ammonium salt siloxane monomer is 1 g: (3-5) mL: (10-15) mL: (0.02-0.05) g.

3. The method for preparing the anti-ultraviolet polyurethane film according to claim 1, characterized in that: In the step (1), the ultrasonic reaction temperature is 40-60°C, the power is 50-80 Hz, and the time is 30-60 min.

4. The method for preparing the anti-ultraviolet polyurethane film according to claim 1, characterized in that: In the step (2), the ratio of dimethoxy quaternary ammonium salt-modified TiO2, dichloromethane, and boron tribromide is 1 g: (30-45) mL: (8-10) g.

5. The method for preparing the anti-ultraviolet polyurethane film according to claim 1, characterized in that: In the step (3), the ratio of polytetrahydrofuran diol, isophorone isocyanate, dimethylol propionic acid, dibutyltin dilaurate, and diol quaternary ammonium salt-modified TiO2 is 100g: (50-70)g: (6-9)g: (3-5)g: (2-10)g.

6. The method for preparing the anti-ultraviolet polyurethane film according to claim 1, characterized in that: The preparation method of the dimethoxy quaternary ammonium salt siloxane monomer in step (1) comprises the following steps: Step S1, under a nitrogen atmosphere, add diethylaminomethyltriethoxysilane and acetonitrile to a reaction flask, stir evenly, add 3-bromopropylene, stir to react, after the reaction is completed, freeze crystallize, filter, wash, and dry to obtain an olefin quaternary ammonium salt siloxane monomer; Step S2, under a nitrogen atmosphere, add alkenyl quaternary ammonium salt siloxane monomer and methanol to a reaction flask, stir evenly, add bis-(4-methoxybenzyl)-amine, react at 40-60° C. for 5-10 h, concentrate under reduced pressure, and obtain dimethoxy quaternary ammonium salt siloxane monomer after drying.

7. The method for preparing the anti-ultraviolet polyurethane film according to claim 6, characterized in that: In the step S1, the ratio of diethylaminomethyltriethoxysilane, acetonitrile and 3-bromopropylene is 1 g: (10-20) mL: (0.52-0.65) g.

8. The method for preparing the anti-ultraviolet polyurethane film according to claim 6, characterized in that: In step S1, the reaction temperature is 60-80° C. and the reaction time is 16-32 hours.

9. The method for preparing the anti-ultraviolet polyurethane film according to claim 6, characterized in that: In the step S2, the ratio of the alkenyl quaternary ammonium salt siloxane monomer, methanol, and bis-(4-methoxybenzyl)-amine is 1 g: (15-30) mL: (1.3-1.5) g.

10. An anti-ultraviolet polyurethane film, characterized in that: Obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Fluorine-silicon composite modified waterborne polyurethane acrylate anti-ultraviolet coating and preparation method thereof

    CN120442119A