A preparation method of light-burned magnesium oxide composite refractory material
By carrying out hydrophilic modification and nanomaterial coating modification of magnesite materials, the density and hardness of light-burned magnesium oxide material are improved, which solves the problem that the amorphous refractory material lining is easily affected by operation, and significantly improves the resistance to Compressive strength and thermal shock resistance extend service life.
Patent Information
- Application Number
- CN202411117885.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing dead-burned magnesium powder or dead-burned magnesium powder composite materials in amorphous refractory linings are easily affected by the pouring or ramming process, resulting in reduced performance and short service life, and the homogeneity and density of multiple raw material composite materials The requirements are high and the operation error is large, which affects the performance.
Magnesite is crushed into different particle size grades, polyvinylpyrrolidone PVP-K30 and water-soluble high-carbon alcohol defoaming agent are hydrophilically modified, and nano-titanium carbide and boron carbide are used for surface coating and defect pore embedding ball milling modification. properties, combined with sodium methylene bisnaphthalene sulfonate and ball milling additives, to increase the density and hardness of the material and reduce creep.
It significantly improves the compressive strength, thermal shock resistance and creep resistance of light-burned magnesium oxide materials, prolongs the service life, and allows larger lining construction operation errors to ensure long-term use of the lining.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a method for preparing a light-burned magnesium oxide composite refractory material. Background Art
[0002] Light-burned magnesium oxide is abbreviated as light-burned magnesium. It is usually obtained by calcining magnesite at 800℃~1000℃. The light-burning temperature and time of magnesite have an effect on the activity of light-burned magnesium. Magnesite forms equiaxed periclase at about 600℃, and gradually transforms into non-equiaxed periclase at 650℃~850℃. The periclase formed by calcination at 800℃~1000℃ has large lattice gaps, point defects and dislocations, high porosity, large specific surface area, high surface energy, easy to absorb water, and reacts with water to form Mg(HO) 2 It hardens and has bonding ability, and is generally used to prepare cement, magnesia building materials, thermal insulation materials, etc. Light-burned magnesia can be calcined at high temperature to obtain dead-burned magnesia powder, which is a high-quality refractory material and can be used as lining of refractory bricks or amorphous refractory materials for metallurgy.
[0003] At present, when heavy burned magnesium powder or a composite material of heavy burned magnesium powder is used as the lining of amorphous refractory materials for kilns, it will be greatly affected by the casting or ramming process. The existing casting or ramming technologies are uneven, and it is easy to cause improper casting or ramming, such as too thick, too thin, uneven materials, uneven thickness, loose fillers, bubbles, etc., which will cause the lining to easily fall off, crack or penetrate the furnace. In addition, if the casting or ramming is uneven, the thermal shock resistance of the furnace lining will be reduced and the service life will be short. In particular, composite materials of multiple raw materials have higher requirements for material homogeneity, thickness homogeneity, and density homogeneity during the lining operation. Slight differences will seriously affect the performance of the lining. Therefore, in view of the fact that amorphous refractory materials are easily affected by the lining operation, which reduces performance and service life, the development and improvement of materials need to be continuously improved. Summary of the invention
[0004] Amorphous refractory materials such as existing castables or ramming materials are easily affected by lining operations, which will reduce the performance and service life of the lining and may even cause safety accidents such as furnace penetration. The invention provides a preparation method of a light-burned magnesium oxide composite refractory material. Magnesite is used as a raw material and crushed into magnesite materials of different particle sizes. Polyvinyl pyrrolidone PVP-K30 and a water-soluble high-carbon alcohol defoamer are used to perform hydrophilic modification on the surface of the magnesite material particles. Then, nano-titanium carbide and boron carbide are used to perform surface coating and defect pore embedding ball milling modification on the magnesite material. Sodium methylene bis-naphthalene sulfonate, a ball milling aid and a hydrophilic film are used in combination to improve the workability and homogeneity of the solid modification. After heat treatment, light-burned magnesium oxide is obtained, which can improve the density and hardness of light-burned magnesium oxide material particles, reduce creep resistance, and substantially improve the characteristics of light-burned magnesium oxide. The compressive strength, thermal shock resistance, creep resistance and the like of magnesium ramming materials after use are greatly improved, and the service life is extended. The material composite homogeneity between the magnesite material particles, nano-titanium carbide and nano-boron carbide is better, a larger lining construction operation error can be allowed, the influence of construction operation is small, and the long-term use of the lining can be guaranteed. The specific technical solution is as follows:
[0005] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0006] S1: taking magnesite, crushing, grading or screening, and obtaining magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively;
[0007] S2: Mix the mixture according to the mass ratio of water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer = 100: (0-20): (1.5-3.5): (2-5) to obtain a liquid modifier;
[0008] Taking magnesite powder, magnesite fine aggregate and magnesite coarse aggregate, respectively placing them in a liquid modifier, stirring, mixing and soaking, filtering, drying, crushing, grading or screening, and respectively obtaining modified magnesite powder, modified magnesite fine aggregate and modified magnesite coarse aggregate;
[0009] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air flow in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = (1-2.5): (1-2.5): (0.3-1) to obtain a solid modifier;
[0010] According to the mass ratio, water: soybean oil: Tween 80 = 100: (10-15): (2-3), mix and prepare the ball milling aid;
[0011] S3.1: According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100: (1.5-4): (3-6), firstly stir the modified magnesite powder and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture A; ball mill the mixture A for 20-30 minutes to obtain a ball-milled magnesite powder, heat treat the ball-milled magnesite powder, break it up, crush it, grade it or sieve it, and obtain a light-burned magnesium oxide powder;
[0012] S3.2: According to the mass ratio, modified magnesite fine aggregate: solid modifier: ball milling aid = 100: (1.5-4): (2-4), firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; ball mill the mixture B for 20-30 minutes to obtain ball milled magnesite fine aggregate, heat treat the ball milled magnesite fine aggregate, break it up, crush it, grade it or sieve it, and obtain light-burned magnesium oxide fine aggregate;
[0013] S3.3: According to the mass ratio, the modified magnesite coarse aggregate: solid modifier: ball milling aid = 100: (1-3): (2-4), firstly stir and evenly mix the modified magnesite coarse aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture C; after ball milling the mixture C for 20min-30min, obtain ball milled magnesite coarse aggregate, heat treat the ball milled magnesite coarse aggregate, break up, crush, grade or screen, and obtain light-burned magnesium oxide coarse aggregate;
[0014] S4: According to the mass ratio, light-burned magnesia coarse aggregate: light-burned magnesia fine aggregate: light-burned magnesia powder = (30-50): (20-60): (10-15), mix them in proportion to obtain light-burned magnesia composite refractory material.
[0015] In S1 of the above preparation method, the particle size range of the magnesite powder is 20μm<particle size ≤500μm; the particle size range of the magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of the magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0016] In S2 of the above preparation method, the solid-liquid mass ratio of the stirring, mixing and soaking is solid:liquid = (1-2): (6-10); the solid is dolomite powder, dolomite fine aggregate or dolomite coarse aggregate, and the liquid is a liquid modifier; the rotation speed of the stirring, mixing and soaking is 80rpm-120rpm, and the time is 20min-40min.
[0017] In S2 of the above preparation method, the particle size range of the modified magnesite powder is 20μm<particle size ≤500μm; the particle size range of the modified magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of the modified magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0018] In S3 of the above preparation method, the particle size range of the titanium carbide, boron carbide and sodium methylene bisnaphthalene sulfonate is 0 nm < particle size less than 300 nm.
[0019] In S3.1 of the above preparation method, the heating curve of the heat treatment is to heat to 600°C and keep warm for 20min to 30min, continue to heat to 650°C to 700°C and keep warm for 30min to 50min, continue to heat to 800°C to 850°C and keep warm for 30min to 50min; the particle size range of the light-burned magnesium oxide powder is 5μm<particle size≤500μm.
[0020] In S3.2 of the above preparation method, the heating curve of the heat treatment is to heat to 600°C and keep warm for 30min to 40min, continue to heat to 650°C to 700°C and keep warm for 30min to 50min, continue to heat to 800°C to 850°C and keep warm for 60min to 120min; the particle size range of the light-burned magnesium oxide fine aggregate is 500μm<particle size≤1mm.
[0021] In S3.3 of the above preparation method, the heating curve of the heat treatment is to heat to 600°C and keep warm for 30min to 40min, continue to heat to 650°C to 700°C and keep warm for 60min to 90min, continue to heat to 800°C to 850°C and keep warm for 120min to 180min; the particle size range of the light-burned magnesia coarse aggregate is 1mm<particle size≤3.5mm.
[0022] In S4 of the above preparation method, the light-burned magnesium oxide composite refractory material is mixed with a binder to obtain a ramming material, which is used as a furnace bottom ramming material and a furnace slope repairing material. After ramming construction in the furnace, the temperature is increased and the furnace is baked for curing.
[0023] The mixing mass ratio of the light-burned magnesium oxide composite refractory material and the binder is light-burned magnesium oxide composite refractory material: binder = 100: (5-10).
[0024] The binder comprises zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = (1-3): (1-3): (2-4): (4-6).
[0025] The curing temperature of the warm oven is above 1400°C.
[0026] The preparation method of a light-burned magnesium oxide composite refractory material provided by the present invention has the following beneficial effects compared with the prior art:
[0027] 1. In the prior art, magnesite is generally sintered to form light-burned magnesium oxide or dead-burned magnesium oxide, which is then compounded with other ingredients to prepare amorphous refractory materials or shaped refractory materials. The particle structure of the light-burned magnesium oxide or dead-burned magnesium oxide does not undergo any essential change, so the performance of magnesium oxide itself cannot be greatly improved.
[0028] The present invention modifies the magnesite ore at the magnesite ore stage, adds titanium carbide and boron carbide, fills and coats the surface of the magnesite ore, reduces surface defects and surface porosity, and forms particles with a dense structure. After subsequent sintering, the crystal structure of the magnesite material particles changes and shrinks, so that part of the titanium carbide and boron carbide are embedded in the light-burned magnesium oxide particles, which changes the characteristics of the particles from the perspective of the actual structure, making the particles denser, harder, and with a lower creep rate.
[0029] 2. The present invention prepares the liquid modifier, and uses polyvinyl pyrrolidone PVP-K30 and a water-soluble high-carbon alcohol defoamer in combination to reduce the bubbles generated during the stirring and mixing of the liquid modifier and the magnesite material, so that the polyvinyl pyrrolidone PVP-K30 can be fully attached to the surface of the magnesite material particles (including defects and pores); forming a hydrophilic film. When the solid modifier and the ball milling aid are subsequently ball milled, the hydrophilic film can make it easier for the surface of the magnesite material particles to combine with the solid modifier and the ball milling aid, without bubbles and repulsion, and the magnesite material particles are more tightly combined with nano-sized titanium carbide and boron carbide, and the magnesite material particles have better defect and pore filling properties.
[0030] 3. The ball milling aid is made of water, soybean oil and Tween 80, which has lubricity, can better disperse nano powders, and has good oil-water emulsification without stratification. In addition, the ball milling aid is used in combination with sodium methylene bis naphthalene sulfonate, which can be dissolved in the ball milling aid to improve the emulsification of the ball milling aid. The liquid adheres to the surface of nano titanium carbide and boron carbide particles, improves the fluidity and dispersibility of nano titanium carbide and boron carbide particles, and improves the affinity of nano powders with magnesite particles. It is easy to modify the surface and evenly adhere to the magnesite particles, achieving a good modification effect, better homogeneity, and improving the overall compressive and flexural strength of the ramming material.
[0031] Fourth, the present invention designs the ball milling time to be 20 minutes to 30 minutes according to the properties and particle size of each powder and the properties and dosage of the ball milling aid, which will not produce a large amount of ball milled fine powder and can well achieve uniform ball milling modification of the powder.
[0032] 5. The present invention designs different proportions of modified magnesite to solid modifier and ball milling aid according to the different particle size ranges of magnesite ore materials, which saves the amount of solid modifier and ball milling aid, ensures the uniformity of surface attachment modification, and does not introduce excessive fine powder, resulting in a large amount of waste of by-product costs.
[0033] 6. The present invention designs a heating curve and holding time for heat treatment according to different particle sizes of ball-milled magnesite materials, which can ensure the orderly transformation of the particle crystal form at 600°C, 650°C-700°C, and 800°C-850°C, and ensure the safe embedding of nano-titanium carbide and boron carbide, and will not cause particle collapse due to the rapid shrinkage of the magnesite material and the resistance of the nano-titanium carbide and boron carbide to shrinkage.
[0034] 7. The present invention adopts light-burned magnesium oxide composite refractory material and binder to prepare ramming mass. The binder contains liquid phenolic resin, which can well improve the binding property of ramming mass components and improve the performance of ramming mass to a certain extent.
[0035] In summary, the present invention uses magnesite as a raw material, crushes it into magnesite materials of different particle sizes, uses polyvinyl pyrrolidone PVP-K30 and a water-soluble high-carbon alcohol defoamer to hydrophilically modify the surface of the magnesite particles, then uses nano-titanium carbide and boron carbide to coat the surface of the magnesite and embed defective pores through ball milling modification, uses sodium methylenebisnaphthalene sulfonate, a ball milling aid and a hydrophilic film in combination to improve the workability and homogeneity of the solid modification, and then performs orderly heat treatment to obtain light-burned magnesium oxide, improves the density and hardness of the light-burned magnesium oxide material particles, reduces creep resistance, and essentially improves the characteristics of light-burned magnesium oxide, greatly improves the compressive strength, thermal shock resistance, creep resistance, etc. of the magnesium ramming material after use, and prolongs the service life. The material composite homogeneity between the magnesite particles, nano-titanium carbide and nano-boron carbide is better, can allow a larger lining construction operation error, is less affected by the construction operation, and can ensure the long-term use of the lining. DETAILED DESCRIPTION
[0036] Embodiment 1:
[0037] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0038] S1: Take magnesite, crush, grade or screen it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; wherein the particle size range of magnesite powder is 20μm<particle size ≤500μm; the particle size range of magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0039] S2: Mix water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer in a mass ratio of 100:5:2.0:3.5 to obtain a liquid modifier; wherein the water-soluble high-carbon alcohol defoamer is a high-carbon alcohol defoamer of Jinan Zhongao Chemical Co., Ltd., model 701C;
[0040] According to the solid-liquid mass ratio of solid: liquid = 1.5:8, the magnesite powder is placed in the liquid modifier, stirred and mixed at 100rpm and soaked for 30min, filtered, dried, crushed, graded or sieved to obtain modified magnesite powder with a particle size range of 20μm < particle size ≤ 500μm;
[0041] According to the solid-liquid mass ratio of solid: liquid = 1.5:8, the magnesite fine aggregate is placed in the liquid modifier, stirred and mixed at 100rpm and soaked for 30min, filtered, dried, crushed, graded or sieved to obtain modified magnesite fine aggregate with a particle size range of 500μm<particle size≤1mm;
[0042] The magnesite coarse aggregate is placed in the liquid modifier at a solid-liquid mass ratio of solid:liquid=1.5:8, and the mixture is stirred and soaked at 100rpm for 30 minutes, filtered, dried, crushed, graded or sieved to obtain modified magnesite coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0043] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 1.8:2.0:0.5 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0044] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100: 12: 2.5 by mass ratio;
[0045] According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100:3:4.5, the modified magnesite powder and the solid modifier are first stirred at 50rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 25 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 25 minutes, continuing to heat to 680°C and keeping warm for 40 minutes, continuing to heat to 820°C and keeping warm for 40 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0046] According to the mass ratio, the modified magnesite fine aggregate: solid modifier: ball milling aid = 100:3:3, firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; after ball milling the mixture B for 25 minutes, obtain the ball milled magnesite fine aggregate, and heat treat the ball milled magnesite fine aggregate, the heating curve is: heating to 600°C and keeping it for 35 minutes, continuing to heat to 680°C and keeping it for 40 minutes, continuing to heat to 820°C and keeping it for 90 minutes, and then breaking up, crushing, grading or screening after cooling to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0047] According to the mass ratio, the modified magnesite coarse aggregate: the solid modifier: the ball milling aid = 100:2:3. The modified magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 25 minutes to obtain the ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated. The heating curve is as follows: heating to 600°C and keeping warm for 35 minutes, continuing to heating to 680°C and keeping warm for 80 minutes, continuing to heating to 820°C and keeping warm for 160 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0048] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is mixed in a ratio of 35:50:12 to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is mixed in a ratio of 100:7 to obtain a ramming material, which is used for furnace bottom ramming material and furnace slope repair material. After ramming construction in the furnace, it is heated to 1500°C and baked in a furnace for curing;
[0049] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 2:2:3:5.
[0050] Embodiment 2:
[0051] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0052] S1: Take magnesite, crush, grade or screen it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; wherein the particle size range of magnesite powder is 20μm<particle size ≤500μm; the particle size range of magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0053] S2: Mix water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer in a mass ratio of 100:10:1.8:2.5 to obtain a liquid modifier; wherein the water-soluble high-carbon alcohol defoamer is a high-carbon alcohol defoamer of Jinan Zhongao Chemical Co., Ltd., model 701C;
[0054] According to the solid-liquid mass ratio of solid: liquid = 1.2:7, the magnesite powder is placed in the liquid modifier, stirred and mixed at 85rpm and soaked for 25min, filtered, dried, crushed, graded or sieved to obtain the modified magnesite powder with a particle size range of 20μm<particle size≤500μm;
[0055] According to the solid-liquid mass ratio of solid: liquid = 1.2:7, the magnesite fine aggregate is placed in the liquid modifier, stirred and mixed at 85rpm and soaked for 25min, filtered, dried, crushed, graded or sieved to obtain modified magnesite fine aggregate with a particle size range of 500μm<particle size≤1mm;
[0056] The magnesite coarse aggregate is placed in the liquid modifier at a solid-liquid mass ratio of solid:liquid=1.2:7, and the mixture is stirred and soaked at 85rpm for 25min, filtered, dried, crushed, graded or sieved to obtain modified magnesite coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0057] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 1.5:1.2:0.4 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0058] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100: 11: 2.2 by mass ratio;
[0059] According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100:2.0:4, the modified magnesite powder and the solid modifier are first stirred at 45rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 25 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 25 minutes, continuing to heat to 660°C and keeping warm for 35 minutes, and continuing to heat to 810°C and keeping warm for 35 minutes. After cooling, the powder is dispersed, crushed, graded or sieved to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0060] According to the mass ratio, the modified magnesite fine aggregate: solid modifier: ball milling aid = 100: 2.0: 2.5, firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; after ball milling the mixture B for 25 minutes, obtain the ball milled magnesite fine aggregate, and heat treat the ball milled magnesite fine aggregate, the heating curve is: heating to 600°C and keeping it for 35 minutes, continuing to heat to 660°C and keeping it for 35 minutes, continuing to heat to 810°C and keeping it for 70 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0061] According to the mass ratio, the modified magnesite coarse aggregate: the solid modifier: the ball milling aid = 100: 1.5: 2.5. The modified magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 25 minutes to obtain the ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 35 minutes, continuing to heating to 660°C and keeping warm for 70 minutes, continuing to heating to 810°C and keeping warm for 140 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0062] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is 40:30:11, and the mixture is mixed to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is 100:6, and the ramming material is obtained, which is used for the furnace bottom ramming material and the furnace slope repair material. After ramming construction in the furnace, the furnace is heated to 1450°C for curing;
[0063] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 1.5:1.2:2.5:4.5.
[0064] Embodiment 3:
[0065] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0066] S1: Take magnesite, crush, grade or screen it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; wherein the particle size range of magnesite powder is 20μm<particle size ≤500μm; the particle size range of magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0067] S2: Mix water: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer in a mass ratio of 100:1.5:2 to obtain a liquid modifier; wherein the water-soluble high-carbon alcohol defoamer is a high-carbon alcohol defoamer of Jinan Zhongao Chemical Co., Ltd., model 701C;
[0068] According to the solid-liquid mass ratio of solid: liquid = 1:6, the magnesite powder is placed in the liquid modifier, stirred and mixed at 80 rpm and soaked for 20 minutes, filtered, dried, crushed, graded or sieved to obtain modified magnesite powder with a particle size range of 20 μm < particle size ≤ 500 μm;
[0069] According to the solid-liquid mass ratio of solid: liquid = 1:6, the magnesite fine aggregate is placed in the liquid modifier, stirred and mixed at 80rpm and soaked for 20min, filtered, dried, crushed, graded or sieved to obtain modified magnesite fine aggregate with a particle size range of 500μm<particle size≤1mm;
[0070] The magnesite coarse aggregate is placed in the liquid modifier at a solid-liquid mass ratio of solid:liquid=1:6, and the mixture is stirred and soaked at 80rpm for 20min, filtered, dried, crushed, graded or sieved to obtain modified magnesite coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0071] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 1:1:0.3 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0072] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100:10:2 by mass ratio;
[0073] According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100: 1.5: 3, the modified magnesite powder and the solid modifier are first stirred at 40 rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 20 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 20 minutes, continuing to heat to 650°C and keeping warm for 30 minutes, and continuing to heat to 800°C and keeping warm for 30 minutes. After cooling, the powder is dispersed, crushed, graded or sieved to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm < particle size ≤ 500μm;
[0074] According to the mass ratio, the modified magnesite fine aggregate: solid modifier: ball milling aid = 100:1.5:2, firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; after ball milling the mixture B for 20 minutes, obtain the ball milled magnesite fine aggregate, and heat treat the ball milled magnesite fine aggregate, the heating curve is: heating to 600°C and keeping it for 30 minutes, continuing to heat to 650°C and keeping it for 30 minutes, continuing to heat to 800°C and keeping it for 60 minutes, and then cooling down, breaking up, crushing, grading or screening to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0075] According to the mass ratio, the modified magnesite coarse aggregate: solid modifier: ball milling aid = 100:1:2, the modified magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 20 minutes to obtain a ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 30 minutes, continuing to heating to 650°C and keeping warm for 60 minutes, and continuing to heating to 800°C and keeping warm for 120 minutes. After cooling, it is dispersed, crushed, graded or sieved to obtain a light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0076] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is mixed in a ratio of 30:20:10 to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is mixed in a ratio of 100:5 to obtain a ramming material, which is used for furnace bottom ramming material and furnace slope repair material. After ramming construction in the furnace, it is heated to 1400°C and baked in a furnace for curing;
[0077] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 1:1:2:4.
[0078] Embodiment 4:
[0079] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0080] S1: Take magnesite, crush, grade or screen it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; wherein the particle size range of magnesite powder is 20μm<particle size ≤500μm; the particle size range of magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0081] S2: Mix water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer in a mass ratio of 100:15:3.0:4 to obtain a liquid modifier; wherein the water-soluble high-carbon alcohol defoamer is a high-carbon alcohol defoamer of Jinan Zhongao Chemical Co., Ltd., model 701C;
[0082] According to the solid-liquid mass ratio of solid: liquid = 1.8:9, the magnesite powder is placed in the liquid modifier, stirred and mixed at 110 rpm and soaked for 35 minutes, filtered, dried, crushed, graded or sieved to obtain modified magnesite powder with a particle size range of 20 μm < particle size ≤ 500 μm;
[0083] According to the solid-liquid mass ratio of solid: liquid = 1.8:9, the magnesite fine aggregate is placed in the liquid modifier, stirred and mixed at 110rpm and soaked for 35min, filtered, dried, crushed, graded or sieved to obtain modified magnesite fine aggregate with a particle size range of 500μm<particle size≤1mm;
[0084] The magnesite coarse aggregate is placed in the liquid modifier at a solid-liquid mass ratio of solid:liquid=1.8:9, and the mixture is stirred and soaked at 110 rpm for 35 minutes, filtered, dried, crushed, graded or sieved to obtain modified magnesite coarse aggregate with a particle size range of 1 mm < particle size ≤ 3.5 mm.
[0085] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 2.2:2.0:0.8 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0086] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100: 14: 2.6 by mass ratio;
[0087] According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100:3:5.5, the modified magnesite powder and the solid modifier are first stirred at 55rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 25 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 25 minutes, continuing to heat to 680°C and keeping warm for 45 minutes, continuing to heat to 840°C and keeping warm for 45 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0088] According to the mass ratio, the modified magnesite fine aggregate: solid modifier: ball milling aid = 100:3.5:3.5, firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; after ball milling the mixture B for 25 minutes, obtain the ball milled magnesite fine aggregate, and heat treat the ball milled magnesite fine aggregate, the heating curve is: heating to 600℃ and keeping it for 35 minutes, continuing to heat to 680℃ and keeping it for 45 minutes, continuing to heat to 840℃ and keeping it for 100 minutes, and then breaking up, crushing, grading or screening after cooling to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0089] According to the mass ratio, the modified magnesite coarse aggregate: solid modifier: ball milling aid = 100:2.5:3.5. The modified magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 25 minutes to obtain a ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated. The heating curve is as follows: heating to 600°C and keeping warm for 35 minutes, continuing to heating to 680°C and keeping warm for 80 minutes, continuing to heating to 840°C and keeping warm for 160 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain a light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0090] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is 45:50:14, and the mixture is mixed to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is 100:8, and the ramming material is obtained after mixing, which is used for the furnace bottom ramming material and the furnace slope repair material. After ramming construction in the furnace, the furnace is heated to 1550°C for curing;
[0091] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 2.5:2.5:3.5:5.5.
[0092] Embodiment 5:
[0093] A method for preparing a light-burned magnesium oxide composite refractory material comprises the following steps:
[0094] S1: Take magnesite, crush, grade or screen it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; wherein the particle size range of magnesite powder is 20μm<particle size ≤500μm; the particle size range of magnesite fine aggregate is 500μm<particle size ≤1mm; the particle size range of magnesite coarse aggregate is 1mm<particle size ≤3.5mm.
[0095] S2: Mix water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer in a mass ratio of 100:20:3.5:5 to obtain a liquid modifier; wherein the water-soluble high-carbon alcohol defoamer is a high-carbon alcohol defoamer of Jinan Zhongao Chemical Co., Ltd., model 701C;
[0096] According to the solid-liquid mass ratio of solid: liquid = 2:10, the magnesite powder is placed in the liquid modifier, stirred and mixed at 120rpm and soaked for 40min, filtered, dried, crushed, graded or sieved to obtain modified magnesite powder with a particle size range of 20μm<particle size≤500μm;
[0097] According to the solid-liquid mass ratio of solid: liquid = 2:10, the magnesite fine aggregate is placed in the liquid modifier, stirred and mixed at 120rpm and soaked for 40min, filtered, dried, crushed, graded or sieved to obtain modified magnesite fine aggregate with a particle size range of 500μm<particle size≤1mm;
[0098] The magnesite coarse aggregate is placed in the liquid modifier at a solid-liquid mass ratio of solid:liquid=2:10, and the mixture is stirred and soaked at 120rpm for 40min, filtered, dried, crushed, graded or sieved to obtain modified magnesite coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0099] S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 2.5:2.5:1 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0100] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100:15:3 by mass ratio;
[0101] According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100:4:6, the modified magnesite powder and the solid modifier are first stirred at 60rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 30 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 30 minutes, continuing to heating to 700°C and keeping warm for 50 minutes, and continuing to heating to 850°C and keeping warm for 50 minutes. After cooling, the powder is dispersed, crushed, graded or sieved to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0102] According to the mass ratio, the modified magnesite fine aggregate: solid modifier: ball milling aid = 100:4:4, firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; after ball milling the mixture B for 30 minutes, obtain the ball milled magnesite fine aggregate, and heat treat the ball milled magnesite fine aggregate, the heating curve is: heating to 600°C and keeping the temperature for 40 minutes, continuing to heat to 700°C and keeping the temperature for 50 minutes, continuing to heat to 850°C and keeping the temperature for 120 minutes, and then cooling down, breaking up, crushing, grading or screening to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0103] According to the mass ratio, the modified magnesite coarse aggregate: solid modifier: ball milling aid = 100:3:4, the modified magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 30 minutes to obtain a ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 40 minutes, continuing to heating to 700°C and keeping warm for 90 minutes, and continuing to heating to 850°C and keeping warm for 180 minutes. After cooling, it is dispersed, crushed, graded or sieved to obtain a light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0104] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is 50:60:15, and the mixture is mixed to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is 100:10, and the ramming material is obtained, which is used for the furnace bottom ramming material and the furnace slope repair material. After ramming construction in the furnace, the furnace is heated to 1600°C for curing;
[0105] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 3:3:4:6.
[0106] Comparative Example 1:
[0107] The light-burned magnesium oxide composite refractory material of Comparative Example 1 is prepared, comprising the following steps:
[0108] S1: Take the magnesite powder, magnesite fine aggregate and magnesite coarse aggregate prepared in Example 1.
[0109] S2: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air stream in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = 1.8:2.0:0.5 to obtain a solid modifier; wherein the particle size of titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate is less than 300 nm;
[0110] The ball milling aid is prepared by mixing water: soybean oil: Tween 80 = 100: 12: 2.5 by mass ratio;
[0111] According to the mass ratio, magnesite powder: solid modifier: ball milling aid = 100:3:4.5, the magnesite powder and the solid modifier are first stirred at 50rpm to be uniformly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture A; the mixture A is ball milled for 25 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping warm for 25 minutes, continuing to heat to 680°C and keeping warm for 40 minutes, continuing to heat to 820°C and keeping warm for 40 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0112] According to the mass ratio, magnesite fine aggregate: solid modifier: ball milling aid = 100:3:3, first stir the magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; ball mill the mixture B for 25 minutes to obtain ball-milled magnesite fine aggregate, and heat treat the ball-milled magnesite fine aggregate, the heating curve is: heating to 600℃ and keeping it for 35 minutes, continuing to heat to 680℃ and keeping it for 40 minutes, continuing to heat to 820℃ and keeping it for 90 minutes, and then breaking up, crushing, grading or screening after cooling to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0113] According to the mass ratio, the magnesite coarse aggregate: solid modifier: ball milling aid = 100:2:3. The magnesite coarse aggregate and the solid modifier are first stirred and evenly mixed, and then the ball milling aid is sprayed under stirring to mix to obtain a mixture C; the mixture C is ball milled for 25 minutes to obtain the ball-milled magnesite coarse aggregate, and the ball-milled magnesite coarse aggregate is heat-treated. The heating curve is as follows: heating to 600°C and keeping warm for 35 minutes, continuing to heating to 680°C and keeping warm for 80 minutes, continuing to heating to 820°C and keeping warm for 160 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0114] S3: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is mixed in a ratio of 35:50:12 to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is mixed in a ratio of 100:7 to obtain a ramming material, which is used for furnace bottom ramming material and furnace slope repair material. After ramming construction in the furnace, it is heated to 1500°C and baked in a furnace for curing;
[0115] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 2:2:3:5.
[0116] Comparative Example 2:
[0117] The light-burned magnesium oxide composite refractory material of Comparative Example 2 is prepared, comprising the following steps:
[0118] S1: Take the magnesite powder, magnesite fine aggregate and magnesite coarse aggregate prepared in Example 1.
[0119] S2: mixing titanium carbide and boron carbide in an air flow at a mass ratio of titanium carbide: boron carbide = 1.8:2.0 to obtain a solid modifier; wherein the particle size of titanium carbide and boron carbide is less than 300 nm;
[0120] According to the mass ratio, the magnesite powder: solid modifier = 100:3, the magnesite powder and the solid modifier are first stirred at 50rpm to obtain a mixture A; the mixture A is ball-milled for 25 minutes to obtain a ball-milled magnesite powder, and the ball-milled magnesite powder is heat-treated, and the heating curve is as follows: heating to 600°C and keeping it for 25 minutes, continuing to heat to 680°C and keeping it for 40 minutes, and continuing to heat to 820°C and keeping it for 40 minutes. After cooling, it is dispersed, crushed, graded or sieved to obtain a light-burned magnesium oxide powder, and the particle size range is 5μm<particle size≤500μm;
[0121] According to the mass ratio, magnesite fine aggregate: solid modifier = 100:3, first stir and mix the magnesite fine aggregate and the solid modifier to obtain a mixture B; ball-mill the mixture B for 25 minutes to obtain ball-milled magnesite fine aggregate, and heat-treat the ball-milled magnesite fine aggregate. The heating curve is: heating to 600°C and keeping it for 35 minutes, then heating to 680°C and keeping it for 40 minutes, then heating to 820°C and keeping it for 90 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia fine aggregate, the particle size range is 500μm<particle size≤1mm;
[0122] According to the mass ratio, the magnesite coarse aggregate: solid modifier = 100:2. The magnesite coarse aggregate and the solid modifier are first stirred and mixed to obtain a mixture C. The mixture C is ball-milled for 25 minutes to obtain ball-milled magnesite coarse aggregate. The ball-milled magnesite coarse aggregate is heat-treated. The heating curve is as follows: heating to 600°C and keeping warm for 35 minutes, then heating to 680°C and keeping warm for 80 minutes, then heating to 820°C and keeping warm for 160 minutes. After cooling, the mixture is broken up, crushed, graded or sieved to obtain light-burned magnesia coarse aggregate. The particle size range is 1mm<particle size≤3.5mm.
[0123] S3: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder is mixed in a ratio of 35:50:12 to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder is mixed in a ratio of 100:7 to obtain a ramming material, which is used for furnace bottom ramming material and furnace slope repair material. After ramming construction in the furnace, it is heated to 1500°C and baked in a furnace for curing;
[0124] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 2:2:3:5.
[0125] Comparative Example 3:
[0126] The light-burned magnesium oxide composite refractory material of Comparative Example 3 is prepared, comprising the following steps:
[0127] S1: Take the magnesite powder, magnesite fine aggregate and magnesite coarse aggregate prepared in Example 1.
[0128] S2: Titanium carbide and boron carbide are mixed in an air flow in a mass ratio of titanium carbide:boron carbide=1.8:2.0 to obtain a solid modifier; wherein the particle size of titanium carbide and boron carbide is less than 300 nm.
[0129] S3: heat-treating the magnesite powder, with a heating curve of heating to 600°C and keeping the temperature for 25 minutes, then heating to 680°C and keeping the temperature for 40 minutes, then heating to 820°C and keeping the temperature for 40 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesium oxide powder with a particle size range of 5μm<particle size≤500μm;
[0130] The magnesite fine aggregate is heat treated, and the heating curve is as follows: heating to 600°C and keeping the temperature for 35 minutes, then heating to 680°C and keeping the temperature for 40 minutes, then heating to 820°C and keeping the temperature for 90 minutes, and then cooling down and breaking up, crushing, grading or screening to obtain light-burned magnesia fine aggregate, with a particle size range of 500μm<particle size≤1mm;
[0131] The magnesite coarse aggregate is heat treated, and the heating curve is as follows: heating to 600°C and keeping the temperature for 35 minutes, then heating to 680°C and keeping the temperature for 80 minutes, then heating to 820°C and keeping the temperature for 160 minutes. After cooling, the aggregate is broken up, crushed, graded or sieved to obtain light-burned magnesia coarse aggregate with a particle size range of 1mm<particle size≤3.5mm.
[0132] S4: According to the mass ratio, the light-burned magnesia coarse aggregate: the light-burned magnesia fine aggregate: the light-burned magnesia powder: the solid modifier = 35:50:12:2.6, and the mixture is mixed to obtain a light-burned magnesia composite refractory material; according to the mass ratio, the light-burned magnesia composite refractory material: the binder = 100:7, and the ramming material is obtained after mixing, which is used for the furnace bottom ramming material and the furnace slope repair material. After ramming construction in the furnace, the furnace is heated to 1500°C for curing;
[0133] The binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = 2:2:3:5.
[0134] Comparative Example 4:
[0135] The binder includes zirconium oxide powder, boron powder and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: soybean oil = 2:2:5. Other method parameters are the same as those of comparative example 3.
[0136] 1. The ramming materials of each embodiment and each comparative example were molded into rectangular specimens of 150mm*150mm*300mm. Several rectangular specimens were prepared for each ramming method. The specimens were baked at 200℃~250℃ for 1h, heated to 600℃ for 2h, heated to 1000℃ for 2h, heated to 1500℃ for 1h, and cooled to obtain test blocks.
[0137] The test blocks were tested for room temperature compressive strength, high temperature compressive strength at 1500℃·30min, creep rate, thermal shock stability at 1500℃·30min·air cooling, and creep rate at 1500℃·60h. Five parallel samples were made for each test and the average value was taken. The test results are shown in Table 1 below:
[0138] Table 1 Performance test results
[0139]
[0140] From the above results, it can be seen that the molding bricks of Examples 1 to 5 have good physical properties. The density and strength of the molding bricks themselves are lower than those of the pressed bricks. They can show a compressive strength of more than 45 MPa, and are high-performance ramming materials. In addition, the molding bricks have excellent thermal shock stability and creep resistance at 1500°C. From the results of Comparative Example 1, it can be seen that after the surface of the magnesite material is modified by water, ethanol, polyvinyl pyrrolidone PVP-K30, and a water-soluble high-carbon alcohol defoamer, the physical properties of the ramming material can be improved. This is because the polyvinyl pyrrolidone PVP-K30 and the water-soluble high-carbon alcohol defoamer are combined to form a hydrophilic film that adheres to the surface of the magnesite on the particle surface, surface defects, and particle pores of the magnesite material, laying the foundation for subsequent solid ball milling modification. The hydrophilic film is combined with the ball milling aid to make the solid modifier more evenly and densely applied to the particle surface, surface defects, and particle structure pores of the magnesite material. After subsequent high-temperature treatment, magnesium oxide particles with low defects and porosity, high hardness, and tight structure are obtained, thereby achieving a comprehensive improvement in various physical properties. From the result of comparative example 2, it can also be seen that the combined use effect of liquid modifier and ball milling aid, sodium methylene bis naphthalene sulfonate, when making ball milling, solid modifier is dispersed more evenly, solid modification and magnesite material bonding are made tighter, and surface defects and particle structure pores of magnesite material are fully filled. From the result of comparative example 3, it can be known that liquid modifier is not adopted to modify magnesite material, and the ball milling surface modification of solid modifier is not carried out, light-burned magnesia coarse aggregate, light-burned magnesia fine aggregate, light-burned magnesia powder are directly mixed with solid modifier, and simple mixing does not reach good surface modification effect, and the particle microstructure of light-burned magnesia material does not have substantial change, and the gap of last ramming material physical property test result and embodiment material is very large. From the result of comparative example 4, it can be known that adding liquid phenolic resin in binding agent helps to improve the bonding of ramming material composition, affects the use performance of ramming material to a certain extent.
[0141] 2. The body length of a small 15-meter test tunnel kiln pre-built by a certain manufacturer is divided into three equal sections of A (furnace head), B (furnace middle), and C (furnace tail). Each section is divided into 9 small sections, which are marked. Refractory bricks and ramming materials are used to build the lining of the test tunnel kiln. The brick joints of adjacent refractory bricks are spaced 6 mm and filled with ramming materials. Each small section corresponds to the ramming materials of Examples 1 to 5 and Comparative Examples 1 to 4. The ramming materials of the three sections are recycled in the 9 small sections. That is, each ramming material forms parallel samples in three different temperature zones.
[0142] After the construction of the small test 15-meter tunnel kiln was completed, the furnace was heated to 1500℃ for curing; then the R&D test samples were heat treated by repeated heating and cooling at 1000℃, and the total time of high temperature of 1200℃ was maintained for not less than 4 hours every day. After 2 months, 4 months, and 6 months of operation, the furnace was stopped, the furnace shell was dismantled, and the furnace lining condition was observed. The results are shown in Table 2 below:
[0143] Table 2 Trial comparison results
[0144]
[0145] Observation and evaluation standards for the ramming material area: 0-no obvious cracks on the surface; 1-fine cracks on the surface (more than 1 and less than 10), with a maximum width of less than 1mm; 2-many fine cracks on the surface (more than 10 and less than 20), with a maximum width of less than 2mm; 3-a large number of cracks on the surface (more than 20), with a maximum width of more than 2mm, which requires timely repair.
[0146] It can be seen from the above test results that the ramming materials of Examples 1 to 5 can have high temperature durability, require no maintenance during the 6-month service life, and will not cause the risk of furnace penetration. They can greatly reduce the maintenance frequency, save maintenance costs, save maintenance time, and improve production efficiency.
Claims
1. A method for preparing a light-burned magnesium oxide composite refractory material, It is characterized in that The steps include: S1: taking magnesite, crushing and classifying it to obtain magnesite powder, magnesite fine aggregate and magnesite coarse aggregate respectively; S2: Mix the mixture according to the mass ratio of water: ethanol: polyvinyl pyrrolidone PVP-K30: water-soluble high-carbon alcohol defoamer = 100: (0-20): (1.5-3.5): (2-5) to obtain a liquid modifier; Taking magnesite powder, magnesite fine aggregate and magnesite coarse aggregate, respectively placing them in a liquid modifier, stirring, mixing and soaking, filtering, drying, crushing and classifying, and respectively obtaining modified magnesite powder, modified magnesite fine aggregate and modified magnesite coarse aggregate; S3: titanium carbide, boron carbide and sodium methylene bis naphthalene sulfonate are mixed in an air flow in a mass ratio of titanium carbide: boron carbide: sodium methylene bis naphthalene sulfonate = (1-2.5): (1-2.5): (0.3-1) to obtain a solid modifier; The particle size range of the titanium carbide, boron carbide and sodium methylene bisnaphthalene sulfonate is 0nm<particle size<300nm; According to the mass ratio, water: soybean oil: Tween 80 = 100: (10-15): (2-3), mix and prepare the ball milling aid; S3.1: According to the mass ratio, the modified magnesite powder: solid modifier: ball milling aid = 100: (1.5-4): (3-6), firstly stir the modified magnesite powder and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture A; ball mill the mixture A for 20-30 minutes to obtain a ball-milled magnesite powder, heat treat the ball-milled magnesite powder, break it up, crush it, and classify it to obtain a light-burned magnesium oxide powder; The heating curve of the heat treatment is: heating to 600°C and keeping it for 20min-30min, then heating to 650°C-700°C and keeping it for 30min-50min, then heating to 800°C-850°C and keeping it for 30min-50min; S3.2: According to the mass ratio, modified magnesite fine aggregate: solid modifier: ball milling aid = 100: (1.5-4): (2-4), firstly stir and evenly mix the modified magnesite fine aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture B; ball mill the mixture B for 20-30 minutes to obtain ball milled magnesite fine aggregate, heat treat the ball milled magnesite fine aggregate, break it up, crush it, and classify it to obtain light-burned magnesium oxide fine aggregate; The heating curve of the heat treatment is: heating to 600°C and keeping it for 30min-40min, then heating to 650°C-700°C and keeping it for 30min-50min, then heating to 800°C-850°C and keeping it for 60min-120min. S3.3: According to the mass ratio, the modified magnesite coarse aggregate: solid modifier: ball milling aid = 100: (1-3): (2-4), firstly stir and evenly mix the modified magnesite coarse aggregate and the solid modifier, then spray the ball milling aid under stirring, mix, and obtain a mixture C; ball mill the mixture C for 20min-30min to obtain ball-milled magnesite coarse aggregate, heat treat the ball-milled magnesite coarse aggregate, break it up, crush it, and classify it to obtain light-burned magnesium oxide coarse aggregate; The heating curve of the heat treatment is: heating to 600°C and keeping it for 30min-40min, then heating to 650°C-700°C and keeping it for 60min-90min, then heating to 800°C-850°C and keeping it for 120min-180min. S4: According to the mass ratio, light-burned magnesia coarse aggregate: light-burned magnesia fine aggregate: light-burned magnesia powder = (30-50): (20-60): (10-15), mix them in proportion to obtain light-burned magnesia composite refractory material.
2. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S1, the particle size range of the magnesite powder is 20 μm < particle size ≤ 500 μm; the particle size range of the magnesite fine aggregate is 500 μm < particle size ≤ 1 mm; the particle size range of the magnesite coarse aggregate is 1 mm < particle size ≤ 3.5 mm.
3. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S2, the solid-liquid mass ratio of the stirring, mixing and soaking is solid:liquid = (1-2): (6-10); the solid is magnesite powder, magnesite fine aggregate or magnesite coarse aggregate, and the liquid is a liquid modifier; the rotation speed of the stirring, mixing and soaking is 80rpm-120rpm, and the time is 20min-40min.
4. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S2, the particle size range of the modified magnesite powder is 20 μm < particle size ≤ 500 μm; the particle size range of the modified magnesite fine aggregate is 500 μm < particle size ≤ 1 mm; the particle size range of the modified magnesite coarse aggregate is 1 mm < particle size ≤ 3.5 mm.
5. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S3.1, the particle size range of the light-burned magnesium oxide powder is 5 μm<particle size≤500 μm.
6. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S3.2, the particle size range of the light-burned magnesia fine aggregate is 500 μm<particle size ≤ 1 mm.
7. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S3.3, the particle size range of the light-burned magnesia coarse aggregate is 1mm<particle size≤3.5mm.
8. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 1, It is characterized in that In S4, the light-burned magnesium oxide composite refractory material is mixed with a binder to obtain a ramming material, which is used as a furnace bottom ramming material and a furnace slope repairing material. After ramming construction in the furnace, the temperature is increased and the furnace is baked for solidification.
9. The method for preparing a light-burned magnesium oxide composite refractory material according to claim 8, It is characterized in that The mass ratio of the mixture is light-burned magnesium oxide composite refractory material: binder = 100: (5-10); the binder includes zirconium oxide powder, boron powder, liquid phenolic resin and soybean oil, and the mass ratio is zirconium oxide powder: boron powder: liquid phenolic resin: soybean oil = (1-3): (1-3): (2-4): (4-6); the curing temperature of the warm baking furnace is above 1400°C.
Citation Information
Patent Citations
Production method of light calcined magnesia
CN107010852A
Method for preparing high-density magnesia by utilizing microwave sintering of magnesite
CN109553311A