A high-strength, high-transparency, degradable film and preparation method thereof

By adopting a bidirectional stretching process with ABA type or ABC type composite layer structure in the degradable film, the component proportion and process flow are optimized, and the shortcomings of existing films in terms of mechanical properties and transparency are solved, and high strength and high strength are achieved Transparency and good degradation properties.

CN118636554BActive Publication Date: 2024-11-22JIANGSU KANGHUI NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096913.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing degradable films have poor performance in terms of mechanical properties and transparency, especially in the fields of disposable transparent films, sealing tapes, transparent foods, pharmaceutical packaging, etc., and transparent during the preparation process caused by the film blowing process. Inadequate properties and tensile strength.

Method used

High-strength, highly transparent and degradable films using ABA, ABC or ABRBA composite layer structures, and through bidirectional tensile treatment, they form PLA, PBAT, styrene-glycidyl methacrylate copolymer and polyethylene glycol ethylene glycol Materials such as diesters optimize the component ratio and process flow of each layer, including raw material drying, melt extrusion, longitudinal and transverse stretching and heat setting treatment to form a high-performance film.

Benefits of technology

A film with high longitudinal and transverse tensile strength ≥160MPa, light transmittance ≥90%, haze ≤1.0% was achieved, with excellent anti-adhesion performance, thickness uniformity, ductility and heat resistance, and at the same time, under compost conditions High decomposition rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of degradable film, and relates to a kind of high-strength and highly transparent degradable film and preparation method thereof, high-strength and highly transparent degradable film has ABA type composite layer structure, ABC type composite layer structure or ABRBA type composite layer structure, through biaxial stretching treatment, A layer is made up of PLA, PBAT, styrene-methacrylate glycidyl copolymer, polyethylene glycol ethylene glycol and opening agent; other layers are made up of PLA, PBAT, styrene-methacrylate glycidyl copolymer and polyethylene glycol ethylene glycol; its preparation process includes: raw material delivery → weighing batching → raw material drying → melt extrusion → metering → filtering → casting sheet → longitudinal stretching → transverse stretching, wherein, heat setting treatment is carried out in transverse stretching process. The present invention has the advantages of high transparency and high tensile strength, and simultaneously has excellent anti-adhesion performance, thickness uniformity, ductility, heat resistance and degradation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of degradable films and relates to a high-strength and high-transparency degradable film and a preparation method thereof. Background Art

[0002] As a new type of material leading the trend of environmental protection, degradable film has been widely used in many fields compared with traditional plastic film due to its significant advantages such as degradability, high safety of degradation products, and low resource consumption. However, with the progress of society and the rapid development of science and technology, the performance requirements of degradable films in the application fields are also increasing, especially in terms of mechanical properties and transparency. Such as disposable transparent films, sealing tapes, transparent food, medical packaging, visible windows of cartons, transparent packaging of toys, disposable anti-fog masks and other fields. These application fields have certain requirements for the mechanical properties and transparency of the films, and the films currently on the market are mainly made of BOPET, BOPP, BOPI, BOPA and other materials, but in such disposable application scenarios, BOPET, BOPP, BOPI, BOPA are very difficult to degrade and easily cause white pollution.

[0003] Currently, most of the biodegradable films on the market are produced using the blown film process. This production method has limitations in controlling the thickness uniformity, flatness, heat resistance and mechanical properties of the film, resulting in poor overall performance of the final product, especially transparency and tensile strength (less than 100MPa).

[0004] For example, patent application CN110283438B discloses a base resin for a blow-molded degradable film and a blow-molded degradable film. The base resin of the degradable film is prepared from raw materials including the following components in parts by mass: 5 to 60 parts of poly (L-lactic acid); 30 to 95 parts of adipic acid-terephthalic acid-butylene glycol copolymer; 0.2 to 5 parts of a foaming regulator; 0.1 to 2 parts of a reactive compatibilizer; and 1 to 5 parts of a diol oligomer. The preparation method is to use poly (L-lactic acid) and adipic acid-terephthalic acid-butylene glycol copolymer (i.e., PBTA) as a matrix, introduce a diol oligomer and a reactive compatibilizer into the system, and form a modified product with a partially cross-linked structure in situ through reaction blending. The modified product can be blended with foamed particles in a film blowing machine to form a film, thereby realizing the blown film molding of degradable polymer materials. However, the maximum longitudinal tensile strength of the degradable film prepared is 55 MPa, and the transverse tensile strength is 42 MPa. In addition, a foaming agent is added during the preparation process, which will affect the haze and transparency of the prepared degradable film, resulting in high haze and opacity.

[0005] Due to the problems existing in the film blowing process, the prior art also considers the use of a biaxial stretching process for production to improve the performance of the degradable film. For example, patent application CN201911138446.X discloses a degradable biaxially stretched polylactic acid cigarette film and a preparation method thereof. The degradable biaxially stretched polylactic acid cigarette film is composed of three layers of co-extruded and stretched A, B and C. In terms of mass percentage, the A layer includes 80-90% heat-sealed type I PLA, 8-15% lubricant and 2-5% anti-blocking agent. The heat-sealed type I PLA is composed of 70-80% crystalline PLA and 20-30% non-crystalline PLA; the B layer includes 9 0~95% crystalline PLA, 1~5% antistatic agent, 1~2% stiffening agent, 1~5% toughening agent; C layer includes 94~97% heat-seal type II PLA, 2~3% slip agent and 1~3% anti-blocking agent, and the heat-seal type II PLA is composed of 75~85% crystalline PLA and 15~25% non-crystalline PLA; the preparation method is to dry each component according to the amount, stretch it biaxially after melt extrusion, then corona treatment, winding, and finally aging and slitting. However, although the obtained degradable biaxially stretched polylactic acid cigarette film has a tensile strength of >100MPa, the haze is 1.27%, which is not suitable for use in fields requiring high transparency of the film.

[0006] Therefore, it is necessary to develop a degradable film with high tensile strength, high transparency and better overall performance. Summary of the invention

[0007] The purpose of the present invention is to solve the problems existing in the prior art and to provide a high-strength and highly transparent degradable film and a preparation method thereof.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A high-strength and highly transparent biodegradable film, having an ABA type composite layer structure (the structure consists of three layers of A, B, and A), an ABC type composite layer structure (the structure consists of three layers of A, B, and C), or an ABRBA type composite layer structure (the structure consists of five layers of A, B, R, B, and A), and after biaxial stretching treatment, the A layer consists of 19.2-80wt% of PLA, 19.2-80wt% of PBAT, 0.1-2wt% of styrene-methacrylate glycidyl ester copolymer, 0.6-5wt% of polyethylene glycol ethylene glycol, and 0.1-5wt% of an anti-blocking agent;

[0010] The other layers consist of 19.3-80wt% of PLA, 19.3-80wt% of PBAT, 0.1-2wt% of styrene-glycidyl methacrylate copolymer and 0.6-5wt% of polyethylene glycol ethylene glycol.

[0011] As the preferred technical solution:

[0012] The high-strength and high-transparency degradable film as described above has a longitudinal tensile strength of ≥160MPa, a transverse tensile strength of ≥160MPa, a light transmittance of ≥90%, and a haze of ≤1.0%. The tensile strength of the degradable film in the prior art is generally less than 100MPa, the transparency is poor, and the haze is >1.0%. The present invention is significantly superior to the prior art for the following reasons:

[0013] (1) The components of each layer are properly selected, and each component can play a positive role in improving the tensile strength or transparency of the film. Among them, PLA has relatively strong rigidity and is dominant in excellent tensile strength; PBAT is relatively flexible, which is conducive to stretching film formation, and is dominant in excellent elongation at break; styrene-methacrylate copolymer is a chain extender, which can extend the chain of both PLA and PBAT. After chain extension, PLA and PBAT have better mechanical properties and are more compatible; polyethylene glycol ester is a plasticizer and compatibilizer, which improves the optical properties of the film and makes the materials compatible into a homogeneous state; the anti-blocking agent can improve the anti-adhesion performance of the film and improve the transparency of the film;

[0014] (2) The compounding ratio of each component in each layer is designed reasonably. PLA is conducive to improving tensile strength, PBAT is conducive to film forming and processability, styrene-methacrylate glycidyl copolymer is conducive to further improving tensile strength, and polyethylene glycol ethylene glycol is conducive to the formation of a homogeneous state of each component to improve transparency. If the compounding ratio is not appropriate, the film will have low tensile strength, poor transparency and be foggy;

[0015] (3) Adding an anti-blocking agent only to layer A can improve the anti-adhesion performance of the film while maintaining the excellent optical properties of the film;

[0016] (4) After biaxial stretching, the molecular chains of the film are arranged regularly and fused with each other, making the components in the film homogeneous.

[0017] The high-strength and high-transparency degradable film as described above has a dynamic friction coefficient of ≤0.7, a warp of ≤2mm, a longitudinal elongation at break ≥100%, a transverse elongation at break ≥100%, a longitudinal elastic modulus of 1615-2016MPa, a transverse elastic modulus of 1752-1996MPa, a glossiness of 45° of 60.5-86.5, and after baking at 90°C for 10min, the longitudinal shrinkage is ≤10%, the transverse shrinkage is ≤10%, and the decomposition rate under composting conditions is ≥85%. It can be seen that the high-strength and high-transparency degradable film of the present invention has excellent anti-adhesion performance, thickness uniformity, ductility, heat resistance and degradation performance.

[0018] The high-strength and highly transparent biodegradable film as described above, wherein layer A is composed of 76wt% PLA, 21.7wt% PBAT, 0.2wt% styrene-glycidyl methacrylate copolymer, 2wt% polyethylene glycol ethylene glycol and 0.1wt% opening agent.

[0019] The high-strength and highly transparent biodegradable film as described above, the other layers are composed of 76wt% of PLA, 21.8wt% of PBAT, 0.2wt% of styrene-glycidyl methacrylate copolymer and 2wt% of polyethylene glycol ethylene glycol.

[0020] As described above, the high-strength, high-transparency and degradable film has a density of 1.20-1.30 g / cm 3 , the melt index at 190℃ and 2.16kg is 2-12g / 10min, the melting point is 155-170℃, and the glass transition temperature is 60℃;

[0021] The density of PBAT is 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 3.6-10g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0022] The weight average molecular weight of styrene-glycidyl methacrylate copolymer is 4500-5500 g / mol, and the purity is ≥99.5%;

[0023] The acid value of polyethylene glycol ester is ≤1.0mg(KOH) / g, the water content is ≤0.1wt%, the hydroxyl value is ≤2.5mg(KOH) / g, the carboxyl value is ≤3.0mg(KOH) / g, the density is 1.02±0.02g / cm³, the refractive index is 1.45±0.05, the melting point is -25±1℃, and the viscosity at 20℃ is 50±3mPa·s;

[0024] The opening agent is calcium carbonate, silicon dioxide, montmorillonite or talc, and the average particle size is 0.5-4.5 μm.

[0025] As described above, the high-strength, high-transparency and biodegradable film has a melting index of 3.6 g / 10 min at 190° C. and 2.16 kg for PBAT; the opening agent is calcium carbonate, and the average particle size is 1.0 μm.

[0026] As described above, the high-strength and high-transparency biodegradable film has a thickness of 2-350 μm, the thickness of a single A layer accounts for 3%-10%, the thickness of a single B layer accounts for 35%-94%, the thickness of a single C layer accounts for 3%-10%, and the thickness of a single R layer accounts for 0%-10%.

[0027] The present invention also provides a method for preparing a high-strength, high-transparency, degradable film as described in any of the preceding items, the process flow comprising: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → casting → longitudinal stretching → transverse stretching, wherein heat setting treatment is performed during the transverse stretching process.

[0028] As the preferred technical solution:

[0029] In the method described above, the stretching ratio of the longitudinal stretching or the transverse stretching is 3-8; and the temperature of the heat setting treatment is 60-130°C.

[0030] Beneficial effects:

[0031] (1) The components of each layer of the present invention can play a positive role in improving the tensile strength or transparency of the film. For example, PLA has a relatively strong rigidity and has an excellent tensile strength; PBAT is relatively flexible and is conducive to stretching and film formation, and has an excellent elongation at break; styrene-methacrylate copolymer is a chain extender, which can extend the chain of both PLA and PBAT. After chain extension, PLA and PBAT have better mechanical properties and are more compatible; polyethylene glycol ester plays the role of a plasticizer and a compatibilizer, improving the optical properties of the film and compatibilizing the materials into a homogeneous state; and an anti-blocking agent can improve the anti-adhesion property of the film and improve the transparency of the film.

[0032] (2) The present invention controls the compounding ratio of each component in each layer, so that the prepared degradable film has the advantages of high transparency, high tensile strength and excellent degradation performance.

[0033] (3) The present invention only adds an anti-blocking agent to the A layer, which can improve the anti-adhesion performance of the film while maintaining the excellent optical properties of the film. At the same time, the film is treated with a biaxial stretching process and a special heat setting treatment method during the production process, so that the thickness uniformity, flatness, heat resistance, mechanical properties, ductility, and thermal stability can be controlled within a certain range, so that each component in the film is in a homogeneous state. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0035] The testing methods of the relevant performance indicators in the following embodiments and comparative examples are as follows:

[0036] Longitudinal and transverse tensile strength: The high-strength and high-transparency biodegradable film is tested in accordance with GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets".

[0037] Longitudinal and transverse elongation at break: The high-strength and high-transparency biodegradable film is tested in accordance with GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets".

[0038] Transverse and longitudinal elastic modulus: The high-strength and high-transparency biodegradable film is tested in accordance with GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets".

[0039] Light transmittance, haze: The high-strength and high-transparency biodegradable film was tested according to the haze meter method A in the standard GB / T2410-2008 "Determination of light transmittance and haze of transparent plastics".

[0040] Gloss 45°: Test the high-strength and high-transparency biodegradable film in accordance with GB / T8807-1988 "Test method for mirror gloss of plastics".

[0041] Dynamic friction coefficient: The high-strength and high-transparency biodegradable film is tested in accordance with the standard GB / T10006-2021 "Determination of friction coefficient of plastic films and sheets".

[0042] Longitudinal and transverse shrinkage: The high-strength and high-transparency biodegradable film is tested in accordance with GB / T12027-2004 "Test method for dimensional change rate of plastic film and sheeting upon heating".

[0043] Thickness: Test high-strength, high-transparency and biodegradable films in accordance with GB / T 6672-2001 "Mechanical measurement method for thickness of plastic films and sheets";

[0044] Warping: The high-strength and high-transparency biodegradable film is tested in accordance with GB / T25257-201 "Determination of Warpage of Optical Functional Films" standard.

[0045] Decomposition rate: The high-strength and high-transparency biodegradable film was tested in accordance with GB / T 19277.1-2011 "Determination of the ultimate aerobic biodegradability of materials under controlled composting conditions - Determination of released carbon dioxide - Part 1: General method".

[0046] Example 1

[0047] A high-strength and highly transparent degradable film having an ABA-type composite layer structure, wherein the thickness of the high-strength and highly transparent degradable film is 19 μm, the thickness of a single A layer accounts for 3%, and the thickness of a single B layer accounts for 94%;

[0048] The A layer is composed of 76wt% PLA, 21.7wt% PBAT, 0.2wt% styrene-glycidyl methacrylate copolymer, 2wt% polyethylene glycol ethylene glycol and 0.1wt% antiblocking agent;

[0049] The B layer is composed of 76 wt % PLA, 21.8 wt % PBAT, 0.2 wt % styrene-co-glycidyl methacrylate and 2 wt % polyethylene glycol.

[0050] The method for preparing the high-strength and high-transparency biodegradable film as described above comprises the following steps:

[0051] (1) Preparation of raw materials;

[0052] PLA: density 1.3g / cm 3 , the melt index at 190℃ and 2.16kg is 2g / 10min, the melting point is 170℃, and the glass transition temperature is 60℃;

[0053] PBAT: density 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 3.6g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0054] Styrene-glycidyl methacrylate copolymer: weight average molecular weight 5000g / mol, purity ≥99.5%;

[0055] Polyethylene glycol ester: acid value 0.6mg(KOH) / g, water content 0.03wt%, hydroxyl value 1.2mg(KOH) / g, carboxyl value 2.3mg(KOH) / g, density 1.02g / cm³, refractive index 1.45, melting point -25℃, viscosity at 20℃ 50mPa·s;

[0056] Opening agent: calcium carbonate, average particle size is 1 μm;

[0057] (2) Preparing a high-strength, high-transparency, biodegradable film according to the compounding ratio of each component in the above-mentioned layers;

[0058] The process flow includes: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → sheet casting → longitudinal stretching → transverse stretching; wherein, heat setting treatment is carried out during the transverse stretching process, the stretching ratio of the longitudinal stretching is 6, the stretching ratio of the transverse stretching is 6, and the temperature of the heat setting treatment is 105°C.

[0059] The final high-strength and high-transparency biodegradable film has a longitudinal tensile strength of 174MPa, a transverse tensile strength of 175MPa, a transmittance of 91%, and a haze of 0.7%; the high-strength and high-transparent biodegradable film has a dynamic friction coefficient of 0.6, a warp of 1mm, a longitudinal elongation at break of 112%, a transverse elongation at break of 109%, a longitudinal elastic modulus of 2016MPa, a transverse elastic modulus of 1907MPa, a glossiness of 45° of 86.5, and after baking at 90°C for 10min, the longitudinal shrinkage was 9.8%, the transverse shrinkage was 8.6%, and the decomposition rate under composting conditions was 86.9%.

[0060] Example 2

[0061] A high-strength and high-transparency biodegradable film having an ABC type composite layer structure, wherein the thickness of the high-strength and high-transparency biodegradable film is 2 μm, the thickness of a single A layer accounts for 5%, the thickness of a single B layer accounts for 92%, and the thickness of a single C layer accounts for 3%;

[0062] The A layer is composed of 19.2wt% PLA, 68.8wt% PBAT, 2wt% styrene-glycidyl methacrylate copolymer, 5wt% polyethylene glycol ethylene glycol and 5wt% antiblocking agent;

[0063] Layer B is composed of 19.3wt% PLA, 80wt% PBAT, 0.1wt% styrene-co-glycidyl methacrylate, and 0.6wt% polyethylene glycol;

[0064] The C layer is composed of 73.7wt% PLA, 19.3wt% PBAT, 2wt% styrene-co-glycidyl methacrylate and 5wt% polyethylene glycol.

[0065] The method for preparing the high-strength and high-transparency biodegradable film as described above comprises the following steps:

[0066] (1) Preparation of raw materials;

[0067] PLA: Density 1.2g / cm 3 , the melt index at 190℃ and 2.16kg is 12g / 10min, the melting point is 170℃, and the glass transition temperature is 60℃;

[0068] PBAT: density 1.22g / cm3 , the melt index at 190℃ and 2.16kg is 3.6g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0069] Styrene-glycidyl methacrylate copolymer: weight average molecular weight 4500g / mol, purity ≥99.5%;

[0070] Polyethylene glycol ester: acid value 1mg(KOH) / g, water content 0.1wt%, hydroxyl value 2.5mg(KOH) / g, carboxyl value 3mg(KOH) / g, density 1g / cm³, refractive index 1.4, melting point -24℃, viscosity at 20℃ 53mPa·s;

[0071] Opening agent: silicon dioxide, average particle size 0.5 μm;

[0072] (2) Preparing a high-strength, high-transparency, biodegradable film according to the compounding ratio of each component in the above-mentioned layers;

[0073] The process flow includes: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → sheet casting → longitudinal stretching → transverse stretching; wherein, heat setting treatment is performed during the transverse stretching process, the stretching ratio of the longitudinal stretching is 8, the stretching ratio of the transverse stretching is 3, and the temperature of the heat setting treatment is 60°C.

[0074] The final high-strength and high-transparency biodegradable film has a longitudinal tensile strength of 168MPa, a transverse tensile strength of 161MPa, a transmittance of 90%, and a haze of 1%; the high-strength and high-transparent biodegradable film has a dynamic friction coefficient of 0.62, a warp of 1mm, a longitudinal elongation at break of 110%, a transverse elongation at break of 112%, a longitudinal elastic modulus of 1988MPa, a transverse elastic modulus of 1753MPa, and a glossiness of 45° of 60.5. After baking at 90°C for 10min, the longitudinal shrinkage was 9.7%, the transverse shrinkage was 9.2%, and the decomposition rate under composting conditions was 85.2%.

[0075] Example 3

[0076] A high-strength and high-transparency biodegradable film having an ABRBA type composite layer structure, wherein the thickness of the high-strength and high-transparency biodegradable film is 350 μm, the thickness of a single A layer accounts for 10%, the thickness of a single B layer accounts for 35%, and the thickness of a single R layer accounts for 10%;

[0077] The A layer is composed of 80wt% PLA, 19.2wt% PBAT, 0.1wt% styrene-glycidyl methacrylate copolymer, 0.6wt% polyethylene glycol ethylene glycol and 0.1wt% antiblocking agent;

[0078] Layer B is composed of 80wt% PLA, 19.3wt% PBAT, 0.1wt% styrene-glycidyl methacrylate copolymer, and 0.6wt% polyethylene glycol ethylene glycol;

[0079] The R layer is composed of 73.7wt% PLA, 19.3wt% PBAT, 2wt% styrene-co-glycidyl methacrylate and 5wt% polyethylene glycol.

[0080] The method for preparing the high-strength and high-transparency biodegradable film as described above comprises the following steps:

[0081] (1) Preparation of raw materials;

[0082] PLA: Density 1.3 g / cm 3 , the melt index at 190℃ and 2.16kg is 2g / 10min, the melting point is 155℃, and the glass transition temperature is 60℃;

[0083] PBAT: density 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 10g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0084] Styrene-glycidyl methacrylate copolymer: weight average molecular weight 5500g / mol, purity ≥99.5%;

[0085] Polyethylene glycol ester: acid value 0.3mg(KOH) / g, water content 0.03wt%, hydroxyl value 1.2mg(KOH) / g, carboxyl value 2.3mg(KOH) / g, density 1.04g / cm³, refractive index 1.5, melting point -26℃, viscosity at 20℃ 47mPa·s;

[0086] Opening agent: montmorillonite (manufacturer: Shanghai Aladdin Biochemical Technology Co., Ltd., product number: M141491), average particle size: 0.6 μm;

[0087] (2) Preparing a high-strength, high-transparency, biodegradable film according to the compounding ratio of each component in the above-mentioned layers;

[0088] The process flow includes: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → sheet casting → longitudinal stretching → transverse stretching; wherein, heat setting treatment is performed during the transverse stretching process, the stretching ratio of the longitudinal stretching is 3, the stretching ratio of the transverse stretching is 8, and the temperature of the heat setting treatment is 130°C.

[0089] The final high-strength and high-transparency degradable film has a longitudinal tensile strength of 163MPa, a transverse tensile strength of 173MPa, a transmittance of 90%, and a haze of 1%; the high-strength and high-transparent degradable film has a dynamic friction coefficient of 0.66, a warp of 1mm, a longitudinal elongation at break of 106%, a transverse elongation at break of 108%, a longitudinal elastic modulus of 1615MPa, a transverse elastic modulus of 1996MPa, a glossiness of 45° of 82.3, and after baking at 90°C for 10min, the longitudinal shrinkage is 8.1%, the transverse shrinkage is 8.3%, and the decomposition rate under composting conditions is 86.1%.

[0090] Example 4

[0091] A high-strength and high-transparency biodegradable film having an ABA-type composite layer structure, wherein the thickness of the high-strength and high-transparency biodegradable film is 30 μm, the thickness of a single A layer accounts for 5%, and the thickness of a single B layer accounts for 90%;

[0092] The A layer is composed of 19.2wt% PLA, 80wt% PBAT, 0.1wt% styrene-glycidyl methacrylate copolymer, 0.6wt% polyethylene glycol ethylene glycol and 0.1wt% antiblocking agent;

[0093] The B layer is composed of 19.3 wt % PLA, 73.7 wt % PBAT, 2 wt % styrene-co-glycidyl methacrylate and 5 wt % polyethylene glycol.

[0094] The method for preparing the high-strength and high-transparency biodegradable film as described above comprises the following steps:

[0095] (1) Preparation of raw materials;

[0096] PLA: Density 1.25g / cm 3 , the melt index at 190℃ and 2.16kg is 3g / 10min, the melting point is 160℃, and the glass transition temperature is 60℃;

[0097] PBAT: density 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 5g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0098] Styrene-glycidyl methacrylate copolymer: weight average molecular weight 5000g / mol, purity ≥99.5%;

[0099] Polyethylene glycol ester: acid value 0.6mg(KOH) / g, water content 0.03wt%, hydroxyl value 1.2mg(KOH) / g, carboxyl value 2.3mg(KOH) / g, density 1.02g / cm³, refractive index 1.45, melting point -25℃, viscosity at 20℃ 50mPa·s;

[0100] Opening agent: talcum powder, average particle size is 2.5μm;

[0101] (2) Preparing a high-strength, high-transparency, biodegradable film according to the compounding ratio of each component in the above-mentioned layers;

[0102] The process flow includes: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → sheet casting → longitudinal stretching → transverse stretching; wherein, heat setting treatment is carried out during the transverse stretching process, the stretching ratio of the longitudinal stretching is 6, the stretching ratio of the transverse stretching is 6, and the temperature of the heat setting treatment is 105°C.

[0103] The final high-strength and high-transparency biodegradable film has a longitudinal tensile strength of 161MPa, a transverse tensile strength of 162MPa, a transmittance of 91%, and a haze of 0.8%; the high-strength and high-transparent biodegradable film has a dynamic friction coefficient of 0.66, a warp of 1mm, a longitudinal elongation at break of 111%, a transverse elongation at break of 109%, a longitudinal elastic modulus of 1770MPa, a transverse elastic modulus of 1752MPa, and a glossiness of 45° of 85.1. After baking at 90°C for 10min, the longitudinal shrinkage was 9.6%, the transverse shrinkage was 9.7%, and the decomposition rate under composting conditions was 86.7%.

[0104] Example 5

[0105] A high-strength and high-transparency biodegradable film having an ABA-type composite layer structure, wherein the thickness of the high-strength and high-transparency biodegradable film is 30 μm, the thickness of a single A layer accounts for 7%, and the thickness of a single B layer accounts for 86%;

[0106] The A layer is composed of 19.2wt% PLA, 79.6wt% PBAT, 0.1wt% styrene-glycidyl methacrylate copolymer, 0.6wt% polyethylene glycol ethylene glycol and 0.5wt% antiblocking agent;

[0107] The B layer is composed of 73.7wt% PLA, 19.3wt% PBAT, 2wt% styrene-co-glycidyl methacrylate and 5wt% polyethylene glycol ether.

[0108] The method for preparing the high-strength and high-transparency biodegradable film as described above comprises the following steps:

[0109] (1) Preparation of raw materials;

[0110] PLA: Density 1.25g / cm 3 , the melt index at 190℃ and 2.16kg is 3g / 10min, the melting point is 160℃, and the glass transition temperature is 60℃;

[0111] PBAT: density 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 5g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t;

[0112] Styrene-glycidyl methacrylate copolymer: weight average molecular weight 5000g / mol, purity ≥99.5%;

[0113] Polyethylene glycol ester: acid value 0.6mg(KOH) / g, water content 0.03wt%, hydroxyl value 1.2mg(KOH) / g, carboxyl value 2.3mg(KOH) / g, density 1.02g / cm³, refractive index 1.45, melting point -25℃, viscosity at 20℃ 50mPa·s;

[0114] Opening agent: calcium carbonate, average particle size 4.5μm;

[0115] (2) Preparing a high-strength, high-transparency, biodegradable film according to the compounding ratio of each component in the above-mentioned layers;

[0116] The process flow includes: raw material transportation → weighing and mixing → raw material drying → melt extrusion → metering → filtration → sheet casting → longitudinal stretching → transverse stretching; wherein, heat setting treatment is carried out during the transverse stretching process, the stretching ratio of the longitudinal stretching is 6, the stretching ratio of the transverse stretching is 6, and the temperature of the heat setting treatment is 105°C.

[0117] The final high-strength and high-transparency biodegradable film has a longitudinal tensile strength of 172MPa, a transverse tensile strength of 169MPa, a transmittance of 91%, and a haze of 0.9%; the high-strength and high-transparent biodegradable film has a dynamic friction coefficient of 0.66, a warp of 1mm, a longitudinal elongation at break of 107%, a transverse elongation at break of 102%, a longitudinal elastic modulus of 1767MPa, a transverse elastic modulus of 1831MPa, a glossiness of 45° of 84.9, and after baking at 90°C for 10min, the longitudinal shrinkage was 9.4%, the transverse shrinkage was 9.3%, and the decomposition rate under composting conditions was 86.4%.

Claims

1. A high-strength and highly transparent biodegradable film having an ABA type composite layer structure, an ABC type composite layer structure or an ABRBA type composite layer structure, and having been subjected to a biaxial stretching treatment, characterized in that: The A layer is composed of 19.2-80wt% of PLA, 19.2-80wt% of PBAT, 0.1-2wt% of styrene-glycidyl methacrylate copolymer, 0.6-5wt% of polyethylene glycol ethylene glycol and 0.1-5wt% of an antiblocking agent; The other layers consist of 19.3-80wt% PLA, 19.3-80wt% PBAT, 0.1-2wt% styrene-glycidyl methacrylate copolymer, and 0.6-5wt% polyethylene glycol ethylene glycol; According to GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets", the longitudinal tensile strength of the high-strength and high-transparency biodegradable film is ≥160MPa, the transverse tensile strength is ≥160MPa, the longitudinal elastic modulus is 1615-2016MPa, the transverse elastic modulus is 1752-1996MPa, the longitudinal elongation at break is ≥100%, and the transverse elongation at break is ≥100%; According to the haze meter method A in GB / T2410-2008 "Determination of light transmittance and haze of transparent plastics", the light transmittance of high-strength, high-transparent and degradable film is ≥90% and the haze is ≤1.0%; According to the GB / T10006-2021 "Determination of friction coefficient of plastic films and sheets" standard, the dynamic friction coefficient of high-strength and high-transparency biodegradable film is ≤0.7; According to the GB / T8807-1988 "Test Method for Mirror Gloss of Plastics" standard, the gloss of the high-strength, high-transparency and degradable film at 45° is 60.5-86.5; According to GB / T12027-2004 "Test Method for Heating Dimensional Change of Plastic Film and Sheet", after baking at 90°C for 10 minutes, the longitudinal shrinkage of the high-strength and high-transparency biodegradable film is ≤10%, and the transverse shrinkage is ≤10%; Tested according to GB / T25257-201 "Measurement Method for Warpage of Optical Functional Films", the warpage of high-strength and high-transparency biodegradable films is ≤2mm; According to the standard GB / T 19277.1-2011 "Determination of the ultimate aerobic biodegradability of materials under controlled composting conditions - Determination of released carbon dioxide - Part 1: General method", the decomposition rate of high-strength and high-transparency biodegradable film under composting conditions is ≥85%.

2. A high-strength and highly transparent degradable film according to claim 1, characterized in that: The A layer is composed of 76wt% PLA, 21.7wt% PBAT, 0.2wt% styrene-glycidyl methacrylate copolymer, 2wt% polyethylene glycol ethylene glycol and 0.1wt% antiblocking agent.

3. The high-strength and highly transparent degradable film according to claim 1, characterized in that: The other layers consisted of 76 wt % PLA, 21.8 wt % PBAT, 0.2 wt % styrene-co-glycidyl methacrylate and 2 wt % polyethylene glycol.

4. The high-strength and highly transparent degradable film according to claim 1, characterized in that: The density of PLA is 1.20-1.30g / cm 3 , the melt index at 190℃ and 2.16kg is 2-12g / 10min, the melting point is 155-170℃, and the glass transition temperature is 60℃; The density of PBAT is 1.22g / cm 3 , the melt index at 190℃ and 2.16kg is 3.6-10g / 10min, the melting point is 116℃, and the terminal carboxyl content is 12mol / t; The weight average molecular weight of styrene-glycidyl methacrylate copolymer is 4500-5500 g / mol, and the purity is ≥99.5%; The acid value of polyethylene glycol ester is ≤1.0mg(KOH) / g, the water content is ≤0.1wt%, the hydroxyl value is ≤2.5mg(KOH) / g, the carboxyl value is ≤3.0mg(KOH) / g, the density is 1.02±0.02g / cm³, the refractive index is 1.45±0.05, the melting point is -25±1℃, and the viscosity at 20℃ is 50±3mPa·s; The opening agent is calcium carbonate, silicon dioxide, montmorillonite or talc, and the average particle size is 0.5-4.5 μm.

5. The high-strength and highly transparent degradable film according to claim 4, characterized in that: The melt index of PBAT at 190°C and 2.16kg is 3.6g / 10min; the opening agent is calcium carbonate, and the average particle size is 1.0μm.

6. The high-strength and highly transparent degradable film according to claim 1, characterized in that: The thickness of the high-strength and high-transparency biodegradable film is 2-350μm, the thickness of a single A layer accounts for 3%-10%, the thickness of a single B layer accounts for 35%-94%, the thickness of a single C layer accounts for 3%-10%, and the thickness of a single R layer accounts for 0%-10%.

7. A method for preparing a high-strength and highly transparent degradable film as claimed in any one of claims 1 to 6, characterized in that: The process flow includes: raw material transportation → weighing and batching → raw material drying → melt extrusion → metering → filtering → sheet casting → longitudinal stretching → transverse stretching, wherein heat setting treatment is performed during the transverse stretching process.

8. The method according to claim 7, characterized in that The stretching ratio of the longitudinal stretching or transverse stretching is 3-8; the temperature of the heat setting treatment is 60-130°C.