Cement kiln high temperature flue gas purification absorbent and preparation method thereof

By combining the modified calcium-based solid waste carbide slag with coal gangue and fly ash, a high-efficiency absorber is prepared, which solves the problem of low removal efficiency of CO2, SO2 and NOX in the flue gas of the cement industry, and achieves high-temperature flue gas removal. Collaborative purification and solid waste disposal have good economic and environmental benefits.

CN118634633BActive Publication Date: 2024-10-25BEIJING UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411106348.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-25
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing cement industry's removal of CO2, SO2 and NOX from flue gas has problems such as complex equipment, cumbersome operations, high costs and secondary pollution. Moreover, the efficiency of carbide slag absorbers decreases after multiple cycles, resulting in environmental pollution.

Method used

By using modified calcium-based solid waste carbide slag, coal gangue and fly ash, a CaO-SiO2-Al2O3-C-based absorbent was prepared. Citric acid was used to modify the carbide slag to increase the pore structure, and it was combined with coal gangue at high temperatures. It works synergistically with fly ash to achieve synergistic absorption and purification of CO2, SO2 and NOX.

Benefits of technology

It improves the removal efficiency of CO2, SO2 and NOX in the flue gas, avoids the sintering deactivation of carbide slag, achieves efficient flue gas purification, reduces environmental pollution, and rationally disposes of solid waste, with good economic and environmental benefits benefit.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of cement production admixtures, and in particular to a cement kiln high-temperature flue gas purification absorbent and a preparation method thereof. The invention uses calcium-based solid waste carbide slag produced in the production of polyvinyl chloride as a raw material, uses an appropriate amount of citric acid for modification, and then adds coal gangue and fly ash to prepare an efficient CaO-SiO2-Al2O3-C-based absorbent, which is directly used for removing CO2, SO2 and NO in high-temperature flue gas. X , which can solve the current problems of complex flue gas components, the need for separate treatment and low removal efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement production admixtures, in particular to a cement kiln high-temperature flue gas purification absorbent and a preparation method thereof. Background Art

[0002] CO2, SO2 and NO X It is an important factor causing the greenhouse effect, triggering a series of environmental problems such as glacier melting, acid rain, haze, and extreme climate. The cement industry is facing a severe task of reducing flue gas pollution.

[0003] At present, the cement industry generally removes the three separately. The CO2 capture technology mainly adopts the calcium cycle capture method in the carbon capture, utilization and storage technology (CCUS), but there is a problem of sintering and deactivation of the absorbent after multiple cycles, and the removal efficiency is greatly reduced; the desulfurization technology mainly includes self-emission reduction technology that uses limestone in the raw materials to absorb SO2 and additional SO2 emission reduction technologies including dry method, wet method, semi-dry method and composite desulfurization technology, but most of them have disadvantages such as large equipment investment and high operating costs.

[0004] Denitrification technologies include selective catalytic reduction technology (SCR) and selective non-catalytic reduction technology (SNCR), but both require ammonia or urea as reducing agents, and require additional ammonia (urea) storage and ammonia (urea) spraying equipment. The reducing agent is prone to escape, causing secondary air pollution, posing a major safety hazard to subsequent equipment and the environment.

[0005] Removing the three separately involves problems such as complex equipment, cumbersome operation, high cost, and secondary pollution. Therefore, it is very important to find a method for synergistic removal of the three.

[0006] For every ton of polyvinyl chloride produced, about 1.5-1.9 tons of carbide slag will be generated.

[0007] As a calcium-based industrial waste, most carbide slag is not reused and is generally landfilled, resulting in land occupation, resource waste and environmental pollution.

[0008] Coal gangue, which is also a kind of solid waste in mines, faces the same situation.

[0009] After calcination, carbide slag is rich in active CaO that can absorb CO2 and can be used as a desulfurizer in cement kilns.

[0010] The concentration of SO2 in cement kiln flue gas is very low, and the acidity of SO2 is stronger than that of CO2. Therefore, carbide slag will preferentially react with SO2 to generate sulfates with a decomposition temperature above 1000°C, and then react with CO2. At this time, part of the pore structure of the carbide slag will be blocked by sulfates that cannot be decomposed, and part of it will be blocked by sulfates that cannot be decomposed. Because the Tammann temperature of the carbide slag itself is extremely low, when the calcination temperature is raised to the Tammann temperature of the absorbent, the vacancy diffusion of the ions is activated, causing the adjacent CaO particles to agglomerate, causing part of the pore structure to collapse or disappear, resulting in a decrease in the efficiency of carbide slag in absorbing CO2. Therefore, optimizing the surface structure of carbide slag is also a key issue. Summary of the invention

[0011] The problems existing in the prior art have not been solved. The present invention provides a cement kiln high-temperature flue gas purification absorbent. The calcium-based solid waste carbide slag produced in the production of polyvinyl chloride is used as a raw material, modified with an appropriate amount of citric acid, and then coal gangue and fly ash are added to prepare an efficient CaO-SiO2-Al2O3-C-based absorbent, which is directly used to remove CO2, SO2 and NO in high-temperature flue gas. X , which can solve the current problems of complex flue gas components, the need for separate treatment and low removal efficiency.

[0012] Specifically, the preparation method of the cement kiln high-temperature flue gas purification absorbent of the present invention comprises the following steps:

[0013] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0014] 2) Dissolve citric acid in water to prepare citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0015] 3) The modified powder, coal gangue and fly ash are mixed and ground in a mass ratio of 1:(0.8-1.1):(0.2-0.3), and sieved to obtain a purification absorbent.

[0016] The invention uses citric acid to modify carbide slag, and then grinds it with coal gangue and fly ash to prepare a catalyst for CO2, SO2 and NO X The synergistic absorption purification absorbent, first, carbide slag reacts with citric acid to form calcium citrate, and during calcination, more small molecular substances will be pyrolyzed, making the carbide slag have a richer pore structure, so that the carbide slag after reacting with SO2 still maintains a high CO2 absorption capacity. In addition, coal gangue contains rich reducing carbon, which can absorb NO X Fully restore to achieve NO XPurification, and the gangue and fly ash play a synergistic role to produce Al2O3 and SiO2 at high temperature, which has an anti-sintering effect on the calcium oxide produced by carbide slag, ensuring a rich contact area for calcium oxide, avoiding the deactivation of carbide slag, and improving the absorption effect of CO2 and SO2.

[0017] Preferably, the carbide slag is solid waste generated in the production of polyvinyl chloride.

[0018] Preferably, in step 1), the particle size of the carbide slag powder is less than 75 μm.

[0019] Preferably, in step 2), the mass concentration of the citric acid solution is 10-15%, and the mass ratio of carbide slag powder to the citric acid solution is 1:(10-15).

[0020] Preferably, in step 2), the stirring speed is 450-550 r / min.

[0021] Preferably, in step 2), the drying temperature is 60-70° C. and the drying time is 40-50 h.

[0022] Preferably, in step 2), the particle size of the modified powder is less than 75 μm.

[0023] Preferably, in step 3), the particle size of the purified absorbent is less than 75 μm.

[0024] The present invention also relates to a cement kiln high-temperature flue gas purification absorbent, which is specifically prepared by the above-mentioned preparation method.

[0025] The present invention also relates to the application of the cement kiln high-temperature flue gas purification absorbent in the purification of cement kiln high-temperature flue gas.

[0026] Preferably, the high temperature is 650-950°C.

[0027] The invention uses modified carbide slag, coal gangue and fly ash as raw materials, optimizes the composition and modifies the microstructure to prepare a purification absorbent which can simultaneously remove CO2, SO2 and NO in cement kiln flue gas at a temperature of 650-950°C. X , directional conversion of CO2 into CaCO3, SO2 into sulfite and sulfate, NO X Catalytic reduction to N2, solving NO under sulfur-containing conditions X Reducing the technical problems of catalyst poisoning and deactivation, and low CO2 adsorption activity, achieving efficient CO2 adsorption / desorption, internal circulation of SO2 system without external discharge, and NO X Safe discharge without ammonia removal. The large-scale use of carbide slag can not only reasonably dispose of waste, but also avoid the environmental impact caused by landfilling these wastes, which has good economic and environmental benefits.

[0028] The purification absorbent of the present invention is easy to use and can be directly added to the decarbonization, desulfurization and denitrification device to remove CO2, SO2 and NO in the cement kiln flue gas in the whole system. X Efficient collaborative removal. DETAILED DESCRIPTION

[0029] In order to characterize the technical effect of the present invention, a purification absorbent was prepared and its purification performance was tested. During the preparation process, the raw materials were ground to a particle size of less than 75 μm, and the mass ratio of calcium carbide slag powder to acid solution was 1:10.

[0030] During the test, the purification absorbent was placed in a decarbonization, desulfurization and denitrification device and its decarbonization, desulfurization and denitrification effects were tested. During the process, the uniform dosage of the absorbent was 0.5g. The test was carried out in an atmosphere with a CO2 concentration of 30%, a SO2 concentration of 300ppm, a NO concentration of 450ppm, N2 as the balance gas, and a gas flow rate of 450mL / min.

[0031] Example 1

[0032] Purification absorbent, the preparation method comprises the following steps:

[0033] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0034] 2) Dissolve citric acid in water to prepare a 10% citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0035] 3) The modified powder, coal gangue and fly ash are mixed and ground in a mass ratio of 1:0.9:0.3, and sieved to obtain a purification absorbent.

[0036] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 89%, at 900℃, the average desulfurization rate in 10 minutes is 93%, and the average denitrification rate in 10 minutes is 89%.

[0037] Example 2

[0038] Purification absorbent, the preparation method comprises the following steps:

[0039] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0040] 2) Dissolve citric acid in water to prepare a citric acid solution with a mass concentration of 15%, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0041] 3) The modified powder, coal gangue and fly ash are mixed and ground in a mass ratio of 1:1:0.2, and sieved to obtain a purification absorbent.

[0042] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 88%, at 900℃, the average desulfurization rate in 10 minutes is 92%, and the average denitrification rate in 10 minutes is 87%.

[0043] Comparative Example 1

[0044] Purification absorbent, the preparation method comprises the following steps:

[0045] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0046] 2) Mix carbide slag powder, coal gangue and fly ash in a mass ratio of 1:0.9:0.3, grind them, sieve them, and prepare a purification absorbent.

[0047] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 66%, at 900℃, the average desulfurization rate in 10 minutes is 79%, and the average denitrification rate in 10 minutes is 70%.

[0048] Comparative Example 2

[0049] Purification absorbent, the preparation method comprises the following steps:

[0050] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0051] 2) Dissolve citric acid in water to prepare a 10% mass concentration citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain a purification absorbent.

[0052] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 76%, and at 900℃, the average desulfurization rate in 10 minutes is 81%, and there is no denitrification ability.

[0053] Comparative Example 3

[0054] Purification absorbent, the preparation method comprises the following steps:

[0055] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0056] 2) Dissolve citric acid in water to prepare a 10% citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0057] 3) The modified powder and coal gangue are mixed and ground in a mass ratio of 1:1, and sieved to obtain a purification absorbent.

[0058] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 82%, at 900℃, the average desulfurization rate in 10 minutes is 89%, and the average denitrification rate in 10 minutes is 88%.

[0059] Comparative Example 4

[0060] Purification absorbent, the preparation method comprises the following steps:

[0061] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0062] 2) Dissolve citric acid in water to prepare a 10% citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0063] 3) The modified powder and fly ash are mixed and ground in a mass ratio of 1:1, and sieved to obtain a purification absorbent.

[0064] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 77%, and at 900℃, the average desulfurization rate in 10 minutes is 85%, and there is no denitrification ability.

[0065] Comparative Example 5

[0066] Purification absorbent, the preparation method comprises the following steps:

[0067] 1) Grind and dry the carbide slag to obtain carbide slag powder.

[0068] 2) Dissolve tartaric acid in water to prepare a 10% tartaric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain modified powder.

[0069] 3) The modified powder, coal gangue and fly ash are mixed and ground in a mass ratio of 1:0.9:0.3, and sieved to obtain a purification absorbent.

[0070] According to the test, at 700℃, the average decarbonization rate in 10 minutes is 85%, at 900℃, the average desulfurization rate in 10 minutes is 83%, and the average denitrification rate in 10 minutes is 85%.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a cement kiln high-temperature flue gas purification absorbent, It is characterized in that The steps include: 1) Grind and dry the carbide slag to obtain carbide slag powder. 2) Dissolve citric acid in water to prepare a citric acid solution, add carbide slag powder, stir, dry, grind, and sieve to obtain a modified powder, wherein the mass concentration of the citric acid solution is 10-15%, and the mass ratio of carbide slag powder to citric acid solution is 1:(10-15). 3) The modified powder, coal gangue and fly ash are mixed and ground in a mass ratio of 1:(0.8-1.1):(0.2-0.3), and sieved to obtain a purification absorbent.

2. The preparation method of the cement kiln high temperature flue gas purification absorbent according to claim 1, It is characterized in that Step 1) The particle size of carbide slag powder is less than 75 μm.

3. The preparation method of the cement kiln high temperature flue gas purification absorbent according to claim 1, It is characterized in that Step 2) The stirring speed is 450-550r / min.

4. The method for preparing the cement kiln high temperature flue gas purification absorbent according to claim 1, It is characterized in that Step 2) The drying temperature is 60-70°C and the drying time is 40-50h.

5. The preparation method of the cement kiln high temperature flue gas purification absorbent according to claim 1, It is characterized in that Step 2) The particle size of the modified powder is less than 75 μm.

6. The method for preparing the cement kiln high temperature flue gas purification absorbent according to claim 1, It is characterized in that Step 3) Purify the absorbent to a particle size less than 75 μm.

7. Cement kiln high temperature flue gas purification absorbent, It is characterized in that The compound is prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the cement kiln high-temperature flue gas purification absorbent according to claim 7 in the purification of cement kiln high-temperature flue gas.

9. The use according to claim 8, It is characterized in that The high temperature is 650-950°C.

Citation Information

Patent Citations

  • Sludge-based desulfurizer and preparation method thereof

    CN101837231A

  • Industrial tail gas deep desulfurizer and preparation method thereof

    CN113663488A

  • Method for preparing cement kiln synergistic desulfurization and denitrification agent through resource utilization of hazardous waste and solid waste

    CN114682085A

  • Dry desulfurizer for ultralow emission of sulfonation tail gas and preparation method of dry desulfurizer

    CN115337896A

  • High-CO2-adsorption-capacity building material prepared by doping modified SiO2 aerogel into calcium-rich solid waste and method