A kind of cold heading steel high carbon wire rod for 14.9 grade bolts and its manufacturing method

By using overeutectoid chemical components containing Cr and online salt bath temperature control technology in cold heading steel strips for grade 14.9 bolts, the microstructure is controlled, and the problem of strength and plasticity is solved, and the cost and energy consumption is reduced. It is applicable. Manufactured in small specification bolts.

CN118621220BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110888.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-19
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The prior art is difficult to take into account both strength and plasticity when manufacturing cold-headed steel strips for grade 14.9 bolts, resulting in high material cost and low material yield, and cannot be suitable for small-sized bolt manufacturing. The existing methods require multiple processes and high energy. Consumption.

Method used

Using overeutectoid chemical composition design, combined with online salt bath temperature control and roller slow cooling technology, the microstructure of the control strip is tempered cordite and tempered pearlite, reducing network carbides and increasing carbon The use value of elements reduces tissue stress and dislocation density, and achieves strong plastic matching.

Benefits of technology

The strength and plasticity of cold-headed steel high-carbon carbon strips for grade 14.9 bolts are achieved, which reduces material costs, improves material yield, simplifies production process, is suitable for small-scale bolt manufacturing, reduces raw material losses and energy consumption .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621220B_ABST
    Figure CN118621220B_ABST
Patent Text Reader

Abstract

The invention relates to a cold heading steel high carbon wire rod for 14.9 grade bolts and a manufacturing method thereof. The invention comprises the following steps: based on a hypereutectoid Cr-containing chemical composition, controlled rolling and spinning to form a wire rod, online salt bath temperature control is performed, the wire rod is cooled to a pearlite phase region at a cooling rate of ≥37°C / s for isothermal phase transformation, secondary network carbon precipitation is controlled, the wire rod is controlled to form pearlite and troostite, and at the same time, the newly formed pearlite and troostite structures are promoted to undergo isothermal softening, and the carbides are transformed into spheroidized structures. Finally, the cold heading steel wire rod is manufactured through roller slow cooling, and the microstructure comprises a small portion of tempered pearlite, a large portion of tempered troostite, and the rest is quasi-spheroidized carbides. The wire rod is matched in strength and plasticity, the tensile strength can reach 1205-1255MPa, and the cross-sectional shrinkage can reach 40%-46%. The wire rod is used in the application fields of manufacturing 14.9 grade bolts, can effectively reduce material cost, improve yield rate, meet the manufacturing requirements of small-size bolts, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a cold-heading steel high-carbon wire rod for 14.9-grade bolts and a manufacturing method thereof. Background Art

[0002] Fasteners are important connecting parts with various types and wide applications. Their mechanical properties are mainly determined by the steel used for fasteners. Therefore, the selection of steel for fasteners is very important. It will not only affect the manufacturing efficiency and manufacturing cost of the product, but also affect the service life of the fasteners. With the improvement of the strength grade of the fasteners, it will also help the fasteners to be used in complex environments such as different temperatures, different pressures, and different loads. Due to the extremely high strength grade of cold heading steel for 14.9 grade bolts, the mechanical properties of heat treatment can reach: tensile strength Rm ≥ 1400MPa, yield strength ratio ≥ 0.9, and it is rarely developed. Steel is often produced by hot-rolled round steel through blanking, heat treatment and other processes to produce raw materials. For example: Patent CN110106443B discloses a method for producing round steel for ultra-high strength bolts, which uses a 42CrMo component system to produce hot-rolled round steel. Blanking and heat treatment are required to achieve the production of round steel for ultra-high strength bolts, or for example: Patent CN116287941B discloses a method for producing high-strength steel for wind power bolts , using the medium C-Si-Mn-Cr-Mo-V-Ni-Nb-Al composition system, round steel is produced under ultra-low temperature final rolling and slow cooling after rolling; this is because the cold heading steel for 14.9 grade bolts requires a stronger composition system, contains more strengthening alloys and / or micro-alloy components, has strong hardenability, and is prone to produce brittle phases. It is very easy to break when directly rolled into wire rods, so it is made into round steel and then annealed to improve the brittleness, but the cost of blanking is high and the time is long, resulting in low production efficiency and high energy consumption, or because the round steel specifications are large, they are only suitable for the manufacture of large-size bolts and cannot meet the manufacturing needs of small-size bolts.

[0003] For example, the patent CN113322410B discloses a high-strength bolt steel with excellent delayed fracture resistance and a preparation method thereof, which adopts a medium C-Mn-Cr-Mo-V-Si-Ti composition design and combines Stelmor fast-then-slow cooling to manufacture wire rods for manufacturing high-strength bolts with a tensile strength of not less than 1400MPa. However, the material cost is high after adding high alloy content and micro-alloy components. At the same time, ferrite + lamellar pearlite + bainite are obtained by rapid air cooling after rolling. Although bainite, as a hard and brittle phase, can improve the strength of the wire rod, it will significantly affect the plasticity of the wire rod, and easily cause the wire rod to break during the coiling process of the steel plant, the transportation process from the steel plant to the downstream users, and the coiling and unwinding process before the heat treatment of the downstream users, resulting in a large waste of raw materials, which is extremely unfavorable to the yield rate and cost control, and brings restrictions to the promotion and application. As a basic and relatively cheap strengthening component in steel, C can replace other alloys or microalloys to reduce material costs. However, compared with hypoeutectoid or eutectoid steel, hypereutectoid steel often contains more than 0.77% carbon. It has higher strength, hardness and wear resistance, but has greater deformation resistance. It is mainly used in bridge cables, cords and other fields. The technical difficulties and causes of its difficulty in cold heading for 14.9 grade bolts are:

[0004] (1) In order to increase the troostite content in the wire rod microstructure to improve the strength and drawing performance of the wire rod, the existing hypereutectoid steel wire rod will reduce the cooling speed of the wire rod after spinning. Under the slow cooling effect of the closed Stelmor wire insulation cover, the incubation time of the wire rod in the troostite phase region is extended, but the wire rod stays in the secondary cementite region for a long time, and the excessively high concentration of carbon precipitates in the form of carbides along the austenite grain boundaries to form network cementite, which destroys the continuity of the matrix. Reducing or eliminating network carbides through post-treatment will further increase the process and energy consumption. Severe network carbides cannot be eliminated in the subsequent spheroidizing annealing process and will remain after quenching and tempering, which can easily lead to drawing, cold heading cracking, quenching cracking or fatigue cracking during the use of bolts.

[0005] (2) Although the Stelmor wire insulation cover is closed to control the slow cooling phase transformation, the degree of supercooling of the wire rod entering the phase transformation temperature range is small during continuous cooling, which reduces the troostite nucleation rate and increases the grain growth rate. Therefore, the interlamellar spacing of the obtained troostite structure is large, which loses the strength of the wire rod. If the cold air cooling rate is further increased, there is a risk of forming bainite or even martensite structure due to the uneven air volume distribution and large temperature difference on the surface of the wire rod. At the same time, the time passing through the troostite phase region is still short. After the troostite structure is incubated, the wire rod is in a low temperature state, and the structure contains high stress and dislocation density. During cold working deformation, the increase in dislocations increases the material strength but reduces the elongation. The impact toughness is adversely affected with the increase in cold deformation. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a high-carbon carbon wire rod of cold heading steel for 14.9 grade bolts and a manufacturing method thereof. The wire rod is matched with the strength and plasticity of the wire rod by combining the hypereutectoid Cr-containing chemical composition design and organizational regulation. The wire rod can be used for the manufacture of 14.9 grade bolts, which is beneficial to reducing material costs, improving the yield rate and the scope of application.

[0007] The technical solution adopted by the present invention to solve the technical problem is:

[0008] A cold heading steel high carbon wire rod for 14.9 grade bolts, the chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.80%-0.84%, Si: 0.30%-0.50%, Mn: 0.53%-0.67%, Cr: 0.30%-0.40%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and the microstructure thereof includes a mixed structure consisting of tempered pearlite accounting for 21%-26% by volume, tempered troostite accounting for 70%-77% by volume, and the rest is quasi-spheroidized carbides.

[0009] The chemical composition and mass percentage design basis of the above-mentioned cold heading steel high carbon wire rod include:

[0010] (1) Carbon: The C element is cheaper than other elements in steel. As the main added element, C can play a role in solid solution strengthening and dispersion precipitation strengthening to ensure the matrix strength and high hardenability of the steel. However, it also increases the risk of decarburization and the risk of cementite distribution along the grain boundaries. In addition, if the C content is too high, there will be more carbides in the steel, and the resulting microstructure lamellae in the medium temperature range will be thicker, which is not conducive to the rapid spheroidization and softening of the matrix structure. Therefore, in order to facilitate microstructure control, ensure the cold deformation performance of cold heading steel wire rod, and meet the final performance level requirements of 14.9 grade bolts without adding microalloy components, the mass percentage of C is controlled to be 0.80%~0.84%.

[0011] (2) Silicon: The Si element is often added to steel as a deoxidizer during the smelting process. It can dissolve in austenite to achieve a solid solution strengthening effect, improve the hardness and strength of the steel, and inhibit grain coarsening in the initial stage of online salt bath temperature control. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization, and reduce the cold heading forming performance of the material. Therefore, the mass percentage of Si is controlled to be 0.30%~0.50%.

[0012] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. As an austenite stabilizing element, it can improve the strength and hardenability of steel. However, too high a Mn content will aggravate the segregation during the solidification of the steel billet, resulting in poor uniformity of the steel, increase the tendency of grain coarsening during the heating process of the material, reduce the activity of carbon and reduce the diffusion rate of carbon, which is not conducive to the spheroidization of carbides. Too high a Mn content will also increase the material cost. Therefore, the mass percentage of Mn is controlled to be 0.53%~0.67%.

[0013] (4) Chromium: Cr is an element that reduces the austenite phase area and can significantly increase the hardenability of steel. It can precipitate fine dispersed carbide particles through online salt bath temperature control, which plays a role in dispersion strengthening and improves the strength of the material. However, if the Cr content is too high, the temper brittleness tendency of the steel will increase, and the precipitation and coarsening of Cr is not conducive to the strength and plasticity of the wire rod. Therefore, the mass percentage of Cr is controlled to be 0.30%~0.40%.

[0014] (5) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0015] The above-mentioned cold heading steel high carbon wire rod is designed with a hypereutectoid Cr-containing chemical composition. The solid solution of carbon element and carbide precipitation strengthening can greatly improve the strength characteristics of the material. The alloy content is relatively small, no expensive micro-alloy components are added, and the hardenability of the components is regulated. The microstructure of the cold heading steel high carbon wire rod includes most of the tempered troostite. The troostite structure has finer interlamellar spacing and higher strength than the pearlite structure, which is beneficial to melting and spheroidization. Compared with the bainite structure, the distortion and dislocation density are smaller and the plasticity is higher. The high carbon Cr-containing carbon component system and the pearlite structure provide higher matrix strength and appropriate plasticity, which can make up for the strength loss of not utilizing micro-alloy strengthening and bainite structure. After being tempered and converted into tempered troostite, the dislocation density of the structure is further reduced, so that the tempered troostite further improves the plasticity, toughness and drawing properties compared with the troostite structure.

[0016] The microstructure also includes a small amount of tempered pearlite and quasi-spheroidized carbides. Compared with the troostite structure, the pearlite has a coarser interlamellar spacing and higher plasticity, and has a higher strength than the ferrite structure. After being tempered and converted into tempered pearlite, the stress and dislocation density of the structure are further reduced, so that the tempered pearlite has higher plasticity and drawing properties than the pearlite structure. During the tempering process, the troostite and cementite lamellae are melted and transformed into spheroidized structure, and a certain amount of fine and uniform quasi-spheroidized carbides are obtained, which further softens the matrix structure. Compared with the wire rod with a mixed structure of ferrite, pearlite and bainite in the existing microstructure, it does not contain hard and brittle phase structure, which can significantly improve the plasticity of the wire rod and avoid its The brittleness makes the wire rod not easy to break during the coiling, transportation and downstream unwinding process, which greatly improves the yield rate and reduces the raw material loss. As a result, round steel can be directly rolled and spun into wire rods without making them, which simplifies the process and speeds up the production process. It is also more convenient for the manufacture of small-sized bolts. Compared with the existing high-carbon steel wire rod structure with a high sorbitization rate, the cold heading steel high-carbon carbon wire rod also has lower organizational stress and dislocation density, which can effectively reduce drawing hardening, and finally achieve strength-plasticity matching of the wire rod, breaking the application restrictions of high-carbon carbon components in the field of cold heading of 14.9 grade bolts. In cold working deformation, it can significantly reduce material costs, improve yield rate and scope of application.

[0017] In a preferred embodiment, the lamellar spacing of the tempered pearlite is 150-180 nm, and the lamellar spacing of the tempered troostite is 80-110 nm. The smaller the lamellar spacing, the better for improving the strength of the wire rod.

[0018] In a preferred embodiment, the network carbide level of the cold heading steel high carbon carbon wire rod is level 0, which has a lower network carbide level than the existing high carbon carbon wire rod, can improve the continuity of the matrix, avoid the difficulty in eliminating and residual problems of network carbides, and further reduce the risks of wire breakage during drawing, cold heading cracking and fatigue cracks caused by network carbides.

[0019] In a preferred embodiment, the diameter of the cold heading steel high carbon wire rod is 16.0~26.0mm, the tensile strength Rm is 1205~1255MPa, the cross-sectional shrinkage rate Z is 40%~46%, and it has a relatively thin wire rod diameter, which is more convenient for the manufacture of small-sized bolts. At the same time, it has high tensile strength, small fluctuations in mechanical properties, and significantly improved wire rod plasticity, which can effectively reduce the risks of wire breakage during drawing and cracking during cold heading, thereby reducing the cost pressure of steel mills and downstream users, and is easier to promote and apply.

[0020] A method for manufacturing a cold heading steel high carbon wire rod for 14.9 grade bolts, the manufacturing method comprising:

[0021] According to the chemical composition of the cold heading steel high carbon wire rod for 14.9 grade bolts described above, the wire rod is produced by controlled rolling. After the wire rod is spun into a wire rod at a spinning temperature of ≥925°C, an online salt bath temperature control is performed to cool the wire rod to the pearlite phase region at a cooling rate of ≥37°C / s for isothermal phase transformation, and the wire rod is controlled to form a small part of pearlite and a large part of troostite, while promoting the isothermal softening of the newly formed pearlite and troostite structures, and the transformation of carbides to spheroidized structures. Finally, it is slowly cooled by a roller to form a cold heading steel wire rod with a microstructure including 21% to 26% by volume of tempered pearlite, 70% to 77% by volume of tempered troostite, and the rest being a mixed structure composed of quasi-spheroidized carbides.

[0022] The above manufacturing method utilizes the carbon element to extremely enhance the strength characteristics of the material. At the same time, the wire rod after spinning is directly subjected to online salt bath temperature control, and the efficient heat exchange capacity of the molten salt is utilized to rapidly cool the wire rod from the spinning temperature to the pearlite phase temperature. On the one hand, compared with the Stelmor strong air cooling process after low-temperature spinning, it can skip the ferrite precipitation temperature range at a faster speed, effectively reduce the residence time of the wire rod in the secondary cementite range, and control the secondary network carbon precipitation through rapid cooling technology, eliminate the network carbon deterioration phase caused by excessive carbon elements, and enhance the use value of the carbon element.

[0023] On the other hand, entering the pearlite phase region with a greater degree of undercooling is beneficial to the transformation of austenite structure into a troostite structure with finer interlamellar spacing. It can control the formation of troostite in large quantities in the wire rod, provide matrix strength and basic toughness, and use the consistency of the wire rod temperature with the molten salt temperature to extend the high-temperature isothermal time, rather than the Stellmor insulation and slow cooling continuous cooling. By extending the high-temperature state of the wire rod in the pearlite phase region, the incubation of the newly formed pearlite and troostite structures is promoted, and the tissue stress and dislocation density caused by rapid cooling are further reduced under high-temperature isothermal conditions. At the same time, at a longer phase temperature, the diffusion of carbon is accelerated, which promotes the melting of troostite lamellae and cementite lamellae, transforming to spheroidized structure, softening the matrix, and regulating the tempering state.

[0024] After the wire rod is fully transformed into tempered pearlite and tempered bainite structure, the formation of hard and brittle phases of bainite or martensite in the structure is also avoided. Finally, after roller slow cooling, the high temperature state of the wire rod after online salt bath temperature control treatment can be utilized to further soften the matrix structure. At the same time, compared with extending the isothermal time of the wire rod in the pearlite phase region, the use of roller slow cooling can reduce energy consumption, avoid the precipitation and coarsening of Cr caused by online salt bath isothermal, or excessive softening and difficulty in controlling the wire rod structure performance, and finally realize the regulation of wire rod structure and strength and plasticity to meet the needs of manufacturing 14.9 grade bolts and other application fields.

[0025] In a preferred embodiment, during the controlled rolling, the steel billet soaking temperature is controlled to be ≤1100°C before rolling, the soaking time is 2-3h, and the time in the furnace is ≤4.5h. This promotes uniform diffusion of high-carbon carbon components under high temperature and reduces segregation. At the same time, a lower steel billet soaking temperature and a shorter time in the furnace are selected to prevent aggravation of high-temperature decarburization and avoid growth of austenite grains.

[0026] In a preferred embodiment, the controlled rolling adopts low-temperature controlled rolling, the initial rolling temperature is controlled to 1060~1090℃, the initial rolling reduction is 35%~45%, and a lower initial rolling temperature is selected to ensure effective control of the rolling temperature to prevent the recrystallization grains from coarsening and destroying the toughness of the steel.

[0027] In a preferred embodiment, the final rolling temperature is controlled to be ≥940°C, the final rolling reduction is 30%~40%, and a lower final rolling temperature and a higher final rolling reduction are selected. The austenite grains are refined through repeated deformation and recrystallization, the overall grain refinement effect is improved, the grain size is ≥10 levels, and the wire rod matrix is ​​strengthened and toughened.

[0028] In a preferred embodiment, the final rolling temperature is 940-970° C., and the spinning temperature is 925-950° C., which further avoids the coarsening of austenite grains and is beneficial to the nucleation of pearlite and troostite and the refinement of the interlamellar spacing.

[0029] In a preferred embodiment, the online salt bath temperature control controls the molten salt temperature to 500-550°C, and the processing time is 250-450s. The lower the molten salt temperature during the online salt bath temperature control process, the higher the content of austenite structure transformed into troostite, the finer the lamellar spacing of tempered troostite, the increased strength of the wire rod and the decreased plasticity, which is beneficial to the rapid melting of the lamellar layers and the transformation to spheroidized structure. However, if the molten salt temperature is too low, the troostite content is too high and the lamellar layers are too fine, which is not conducive to the plasticity of the matrix structure. If the molten salt temperature is too low, there is a risk of the appearance of bainite brittle phase. On the contrary, the higher the molten salt temperature, the higher the content of austenite structure transformed into pearlite, the coarser the lamellar spacing of tempered pearlite, and the wire rod strength. The decrease in matrix softening effect and the increase in plasticity are beneficial to reducing the organizational stress and dislocation density. However, the molten salt temperature is too high and the tempered pearlite content in the organization is too high, which is not conducive to the strength of the wire rod. If the molten salt temperature is too high, there is a risk of failure to form troostite and an increase in soft-phase ferrite. The longer the treatment time, the more obvious the matrix softening effect, the decrease in wire rod strength and increase in plasticity. However, if the treatment time is too long, there is a risk of Cr precipitation coarsening and quasi-spheroidized carbide agglomeration and growth, which will cause a significant decrease in the strength and plasticity of the wire rod. Therefore, the molten salt temperature and treatment time can be further controlled, the content of tempered pearlite and tempered troostite in the wire rod can be controlled, the dispersion precipitation of carbides and the transformation to spheroidization can be controlled, and the organization and strength and plasticity of the wire rod can be better regulated.

[0030] In a preferred embodiment, the online salt bath temperature control controls the molten salt circulation rate to 450~650t / h, and the molten salt temperature rise is ≤9°C. The molten salt circulation rate can be further controlled to control the molten salt temperature rise, maintain the processing accuracy of the online salt bath temperature control, and avoid excessive temperature rise that is unfavorable to tissue regulation.

[0031] In a preferred embodiment, the online salt bath temperature control controls the roller conveying speed to 16~30m / min. When the wire rod is conveyed through the molten salt by rollers, the roller speed can be further controlled to control the time for the wire rod to pass through the molten salt, thereby promoting uniform heat exchange.

[0032] In a preferred embodiment, the roller slow cooling adopts a heat preservation cover to close, and the wire rod is controlled to be cooled to below 300°C at a cooling rate of 0.35~0.65°C / s until it is coiled. A lower cooling rate is used to control the wire rod after online molten salt temperature control to maintain slow cooling, promote further softening of tempered pearlite and tempered troostite structures, and obtain more quasi-spheroidized carbides to improve the plasticity of the wire rod.

[0033] Compared with the prior art, the beneficial effects of the present invention are at least:

[0034] (1) Aiming at the current situation that only round steel can be manufactured, resulting in many processes and being unfavorable for the manufacture of small-size bolts, or the addition of microalloy components and bainite structure leads to high wire rod cost, low plasticity and yield rate, the cold heading steel high carbon wire rod for 14.9 grade bolts of the present invention adopts a hypereutectoid Cr-containing chemical composition design, utilizes carbon elements and precipitation strengthening to greatly improve the material strength characteristics, maintains the hardenability of the material to prepare for subsequent tempering to achieve the final performance level, and the microstructure type includes a mixed structure composed of mainly tempered troostite, a small amount of tempered pearlite and quasi-spheroidized carbide, so as to achieve the strength and plasticity matching of the wire rod, and the tensile strength Rm of the wire rod with a diameter of 16.0~26.0mm can reach 1205~1255MPa, and the cross-sectional shrinkage Z can reach 40%~46%. It is used in the manufacture of 14.9 grade bolts and other application fields, can effectively reduce material costs, improve yield rate, meet the manufacturing needs of small-size bolts, and has good application prospects.

[0035] (2) The manufacturing method of the present invention adopts a hypereutectoid Cr-containing chemical composition design, combined with an online salt bath temperature control and roller slow cooling technology process design. Through the rapid cooling technology, the network carbon deterioration phase caused by excessive carbon elements is eliminated, and the use value of the carbon element is improved. At the same time, the wire rod is controlled to form a large amount of troostite, and the newly formed pearlite and troostite structures are promoted to be isothermal at high temperature, and the carbides are transformed into spheroidized structures, softening the matrix, and avoiding the precipitation and coarsening of Cr and the agglomeration and growth of quasi-spheroidized carbides. The hot-rolled wire rod structure performance is regulated, and the high-carbon carbon wire rod of cold heading steel for 14.9 grade bolts is successfully developed. The process is simple and has good industrial adaptability.

[0036] (3) The present invention adopts low-temperature heating rolling to prevent the aggravation of high-temperature decarburization and the coarsening of recrystallized grains, thereby improving the overall grain refinement effect, further strengthening the matrix, and at the same time avoiding excessively low rolling temperatures that aggravate the wear of the rolling line, thereby improving the rolling speed and efficiency and having good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0038] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0039] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0040] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0041] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0042] A preferred embodiment of the manufacturing method of the cold heading steel high carbon wire rod for 14.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.82%, Si: 0.39%, Mn: 0.53%, Cr: 0.38%, P: 0.012%, S: 0.014%, and the manufacturing method thereof is manufactured according to the process flow of low temperature heating rolling → wire laying → online salt bath temperature control → roller slow cooling → coiling, specifically:

[0043] The low temperature heating rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high carbon carbon components under high temperature, reduce segregation, and avoid the risk of decarburization and austenite grain growth. After heating to achieve high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into wire with a diameter of 24mm through a rolling line. Low temperature controlled rolling is used to prevent coarsening of recrystallized grains, improve the overall grain refinement effect, strengthen and toughen the wire rod matrix, and create favorable conditions for pearlite and troostite nucleation and refinement of lamellar spacing. Specifically: the heating procedure of the heating furnace is preheating section, heating section and soaking section in sequence. The soaking temperature of the steel billet is controlled to be 1095℃, the soaking time is 2.5h, the time in the furnace is 4.5h, the initial rolling temperature is 1080℃, the initial rolling reduction is 38%, the final rolling temperature is 960℃, the final rolling reduction is 32%, and the grain size is ≥10 grades.

[0044] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller to avoid the precipitation of network carbides in the wire rod during the spinning stage, reduce the tendency of grain growth, and create conditions for forming a larger undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 940°C.

[0045] The online salt bath temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 38°C / s for isothermal phase transformation, eliminating the network carbon deterioration phase caused by excessive carbon element, improving the use value of carbon element, controlling the wire rod to form a small part of pearlite and most of troostite, and promoting the newly formed pearlite and troostite structure to undergo isothermal softening, reducing the structure stress and dislocation density, and the carbide is transformed into a spheroidized structure, softening the matrix, avoiding the precipitation and coarsening of Cr and the agglomeration and growth of quasi-spheroidized carbides. Specifically: the molten salt temperature is controlled to be 535°C, the processing time is 450s, the molten salt circulation volume is 500t / h, the molten salt temperature rise is ≤9°C, and the roller conveying speed is 16m / min.

[0046] The roller slow cooling process is closed with a heat preservation cover, and the wire rod coming out of the salt bath tank is conveyed by a roller into the heat preservation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 285°C at a cooling rate of 0.5°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a finished product of cold heading steel high carbon wire rod is obtained, and its metallographic structure diagram is as follows Figure 1 shown.

[0047] Comparative Example 1:

[0048] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire drawing → Stelmor insulation and slow cooling → coiling, specifically: the steel billet uniform heating temperature is controlled to be 1050°C, the uniform heating time is 3h, the furnace time is 5h, the initial rolling temperature is 1035°C, the final rolling temperature is 910°C, the wire drawing temperature is 890°C, the Stelmor insulation and slow cooling adopts closing all fans and insulation covers, and the wire rod is conveyed by rollers, the wire rod completes phase change in the cover at a cooling rate of 1.6°C / s, and the finished wire rod is obtained after coiling off the line.

[0049] Comparative Example 2:

[0050] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling → roller slow cooling → coiling. Specifically: the Stelmor rapid cooling is performed by opening 1~6# fans at 65%, so that the wire rod is cooled to 670°C at a cooling rate of 4.5°C / s; the roller slow cooling is performed by closing all fans and insulation covers, so that the wire rod completes a phase change at a cooling rate of 1.4°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0051] Comparative Example 3:

[0052] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of controlled rolling → wire laying → Stelmor rapid cooling → roller slow cooling, specifically: controlling the steel billet soaking temperature to 1120°C, the soaking time to 2h, the furnace time to 4h, the initial rolling temperature to 1105°C, the final rolling temperature to 985°C, the wire laying temperature to 965°C, the Stelmor rapid cooling adopts opening 1~7# fans at 95%, so that the wire rod is cooled to 655°C at a cooling rate of 9.5°C / s, the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after going offline.

[0053] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0054] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0055]

[0056] From the comparison results of Example 1 and Comparative Example 1, it can be seen that the eutectic carbon chemical composition design is adopted without adding high alloy content and expensive micro-alloy components. Compared with the troostite and ferrite structures obtained by low-temperature rolling and wire spinning followed by insulation cooling, although the wire rod strength is higher, the network carbide level is higher and the dislocation density of the troostite structure is higher, resulting in insufficient plasticity of the wire rod. The cold heading steel high carbon wire rod of the present invention is based on the eutectic carbon chemical composition, combined with online salt bath temperature control and roller strong slow cooling technology, to control the wire rod to quickly enter the pearlite phase region with a large degree of supercooling for strong isothermal phase transformation, to avoid the wire rod staying in the secondary cementite range and the tertiary cementite peak range for a long time, the network carbide level can reach level 0, and the pearlite and troostite content of the wire rod is controlled, to promote high-temperature tempering of the pearlite and troostite structures, and to effectively reduce the tissue stress and dislocation density.

[0057] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with increasing the cooling rate of the wire rod after spinning, but the spacing between the tissue lamellae is larger, and the stress is higher and cannot be eliminated, resulting in strength degradation, and the plasticity is still insufficient, the present invention enters the pearlite phase region with a larger degree of supercooling, which is beneficial to the transformation of the austenite structure into a troostite structure with finer troostite spacing. It can control the wire rod to form a large amount of troostite, provide matrix strength and basic toughness, and at a longer phase temperature, it can promote the melting of troostite lamellae and cementite lamellae, transform to spheroidized structure, soften the matrix, and regulate the tempering state.

[0058] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with further increasing the spinning temperature and the cooling rate after spinning to improve the network carbon level, the organization produces hard and brittle bainite, and although the strength is higher, the plasticity is significantly reduced. After the wire rod is fully transformed into tempered pearlite and tempered troostite organization, the present invention also avoids the organization from producing hard and brittle bainite or martensite, and finally realizes the regulation of the wire rod organization and strength and plasticity. Embodiment 2:

[0059] A preferred embodiment of the manufacturing method of the cold heading steel high carbon wire rod for 14.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.84%, Si: 0.5%, Mn: 0.59%, Cr: 0.4%, P: 0.015%, S: 0.015%, and the manufacturing method thereof is manufactured according to the process flow of low temperature heating rolling → wire laying → online salt bath temperature control → roller slow cooling → coiling, specifically:

[0060] The low temperature heating rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high carbon carbon components under high temperature, reduce segregation, and avoid the risk of decarburization and austenite grain growth. After heating to achieve high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into wire with a diameter of 26mm through a rolling line. Low temperature controlled rolling is used to prevent coarsening of recrystallized grains, improve the overall grain refinement effect, strengthen and toughen the wire rod matrix, and create favorable conditions for pearlite and troostite nucleation and refinement of lamellar spacing. Specifically: the heating procedure of the heating furnace is preheating section, heating section and soaking section in sequence. The soaking temperature of the steel billet is controlled to be 1100℃, the soaking time is 3h, the time in the furnace is 4.5h, the initial rolling temperature is 1090℃, the initial rolling reduction is 35%, the final rolling temperature is 970℃, the final rolling reduction is 30%, and the grain size is ≥10 grades.

[0061] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism, and the wire rod is spread on a roller and transported along the roller to avoid the precipitation of network carbides in the wire rod during the spinning stage, reduce the tendency of grain growth, and create conditions for forming a larger undercooling and sorbite nucleation. Specifically: the spinning temperature is controlled to be 950°C.

[0062] The online salt bath temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 37°C / s for isothermal phase transformation, eliminating the network carbon deterioration phase caused by excessive carbon element, improving the use value of carbon element, controlling the wire rod to form a small part of pearlite and most of troostite, and promoting the newly formed pearlite and troostite structure to undergo isothermal softening, reducing the structure stress and dislocation density, and the carbide is transformed into a spheroidized structure, softening the matrix, avoiding the precipitation coarsening of Cr and the agglomeration and growth of quasi-spheroidized carbides. Specifically: the molten salt temperature is controlled to be 550°C, the processing time is 395s, the molten salt circulation volume is 450t / h, the molten salt temperature rise is ≤9°C, and the roller conveying speed is 21m / min.

[0063] The roller slow cooling process is closed with a heat preservation cover, and the wire rod coming out of the salt bath tank is conveyed by rollers into the heat preservation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 295°C at a cooling rate of 0.6°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a finished product of cold heading steel high carbon wire rod is obtained, and its metallographic structure diagram is as follows Figure 2 shown.

[0064] Comparative Example 4:

[0065] A method for manufacturing a wire rod, which differs from that of Example 2 in that the steel billet soaking temperature is controlled to be 1105°C, the initial rolling temperature is 1095°C, the final rolling temperature is 975°C, the spinning temperature is 915°C, the wire rod is cooled at a cooling rate of 35°C / s to the pearlite phase region for isothermal phase transformation, and a finished wire rod is obtained after it comes off the production line.

[0066] Comparative Example 5:

[0067] A method for manufacturing a wire rod, which differs from Example 2 in that the wire rod is cooled at a cooling rate of 36°C / s to a pearlite phase region for isothermal phase transformation, the molten salt temperature is 575°C, and a finished wire rod is obtained after the wire rod is off the line.

[0068] Comparative Example 6:

[0069] A method for manufacturing a wire rod, which differs from Example 2 in that the wire rod is cooled at a cooling rate of 41°C / s to the pearlite phase region for isothermal phase transformation, the molten salt temperature is 495°C, the molten salt circulation rate is 550t / h, and the finished wire rod is obtained after it comes off the line. Embodiment 3:

[0070] A preferred embodiment of the manufacturing method of the cold heading steel high carbon wire rod for 14.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.82%, Si: 0.46%, Mn: 0.62%, Cr: 0.3%, P: 0.014%, S: 0.015%, and the manufacturing method thereof is manufactured according to the process flow of low temperature heating rolling → wire laying → online salt bath temperature control → roller slow cooling → coiling, specifically:

[0071] The low temperature heating rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high carbon carbon components under high temperature, reduce segregation, and avoid the risk of decarburization and austenite grain growth. After heating to achieve high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into wire with a diameter of 22mm through a rolling line. Low temperature controlled rolling is used to prevent coarsening of recrystallized grains, improve the overall grain refinement effect, strengthen and toughen the wire rod matrix, and create favorable conditions for pearlite and troostite nucleation and refinement of lamellar spacing. Specifically: the heating procedure of the heating furnace is preheating section, heating section and soaking section in sequence. The soaking temperature of the steel billet is controlled to be 1090℃, the soaking time is 2.5h, the time in the furnace is 4h, the initial rolling temperature is 1075℃, the initial rolling reduction is 40%, the final rolling temperature is 955℃, the final rolling reduction is 37%, and the grain size is ≥10 grades.

[0072] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller to avoid the precipitation of network carbides in the wire rod during the spinning stage, reduce the tendency of grain growth, and create conditions for forming a larger undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 935°C.

[0073] The online salt bath temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 39°C / s for isothermal phase transformation, eliminating the network carbon deterioration phase caused by excessive carbon element, improving the use value of carbon element, controlling the wire rod to form a small part of pearlite and most of troostite, and promoting the newly formed pearlite and troostite structure to undergo isothermal softening, reducing the structure stress and dislocation density, and the carbide is transformed into a spheroidized structure, softening the matrix, avoiding the precipitation and coarsening of Cr and the agglomeration and growth of quasi-spheroidized carbides. Specifically: the molten salt temperature is controlled to be 515°C, the processing time is 305s, the molten salt circulation volume is 580t / h, the molten salt temperature rise is ≤9°C, and the roller conveying speed is 26m / min.

[0074] The roller slow cooling process is closed with a heat preservation cover, and the wire rod coming out of the salt bath tank is conveyed by rollers into the heat preservation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 295°C at a cooling rate of 0.45°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a finished product of cold heading steel high carbon wire rod is obtained, and its metallographic structure diagram is as follows Figure 3 shown.

[0075] Comparative Example 7:

[0076] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online salt bath temperature control is controlled to be 200s, the roller conveying speed is 32m / min, and the finished wire rod is obtained after going offline.

[0077] Comparative Example 8:

[0078] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online salt bath temperature control is controlled to be 500s, the roller conveying speed is 15m / min, and the finished wire rod is obtained after going offline.

[0079] Comparative Example 9:

[0080] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online salt bath temperature control is controlled to be 570s, the roller conveying speed is 14m / min, and the finished wire rod is obtained after going offline. Embodiment 4:

[0081] A preferred embodiment of the manufacturing method of the cold heading steel high carbon wire rod for 14.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.8%, Si: 0.3%, Mn: 0.67%, Cr: 0.37%, P: 0.014%, S: 0.013%, and the manufacturing method thereof is manufactured according to the process flow of low temperature heating rolling → wire laying → online salt bath temperature control → roller slow cooling → coiling, specifically:

[0082] The low temperature heating rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high carbon carbon components under high temperature, reduce segregation, and avoid the risk of decarburization and austenite grain growth. After heating to achieve high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into wire with a diameter of 16mm through a rolling line. Low temperature controlled rolling is used to prevent coarsening of recrystallized grains, improve the overall grain refinement effect, strengthen and toughen the wire rod matrix, and create favorable conditions for pearlite and troostite nucleation and refinement of lamellar spacing. Specifically: the heating procedure of the heating furnace is preheating section, heating section and soaking section in sequence. The soaking temperature of the steel billet is controlled to be 1070℃, the soaking time is 2h, the time in the furnace is 4h, the initial rolling temperature is 1060℃, the initial rolling reduction is 45%, the final rolling temperature is 940℃, the final rolling reduction is 40%, and the grain size is ≥10 grades.

[0083] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller to avoid the precipitation of network carbides in the wire rod during the spinning stage, reduce the tendency of grain growth, and create conditions for forming a larger undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 925°C.

[0084] The online salt bath temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 39°C / s for isothermal phase transformation, eliminating the network carbon deterioration phase caused by excessive carbon element, improving the use value of carbon element, controlling the wire rod to form a small part of pearlite and most of troostite, and promoting the newly formed pearlite and troostite structure to undergo isothermal softening, reducing the structure stress and dislocation density, and the carbide is transformed into a spheroidized structure, softening the matrix, avoiding the precipitation and coarsening of Cr and the agglomeration and growth of quasi-spheroidized carbides. Specifically: the molten salt temperature is controlled to be 500°C, the processing time is 250s, the molten salt circulation volume is 650t / h, the molten salt temperature rise is ≤9°C, and the roller conveying speed is 30m / min.

[0085] The roller slow cooling process is closed with an insulation cover, and the wire rod coming out of the salt bath tank is transported by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled to 290°C at a cooling rate of 0.35°C / s; the coiling process is used to coil the wire rod into coils through a coiling drum, and after packaging and storage, the finished cold heading steel high carbon wire rod is obtained.

[0086] Comparative Example 10:

[0087] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of low-temperature heating rolling → spinning → online salt bath temperature control → air cooling → coiling. Specifically: the roller slow cooling process uses a heat preservation cover to open, and the wire rod coming out of the salt bath tank is transported by a roller, and the wire rod is controlled to be cooled to 290°C at a cooling rate of 2.3°C / s, and the finished wire rod is obtained after it comes off the line.

[0088] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0089] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0090]

[0091] It can be seen from the results of Examples 1 to 4 that the tensile strength Rm of the wire rod with a diameter of 16.0 to 26.0 mm can reach 1205 to 1255 MPa, and the cross-sectional shrinkage Z can reach 40% to 46%. It is used in the manufacture of 14.9 grade bolts and other application fields, which can effectively reduce material costs, increase the yield rate, meet the manufacturing needs of small-size bolts, and has good application prospects.

[0092] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the low-temperature heating rolling is used to prevent the aggravation of high-temperature decarburization and the coarsening of recrystallized grains, improve the overall grain refinement effect, and further strengthen the matrix.

[0093] From the comparison results of Examples 1 to 4 and Comparative Example 5, it can be seen that the higher the molten salt temperature, the higher the content of austenite structure transformed into pearlite, the coarser the lamellar spacing of tempered pearlite, the lower the strength of the wire rod and the higher the plasticity, which is beneficial to reducing the organizational stress and dislocation density, but the molten salt temperature is too high, and the content of tempered pearlite in the organization is too high, which is not conducive to the strength of the wire rod; from the comparison results of Examples 1 to 4 and Comparative Example 6, it can be seen that the lower the molten salt temperature, the higher the content of austenite structure transformed into troostite, the finer the lamellar spacing of tempered troostite, the higher the strength of the wire rod and the lower the plasticity, which is beneficial to the rapid melting of the troostite to the spheroidized organization, but the molten salt temperature is too low, the content of troostite is too high, and the troostite is too fine, which is not conducive to the plasticity of the matrix organization.

[0094] From the comparison results of Examples 1 to 4 and Comparative Example 7, it can be seen that if the treatment time is too short, the matrix softening effect will be significantly reduced; from the comparison results of Examples 1 to 4 and Comparative Example 8, it can be seen that the longer the treatment time, the more obvious the matrix softening effect, the wire rod strength decreases and the plasticity increases; from the comparison results of Example 3 and Comparative Example 9, it can be seen that if the treatment time is too long, there is a risk of Cr precipitation coarsening and quasi-spheroidized carbide agglomeration and growth, which will cause a significant decrease in the strength and plasticity of the wire rod.

[0095] From the comparison results of Example 4 and Comparative Example 10, it can be seen that after slow cooling on a roller, the high temperature state of the wire rod after the online salt bath temperature control treatment can be utilized to further soften the matrix structure.

[0096] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on steelmaking raw materials. Any equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A cold heading steel high carbon wire rod for 14.9 grade bolts, characterized in that: The chemical composition and mass percentage of the cold heading steel high carbon wire rod include: C: 0.80%~0.84%, Si: 0.30%~0.50%, Mn: 0.53%~0.67%, Cr: 0.30%~0.40%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities, and its microstructure includes tempered pearlite accounting for 21%~26% by volume, tempered troostite accounting for 70%~77% by volume, and the rest is a mixed structure composed of quasi-spheroidized carbides; The manufacturing method comprises: producing a wire rod by controlled rolling according to the chemical composition of the cold heading steel high carbon wire rod for 14.9 grade bolts, after the wire rod is spun into a wire rod at a spinning temperature of ≥925°C, performing online salt bath temperature control, cooling the wire rod to the pearlite phase region at a cooling rate of ≥37°C / s for isothermal phase transformation, controlling the wire rod to form a small part of pearlite and a large part of troostite, and promoting the newly formed pearlite and troostite structures to undergo isothermal softening, and the carbide to transform into a spheroidized structure, and finally slowly cooling through a roller to produce a cold heading steel wire rod with a microstructure including a mixed structure composed of tempered pearlite, tempered troostite and quasi-spheroidized carbide; the online salt bath temperature control controls the molten salt temperature to 500-550°C, and the processing time is 250-450s.

2. The cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 150-180 nm, the interlamellar spacing of the tempered troostite is 80-110 nm, and the network carbide level of the cold heading steel high carbon wire rod is level 0.

3. The cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 1 or 2, characterized in that: The cold heading steel high carbon wire rod has a diameter of 16.0-26.0 mm, a tensile strength of 1205-1255 MPa, and a cross-sectional shrinkage of 40%-46%.

4. A method for manufacturing cold heading steel high carbon wire rod for 14.9 grade bolts, characterized in that: The manufacturing method thereof comprises: According to the chemical composition controlled rolling production line of the 14.9 grade cold heading steel high carbon wire rod for bolts as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥925°C, an online salt bath temperature control is performed to cool the wire rod to the pearlite phase region at a cooling rate of ≥37°C / s for isothermal phase transformation, and the wire rod is controlled to form a small part of pearlite and a large part of troostite, while promoting the newly formed pearlite and troostite structures to undergo isothermal softening and the carbide to transform into a spheroidized structure, and finally slowly cooled by a roller to produce a cold heading steel wire rod with a microstructure including 21% to 26% by volume of tempered pearlite, 70% to 77% by volume of tempered troostite, and the rest being a mixed structure composed of quasi-spheroidized carbides; the online salt bath temperature control controls the molten salt temperature to 500 to 550°C, and the processing time is 250 to 450s.

5. The method for manufacturing cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 4, characterized in that: During the controlled rolling, the steel billet soaking temperature is controlled to be ≤1100°C before rolling, the time in the furnace is ≤4.5h, and the soaking time is 2-3h.

6. The method for manufacturing the cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 4, characterized in that: The controlled rolling adopts low temperature controlled rolling, controls the initial rolling temperature to be 1060-1090°C, the initial rolling reduction to be 35%-45%, the final rolling temperature to be ≥940°C, and the final rolling reduction to be 30%-40%.

7. The method for manufacturing the cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 6, characterized in that: The final rolling temperature is 940-970°C, and the spinning temperature is 925-950°C.

8. The method for manufacturing cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 4, characterized in that: The online salt bath temperature control controls the molten salt circulation volume to 450-650t / h, the molten salt temperature rise is ≤9°C, and the roller conveying speed is 16-30m / min.

9. The method for manufacturing cold heading steel high carbon wire rod for 14.9 grade bolts according to claim 4, characterized in that: The roller slow cooling is closed with a heat preservation cover, and the wire rod is controlled to be cooled to below 300°C at a cooling rate of 0.35-0.65°C / s.