Cemented carbide stamping die for high-hardness die steel stamping and preparation method thereof

By using additives such as tungsten carbide, chromium carbide, molybdenum carbide and cerium ammonium nitrate in cemented carbide stamping molds, combined with sintering and heat treatment processes, the problem of insufficient impact resistance and wear resistance of the mold when stamping high-hard mold steel is solved. problem, achieving the effects of high hardness and long life.

CN118621168BActive Publication Date: 2024-10-29CHONGYI ZHANGYUAN TUNGSTEN
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411115019.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing carbide stamping dies are prone to cracking and chipping when stamping high-hard die steel, have short service life, and lack of impact resistance and wear resistance, making it difficult to meet market demand.

Method used

Using the combination of tungsten carbide, chromium carbide, molybdenum carbide and cerium ammonium nitrate and other additives, through processes such as ball milling, spray drying, dewaxing sintering, quenching, cryogenic cooling and low-temperature tempering, a hardened material with high hardness and flexural strength is prepared. High-quality alloy stamping dies.

Benefits of technology

The high hardness, wear resistance and flexural strength of the cemented carbide stamping die is achieved. The average WC grain size is 4~8μm, the density is 11.5~12.7g/cm3, the hardness HRA is 78~81, and the flexural strength is >2700MPa , extending the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621168B_ABST
    Figure CN118621168B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy, and specifically relates to a cemented carbide stamping die for high-hardness die steel stamping and a preparation method thereof. By adding rare earth elements and additives such as chromium carbide and molybdenum carbide, and coordinating with a secondary sintering process and a heat treatment process, the synergistic strengthening of a binder phase and a hard phase is achieved; the WC average grain size of the prepared cemented carbide stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3 , hardness HRA is 78.0~81.0, and flexural strength is >2700MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and specifically relates to a cemented carbide stamping die for stamping high-hardness die steel and a preparation method thereof. Background Art

[0002] For the hardware stamping dies of high-hardness die steel, they need to have high hardness, high toughness and impact resistance. Traditional cemented carbide grades can no longer meet the market demand. At present, there are few cemented carbide grades for this type of application, and the application is not ideal. There are many mold cracking phenomena and short service life. Therefore, it is urgent to develop a stamping die with high hardness, high toughness and impact resistance for high-hardness die steel stamping.

[0003] At present, there are few cemented carbide grades used in stamping dies for high-hardness die steel. Due to the difficulty of stamping and the high impact toughness requirements of the alloy, most of them adopt the WC-25~27% (Co-Ni-Cr) solution, in which the metal bonding phase is composed of a certain ratio of cobalt and nickel. During use, due to the poor wettability of metal nickel during sintering, the bonding strength of nickel is lower than that of cobalt, which leads to cracking and corner collapse problems in cemented carbide stamping dies when stamping high-hardness die steel. For molds using pure cobalt as the bonding phase, due to the high cobalt content, a large amount of liquid phase appears during sintering, resulting in serious sintering deformation of the product; at the same time, pure cobalt has poor corrosion resistance, and the bonding phase will be corroded during mold processing and use, resulting in a short product life. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a cemented carbide stamping die for high-hardness die steel stamping and a preparation method thereof.

[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0006] A method for preparing a cemented carbide stamping die for high-hardness die steel stamping comprises the following steps:

[0007] S1. Take tungsten carbide, a binder phase, and an additive to obtain a raw material, wherein the tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide, and the additives include chromium carbide, molybdenum carbide, and ammonium cerium nitrate;

[0008] S2, ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact;

[0009] S3, dewaxing and sintering the pressed green body to obtain a sintered green body;

[0010] S4. The sintered blank is subjected to quenching treatment, deep cryogenic treatment, and low temperature tempering treatment to obtain a cemented carbide stamping die for stamping high-hardness die steel.

[0011] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping described in the present invention, in the step S1, the proportion of chromium carbide in the raw material is 0.8~1.5wt%, the proportion of molybdenum carbide is 0.3~1.0wt%, and the proportion of ammonium cerium nitrate is 0.3~0.4wt%.

[0012] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping described in the present invention, wherein: in the step S1, the Fischer-Matz particle size of coarse-grained tungsten carbide is 20~35μm, and the Fischer-Matz particle size of medium-grained tungsten carbide is 2.0~4.0μm; the coarse-grained tungsten carbide accounts for 35~60wt% of the raw material, and the medium-grained tungsten carbide accounts for 10~20wt% of the raw material.

[0013] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping described in the present invention, wherein: in the step S1, the binding phase is 0-1wt% nickel powder and the remainder cobalt powder, and the binding phase accounts for 30-40wt% of the raw material.

[0014] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping according to the present invention, wherein: in the step S2, the ball milling is divided into two ball millings:

[0015] First ball milling: Use granular paraffin as a molding agent, the weight of which is 1.8~2.0wt% of the weight of the raw material. Pre-grind the granular paraffin for 10~20min, then add all the components in the raw material except the coarse tungsten carbide particles, and then add anhydrous ethanol calculated at a liquid-solid ratio of (0.26~0.28)L:1kg, and ball mill for 20~30h at a ball mill speed of 36~38r / min and a ball-to-material ratio of (1.2~1.5):1 to obtain a slurry;

[0016] Secondary ball milling: add coarse tungsten carbide particles into the slurry, and add anhydrous ethanol calculated at a liquid-to-solid ratio of (0.26-0.28) L:1 kg, and mill for 10-15 hours at a ball mill speed of 15-20 r / min and a ball-to-material ratio of (1.2-1.5):1. After unloading, spray dry to obtain a mixture.

[0017] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping described in the present invention, wherein: in the step S3, the wax molding agent is removed from the pressed blank by a hydrogen dewaxing process, and the heating rate is controlled to be 0.2°C / min in the 220~260°C stage.

[0018] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping according to the present invention, in step S3, the sintering is divided into two sintering steps:

[0019] First sintering: sintering temperature is 1320~1340℃, high pressure argon is introduced, sintering pressure is 10bar, sintering time is 30min, and it is taken out of the furnace after cooling;

[0020] Second sintering: Wrap the product after being fired with wood pulp paper with a thickness of 0.2~0.3mm, and then use calcined alumina to completely fill it for the second sintering to obtain a sintered blank. When the sintering temperature is 1280~1300℃, introduce argon gas and control the sintering pressure to 10~100mbar. When the sintering temperature is 1400~1420℃, introduce high-pressure argon gas and control the pressurized sintering pressure to 10~50bar. The pressure and temperature holding time is 40~60min.

[0021] As a preferred embodiment of the method for preparing a cemented carbide stamping die for high-hardness die steel stamping described in the present invention, wherein: in the step S4, the quenching process is: placing the sintered blank in a gas quenching furnace, heating the temperature from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, keeping the temperature for 20 minutes, then heating the temperature from 800°C to 1100°C at a heating rate of 3.75°C / min, keeping the temperature for 30 minutes, and finally filling with 1-3 bar argon gas to quickly cool to room temperature;

[0022] The cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is lowered to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 150-200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature;

[0023] Low temperature tempering process: Place the product after deep cryogenic treatment in a vacuum furnace, heat it to 200°C at a heating rate of 1°C / min, keep it warm for 4 hours, and then stop the furnace to cool it to room temperature.

[0024] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0025] A cemented carbide stamping die for stamping high-hard die steel is prepared by adopting the above-mentioned preparation method of the cemented carbide stamping die for stamping high-hard die steel.

[0026] As a preferred embodiment of a cemented carbide stamping die for high-hardness die steel stamping according to the present invention, wherein: the WC average grain size of the cemented carbide stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3, hardness HRA is 78~81, and flexural strength is >2700MPa.

[0027] The beneficial effects of the present invention are as follows:

[0028] The present invention provides a cemented carbide stamping die for high-hardness die steel stamping and a preparation method thereof. By adding rare earth elements and additives such as chromium carbide and molybdenum carbide, and coordinating with a secondary sintering process and a heat treatment process, the synergistic strengthening of the binder phase and the hard phase is achieved. The WC average grain size of the prepared cemented carbide stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3 , hardness HRA is 78~81, and flexural strength is >2700MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0030] Figure 1 This is a picture of the product prepared in Example 1 of the present invention.

[0031] Figure 2 This is a picture of the product prepared in Example 2 of the present invention.

[0032] Figure 3 This is a picture of the product prepared in Example 3 of the present invention.

[0033] Figure 4 This is a picture of the product prepared in Comparative Example 1 of the present invention.

[0034] Figure 5 This is a picture of the product prepared in Comparative Example 2 of the present invention.

[0035] Figure 6 This is a picture of the product prepared in Comparative Example 3 of the present invention.

[0036] Figure 7 This is a picture of the product prepared in Comparative Example 4 of the present invention.

[0037] Figure 8 This is a picture of the product prepared in Comparative Example 5 of the present invention.

[0038] Fig. 9 This is a picture of the product prepared in Comparative Example 6 of the present invention.

[0039] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0040] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The present invention provides a cemented carbide stamping die for high-hardness die steel stamping and a preparation method thereof, which has the following advantages:

[0042] (1) The present invention reduces the ball milling speed and the crushing of the coarse tungsten carbide particles by adding coarse tungsten carbide particles for a second time, thereby retaining the original particle size of the coarse tungsten carbide particles to a great extent and ensuring the impact resistance of the product. At the same time, the medium tungsten carbide particles fill the gaps in the coarse tungsten carbide particles and ensure the wear resistance and hardness of the product.

[0043] (2) The present invention adds rare earth elements in the form of ammonium cerium nitrate dissolved in alcohol, thereby improving the dispersion uniformity of the rare earth elements and effectively strengthening the bonding phase.

[0044] (3) The quenching process can increase the solid solubility of tungsten in cobalt and improve the bending strength and toughness of the alloy, while the cryogenic process can improve the wear resistance of the alloy. Finally, the tempering process can eliminate the internal stress generated during the heat treatment and cryogenic process and improve the comprehensive service life of the product.

[0045] (4) The secondary sintering is wrapped with wood pulp paper and combined with alumina landfill, which can effectively prevent the deformation of high-cobalt products caused by the high-cobalt liquid phase during the sintering process. At the same time, a certain thickness of paper can isolate alumina after high-temperature carbonization, which can reduce the pits on the product surface caused by the use of alumina landfill.

[0046] According to one aspect of the present invention, the present invention provides the following technical solution:

[0047] A method for preparing a cemented carbide stamping die for high-hardness die steel stamping comprises the following steps:

[0048] S1. Take tungsten carbide, a binder phase, and an additive to obtain a raw material, wherein the tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide, and the additives include chromium carbide, molybdenum carbide, and ammonium cerium nitrate;

[0049] S2, ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact;

[0050] S3, dewaxing and sintering the pressed green body to obtain a sintered green body;

[0051] S4. The sintered blank is subjected to quenching treatment, deep cryogenic treatment, and low temperature tempering treatment to obtain a cemented carbide stamping die for stamping high-hardness die steel.

[0052] Preferably, in step S1, the proportion of chromium carbide in the raw material is 0.8-1.5wt%, the proportion of molybdenum carbide is 0.3-1.0wt%, and the proportion of ammonium cerium nitrate is 0.3-0.4wt%.

[0053] Preferably, in step S1, the Fisher particle size of coarse tungsten carbide is 20-35 μm, and the Fisher particle size of medium tungsten carbide is 2.0-4.0 μm; the coarse tungsten carbide accounts for 35-60wt% of the raw material, and the medium tungsten carbide accounts for 10-20wt% of the raw material.

[0054] Preferably, in step S1, the binder phase is 0-1wt% nickel powder and the balance cobalt powder, and the binder phase accounts for 30-40wt% of the raw material.

[0055] Preferably, in step S2, the ball milling is divided into two ball millings:

[0056] First ball milling: Use granular paraffin as a molding agent, the weight of which is 1.8~2.0wt% of the weight of the raw material. Pre-grind the granular paraffin for 10~20min, then add all the components in the raw material except the coarse tungsten carbide particles, and then add anhydrous ethanol calculated at a liquid-solid ratio of (0.26~0.28)L:1kg, and ball mill for 20~30h at a ball mill speed of 36~38r / min and a ball-to-material ratio of (1.2~1.5):1 to obtain a slurry;

[0057] Secondary ball milling: add coarse tungsten carbide particles into the slurry, and add anhydrous ethanol calculated at a liquid-to-solid ratio of (0.26-0.28) L:1 kg, and mill for 10-15 hours at a ball mill speed of 15-20 r / min and a ball-to-material ratio of (1.2-1.5):1. After unloading, spray dry to obtain a mixture.

[0058] Preferably, in step S3, the pressed green sheet is dewaxed with hydrogen to remove the paraffin molding agent. In the dewaxing stage, in order to prevent the ammonium cerium nitrate from releasing gas too quickly by thermal decomposition, the heating rate needs to be controlled at 0.2°C / min in the stage of 220-260°C.

[0059] Preferably, in step S3, the sintering is divided into two sintering steps:

[0060] First sintering: sintering temperature is 1320~1340℃, high pressure argon is introduced, sintering pressure is 10bar, sintering time is 30min, and it is taken out of the furnace after cooling;

[0061] Second sintering: Wrap the product after being fired with wood pulp paper with a thickness of 0.2~0.3mm, and then use calcined alumina to completely fill it for the second sintering to obtain a sintered blank. When the sintering temperature is 1280~1300℃, introduce argon gas and control the sintering pressure to 10~100mbar. When the sintering temperature is 1400~1420℃, introduce high-pressure argon gas and control the pressurized sintering pressure to 10~50bar. The pressure and temperature holding time is 40~60min.

[0062] Preferably, in step S4, the quenching process is: placing the sintered blank in a gas quenching furnace, heating the temperature from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, keeping the temperature for 20 minutes, then heating the temperature from 800°C to 1100°C at a heating rate of 3.75°C / min, keeping the temperature for 30 minutes, and finally filling with 1-3 bar argon gas to quickly cool to room temperature;

[0063] The cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is lowered to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 150-200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature;

[0064] Low temperature tempering process: Place the product after deep cryogenic treatment in a vacuum furnace, heat it to 200°C at a heating rate of 1°C / min, keep it warm for 4 hours, and then stop the furnace to cool it to room temperature.

[0065] According to another aspect of the present invention, the present invention provides the following technical solution:

[0066] A cemented carbide stamping die for stamping high-hard die steel is prepared by adopting the above-mentioned preparation method of the cemented carbide stamping die for stamping high-hard die steel.

[0067] Preferably, the WC average grain size of the cemented carbide stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3 , hardness HRA is 78~81, and flexural strength is >2700MPa.

[0068] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0069] Example 1

[0070] A method for preparing a cemented carbide stamping die for high-hardness die steel stamping comprises the following steps:

[0071] S1. Take tungsten carbide, a binder phase and additives to obtain a raw material. The tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide. The additives are chromium carbide, molybdenum carbide and ammonium cerium nitrate. The proportion of chromium carbide in the raw material is 1.0wt%, the proportion of molybdenum carbide is 0.5wt%, and the proportion of ammonium cerium nitrate is 0.4wt%. The Fisher particle size of the coarse-grained tungsten carbide is 35μm, and the Fisher particle size of the medium-grained tungsten carbide is 4.0μm. The proportion of coarse-grained tungsten carbide in the raw material is 58.1wt%, and the proportion of medium-grained tungsten carbide in the raw material is 10wt%. The binder phase is cobalt powder, and the binder phase accounts for 30wt% of the raw material.

[0072] S2. Ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact; the ball milling is divided into two ball millings: the first ball milling: using granular paraffin as a molding agent, its weight is 2.0wt% of the weight of the raw material, first pre-grinding the granular paraffin for 20 minutes, then adding all the components in the raw materials except the coarse tungsten carbide particles, and then adding anhydrous ethanol calculated at a liquid-solid ratio of 0.28L:1kg, and ball milling for 20 hours at a ball milling speed of 36r / min and a ball-to-material ratio of 1.2:1 to obtain a slurry; the second ball milling: adding coarse tungsten carbide particles to the slurry, and adding anhydrous ethanol calculated at a liquid-solid ratio of 0.28L:1kg, ball milling for 10 hours at a ball milling speed of 15r / min and a ball-to-material ratio of 1.2:1, and spray drying after unloading to obtain a mixture.

[0073] S3, dewaxing and sintering the pressed green sheet to obtain a sintered green sheet; the pressed green sheet is dewaxed by a hydrogen dewaxing process to remove the paraffin molding agent, and the heating rate is controlled to be 0.2°C / min in the stage of 220-260°C; the sintering is divided into two sintering steps: the first sintering step: the sintering temperature is 1320°C, high-pressure argon is introduced to increase the sintering pressure to 10 bar, the sintering time is 30 minutes, and the pressed green sheet is taken out of the furnace after cooling; the second sintering step: the product taken out of the furnace is wrapped with wood pulp paper with a thickness of 0.3 mm, and then the calcined alumina is used to completely fill it for the second sintering step to obtain a sintered green sheet, argon is introduced to control the sintering pressure to 10 mbar when the sintering temperature is 1280°C, and high-pressure argon is introduced to control the pressurized sintering pressure to 30 bar when the sintering temperature is 1400°C, and the pressure and heat preservation time is 60 minutes.

[0074] S4, the sintered blank is subjected to quenching treatment, cryogenic treatment, and low-temperature tempering treatment. The quenching treatment process is as follows: the sintered blank is placed in a gas quenching furnace, and the temperature is increased from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, and the temperature is kept for 20 minutes. Then, the temperature is increased from 800°C to 1100°C at a heating rate of 3.75°C / min, and the temperature is kept for 30 minutes. Finally, 2 bar argon gas is filled to quickly cool to room temperature; the cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is cooled to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature; the low-temperature tempering process is as follows: the cryogenically treated product is placed in a vacuum furnace, and heated to 200°C at a heating rate of 1°C / min, and the temperature is kept for 4 hours, and then the furnace is stopped to allow it to cool to room temperature. A cemented carbide stamping die for high-hardness die steel stamping is obtained.

[0075] The pictures of the products obtained in this embodiment are as follows Figure 1 As shown, the average grain size of WC is 7 μm and the density is 12.55 g / cm 3 , hardness HRA is 80.1, and flexural strength is 2860MPa.

[0076] Example 2

[0077] A method for preparing a cemented carbide stamping die for high-hardness die steel stamping comprises the following steps:

[0078] S1. Take tungsten carbide, a binder phase, and additives to obtain a raw material. The tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide. The additives are chromium carbide, molybdenum carbide, and ammonium cerium nitrate. The proportion of chromium carbide in the raw material is 1.5wt%, the proportion of molybdenum carbide is 1.0wt%, and the proportion of ammonium cerium nitrate is 0.4wt%. The Fisher particle size of the coarse-grained tungsten carbide is 20μm, and the Fisher particle size of the medium-grained tungsten carbide is 2.5μm. The proportion of coarse-grained tungsten carbide in the raw material is 52.1wt%, and the proportion of medium-grained tungsten carbide in the raw material is 10wt%. The binder phase is cobalt powder, and the binder phase accounts for 35wt% in the raw material.

[0079] S2. Ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact; the ball milling is divided into two ball millings: the first ball milling: using granular paraffin as a molding agent, its weight is 2.0wt% of the weight of the raw material, and pre-grinding the granular paraffin for 20 minutes, then adding all the components in the raw materials except the coarse tungsten carbide particles, and then adding anhydrous ethanol calculated at a liquid-solid ratio of 0.28L:1kg, and ball milling for 25h at a ball milling speed of 36r / min and a ball-to-material ratio of 1.2:1 to obtain a slurry; the second ball milling: adding coarse tungsten carbide particles to the slurry, and adding anhydrous ethanol calculated at a liquid-solid ratio of 0.28L:1kg, at a ball milling speed of 20r / min and a ball-to-material ratio of 1.2:1 for 10 hours, and spray drying after unloading to obtain a mixture.

[0080] S3, dewaxing and sintering the pressed green sheet to obtain a sintered green sheet; the pressed green sheet is dewaxed by a hydrogen dewaxing process to remove the paraffin molding agent, and the heating rate is controlled to be 0.2°C / min in the stage of 220-260°C; the sintering is divided into two sintering steps: the first sintering step: the sintering temperature is 1320°C, high-pressure argon is introduced to increase the sintering pressure to 10 bar, the sintering time is 30 minutes, and the green sheet is taken out of the furnace after cooling; the second sintering step: the product taken out of the furnace is wrapped with wood pulp paper with a thickness of 0.3 mm, and then the calcined alumina is used to completely fill it for the second sintering step to obtain a sintered green sheet, argon is introduced to control the sintering pressure to 10 mbar when the sintering temperature is 1280°C, and high-pressure argon is introduced to control the pressurized sintering pressure to 30 bar when the sintering temperature is 1420°C, and the pressure and heat preservation time is 40 minutes.

[0081] S4, the sintered blank is subjected to quenching treatment, cryogenic treatment, and low-temperature tempering treatment. The quenching treatment process is as follows: the sintered blank is placed in a gas quenching furnace, and the temperature is increased from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, and the temperature is kept for 20 minutes. Then, the temperature is increased from 800°C to 1100°C at a heating rate of 3.75°C / min, and the temperature is kept for 30 minutes. Finally, 2 bar argon gas is filled to quickly cool to room temperature; the cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is cooled to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature; the low-temperature tempering process is as follows: the cryogenically treated product is placed in a vacuum furnace, and heated to 200°C at a heating rate of 1°C / min, and the temperature is kept for 4 hours, and then the furnace is stopped to allow it to cool to room temperature. A cemented carbide stamping die for high-hardness die steel stamping is obtained.

[0082] The pictures of the products obtained in this embodiment are as follows Figure 2 As shown, the average grain size of WC is 6 μm and the density is 12.1 g / cm 3 , hardness HRA is 79.4, and flexural strength is 2840MPa.

[0083] Example 3

[0084] A method for preparing a cemented carbide stamping die for high-hardness die steel stamping comprises the following steps:

[0085] S1. Take tungsten carbide, a binder phase and additives to obtain a raw material. The tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide. The additives are chromium carbide, molybdenum carbide and ammonium cerium nitrate. The proportion of chromium carbide in the raw material is 1.5wt%, the proportion of molybdenum carbide is 1.0wt%, and the proportion of ammonium cerium nitrate is 0.4wt%. The Fisher particle size of the coarse-grained tungsten carbide is 20μm, and the Fisher particle size of the medium-grained tungsten carbide is 2.5μm. The proportion of coarse-grained tungsten carbide in the raw material is 37.1wt%, and the proportion of medium-grained tungsten carbide in the raw material is 20wt%. The binder phase is cobalt powder, and the binder phase accounts for 40wt% in the raw material.

[0086] S2. Ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact; the ball milling is divided into two ball millings: the first ball milling: using granular paraffin as a molding agent, its weight is 2.0wt% of the weight of the raw material, and pre-grinding the granular paraffin for 20 minutes, then adding all the components in the raw materials except coarse tungsten carbide particles, and then adding anhydrous ethanol calculated at a liquid-solid ratio of 0.26L:1kg, and ball milling for 30 hours at a ball milling speed of 37r / min and a ball-to-material ratio of 1.5:1 to obtain a slurry; the second ball milling: adding coarse tungsten carbide particles to the slurry, and adding anhydrous ethanol calculated at a liquid-solid ratio of 0.28L:1kg, ball milling for 10 hours at a ball milling speed of 15r / min and a ball-to-material ratio of 1.5:1, and spray drying after unloading to obtain a mixture.

[0087] S3, dewaxing and sintering the pressed green sheet to obtain a sintered green sheet; the pressed green sheet is dewaxed by a hydrogen dewaxing process to remove the paraffin molding agent, and the heating rate is controlled to be 0.2°C / min in the stage of 220-260°C; the sintering is divided into two sintering steps: the first sintering step: the sintering temperature is 1320°C, the pressurized sintering pressure is 10 bar, the sintering time is 30 minutes, and the pressed green sheet is taken out of the furnace after cooling; the second sintering step: the product taken out of the furnace is wrapped with wood pulp paper with a thickness of 0.3 mm, and then the calcined alumina is used to completely fill it for the second sintering step to obtain a sintered green sheet, argon is introduced at a sintering temperature of 1280°C to control the sintering pressure to 10 mbar, and high-pressure argon is introduced at a sintering temperature of 1400°C to control the pressurized sintering pressure to 30 bar, and the pressure and heat preservation time is 40 minutes.

[0088] S4, the sintered blank is subjected to quenching treatment, cryogenic treatment, and low-temperature tempering treatment. The quenching treatment process is as follows: the sintered blank is placed in a gas quenching furnace, and the temperature is increased from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, and the temperature is kept for 20 minutes. Then, the temperature is increased from 800°C to 1100°C at a heating rate of 3.75°C / min, and the temperature is kept for 30 minutes. Finally, 2 bar argon gas is filled to quickly cool to room temperature; the cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is cooled to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature; the low-temperature tempering process is as follows: the cryogenically treated product is placed in a vacuum furnace, and heated to 200°C at a heating rate of 1°C / min, and the temperature is kept for 4 hours, and then the furnace is stopped to allow it to cool to room temperature. A cemented carbide stamping die for high-hardness die steel stamping is obtained.

[0089] The pictures of the products obtained in this embodiment are as follows Figure 3 As shown, the average grain size of WC is 5 μm and the density is 11.72 g / cm 3 , hardness HRA is 78.6, and flexural strength is 2740MPa.

[0090] Comparative Example 1

[0091] The difference from Example 1 is that the tungsten carbide is medium-grained tungsten carbide and no secondary ball milling is performed.

[0092] The pictures of the products obtained in this comparative example are as follows Figure 4 As shown in the figure, the average grain size of WC is smaller than that of Example 1, the coarse particles of tungsten carbide are severely broken, and the fine particles of WC increase significantly after breaking. The average grain size of WC is 5 μm and the density is 12.54 g / cm 3 , hardness HRA is 80.7, and flexural strength is 2680MPa.

[0093] Comparative Example 2

[0094] The difference from Example 1 is that rare earth Ce which can provide the same amount of rare earth elements as ammonium cerium nitrate is used instead of ammonium cerium nitrate.

[0095] The pictures of the products obtained in this comparative example are as follows Figure 5 As shown in the figure, the rare earth Ce is an active metal and will react with water in the alcohol solution to form insoluble cerium hydroxide. This process is not conducive to safe production and the dispersion of cerium elements. The average grain size of WC is 7μm and the density is 12.55g / cm 3 , hardness HRA is 80.2, and flexural strength is 2650MPa.

[0096] Comparative Example 3

[0097] The difference from Example 1 is that the secondary sintering does not use wood pulp paper wrapping. Figure 6 As shown, after sintering, a large amount of alumina particles are attached to the surface of the product, the appearance quality is poor, and the mold repair process is required, which increases the production cost.

[0098] Comparative Example 4

[0099] The difference from Example 1 is that no quenching treatment is performed.

[0100] The pictures of the products obtained in this comparative example are as follows Figure 7 As shown in the figure, the content of solid tungsten in cobalt is lower than that of quenched product through SEM analysis, and the bending strength is lower than that of quenched product. The average grain size of WC is 7μm and the density is 12.52g / cm 3 , hardness HRA is 80.0, and flexural strength is 2570MPa.

[0101] Comparative Example 5

[0102] The difference from Example 1 is that no cryogenic treatment is performed.

[0103] The pictures of the products obtained in this comparative example are as follows Figure 8 As shown in the figure, the surface compressive stress and wear resistance of the product without cryogenic treatment are significantly lower than those of the product in Example 1. The average grain size of WC is 6 μm and the density is 12.54 g / cm 3 , hardness HRA is 80.1, and flexural strength is 2630MPa.

[0104] Comparative Example 6

[0105] The difference from Example 1 is that no tempering treatment is performed.

[0106] The pictures of the products obtained in this comparative example are as follows Fig. 9 As shown in the figure, the surface microhardness HV1 of the product without tempering treatment is lower than that of the tempered product, but the difference is not obvious when characterized by Rockwell hardness HRA. The average grain size of WC is 7μm and the density is 12.54g / cm 3 , hardness HRA is 80.0, and flexural strength is 2670MPa.

[0107] Comparative Example 7

[0108] The difference from Example 1 is that the heating rate in the dewaxing stage from 220°C to 260°C is controlled at 2°C / min.

[0109] The product obtained in this comparative example was found to be cracked after being sintered for the first time in step S3 and could not proceed to the subsequent steps.

[0110] It can be seen from the above embodiments and comparative examples that the present invention achieves synergistic strengthening of the binder phase and the hard phase by adding rare earth elements and additives such as chromium carbide and molybdenum carbide, in combination with a secondary sintering process and a heat treatment process; the WC average grain size of the prepared cemented carbide stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3 , hardness HRA is 78.0~81.0, and flexural strength is >2700MPa.

[0111] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a cemented carbide stamping die for high-hardness die steel stamping, characterized in that: The steps include: S1. Take tungsten carbide, a binder phase and additives to obtain a raw material. The tungsten carbide includes coarse-grained tungsten carbide and medium-grained tungsten carbide. The additives are chromium carbide, molybdenum carbide and ammonium cerium nitrate. The coarse-grained tungsten carbide has a Fischer-Tropsch particle size of 20-35 μm, and the medium-grained tungsten carbide has a Fischer-Tropsch particle size of 2.0-4.0 μm. The coarse-grained tungsten carbide accounts for 37.1-58.1 wt% of the raw material, and the medium-grained tungsten carbide accounts for 10-20 wt% of the raw material. S2, ball milling the raw materials, spray drying to obtain a mixture, and pressing the mixture to obtain a compact; the ball milling is divided into two ball millings: the first ball milling: using granular paraffin as a molding agent, the weight of which is 1.8-2.0wt% of the weight of the raw material, pre-grinding the granular paraffin for 10-20min, then adding all the components in the raw material except the coarse tungsten carbide particles, and then adding anhydrous ethanol calculated according to a liquid-solid ratio of (0.26-0.28) L: 1kg, and milling for 20-30h at a ball milling speed of 36-38r / min and a ball-to-material ratio of (1.2-1.5): 1 to obtain a slurry; the second ball milling: adding coarse tungsten carbide particles to the slurry, and adding anhydrous ethanol calculated according to a liquid-solid ratio of (0.26-0.28) L: 1kg, at a ball milling speed of 15-20r / min, a ball-to-material ratio of (1.2-1.5): 1 for 10-15h, and spray drying after unloading to obtain a mixture; S3, dewaxing and sintering the pressed green sheet to obtain a sintered green sheet; the pressed green sheet is dewaxed by a hydrogen dewaxing process to remove the paraffin molding agent, and the heating rate is controlled to be 0.2°C / min in the 220~260°C stage; the sintering is divided into two sintering steps: the first sintering step: the sintering temperature is 1320~1340°C, high-pressure argon is introduced for pressure sintering, the pressure is 10 bar, the sintering time is 30 minutes, and the product is taken out of the furnace after cooling; the second sintering step: the product taken out of the furnace is wrapped with wood pulp paper with a thickness of 0.2~0.3mm, and then the calcined alumina is used to completely fill it for the second sintering step to obtain a sintered green sheet, argon is introduced at a sintering temperature of 1280~1300°C, the sintering pressure is controlled to be 10~100mbar, and high-pressure argon is introduced at a sintering temperature of 1400~1420°C, the pressure of the pressure sintering is controlled to be 10~50bar, and the pressure and temperature holding time is 40~60min; S4. The sintered blank is subjected to quenching treatment, deep cryogenic treatment, and low temperature tempering treatment to obtain a cemented carbide stamping die for stamping high-hardness die steel.

2. The method for preparing a cemented carbide stamping die for high-hardness die steel stamping according to claim 1, characterized in that: In the step S1, the proportion of chromium carbide in the raw materials is 0.8-1.5wt%, the proportion of molybdenum carbide is 0.3-1.0wt%, and the proportion of ammonium cerium nitrate is 0.3-0.4wt%.

3. The method for preparing a cemented carbide stamping die for high-hardness die steel stamping according to claim 1, characterized in that: In the step S1, the binder phase is 0-1wt% nickel powder and the balance cobalt powder, and the binder phase accounts for 30-40wt% of the raw material.

4. The method for preparing a cemented carbide stamping die for high-hardness die steel stamping according to claim 1, characterized in that: In step S4, the quenching process is as follows: placing the sintered blank in a gas quenching furnace, heating the temperature from room temperature to 800°C at a heating rate of 3°C / min under a vacuum environment, keeping the temperature for 20 minutes, then heating the temperature from 800°C to 1100°C at a heating rate of 3.75°C / min, keeping the temperature for 30 minutes, and finally filling the furnace with 1-3 bar argon gas to rapidly cool the furnace to room temperature; The cryogenic treatment process is as follows: the quenched product is placed in a cryogenic treatment furnace, and the temperature is lowered to -190°C at a cooling rate of 0.8°C / min by controlling the flow rate of liquid nitrogen, and the temperature is kept for 150-200 minutes, and then the furnace is stopped to allow it to naturally return to room temperature; Low temperature tempering process: Place the product after deep cryogenic treatment in a vacuum furnace, heat it to 200°C at a heating rate of 1°C / min, keep it warm for 4 hours, and then stop the furnace to cool it to room temperature.

5. A cemented carbide stamping die for high-hardness die steel stamping, characterized in that: The die is prepared by the method for preparing a cemented carbide stamping die for high-hardness die steel stamping as described in any one of claims 1 to 4.

6. The hard alloy stamping die for high hardness die steel stamping according to claim 5, characterized in that: The WC average grain size of the hard alloy stamping die for high-hardness die steel stamping is 4-8 μm, and the density is 11.5-12.7 g / cm 3 , hardness HRA is 78.0~81.0, and flexural strength is >2700MPa.

Citation Information

Patent Citations

  • Method for preparing cemented carbides with nearly equiaxed WC crystal particle

    CN101397615B

  • Extra coarse grain WC-Co hard alloy and preparation process thereof

    CN102534344A

  • Hard alloy wear part and preparation method and application thereof.

    CN109468516A