Electronic adhesive containing modified butadiene and preparation method thereof

Through the combination of modified polyester polyol and modified butadiene, the electronic glue formula and preparation method are optimized, and the existing electronic glue has poor stability and low production efficiency at extreme temperatures are solved, and the flexibility of electronic glue is achieved. The improvement of surface drying time and shear strength improves its application reliability and production efficiency.

CN118638504BActive Publication Date: 2024-11-08山东威特化工有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411102738.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing electronic glue has poor stability at extreme temperatures and low production efficiency, making it difficult to meet the requirements of flexibility, surface drying time and shear strength at the same time, affecting its application reliability and production efficiency.

Method used

Using a combination of modified polyester polyol and modified butadiene, combined with toluene diisocyanate, bis(2-morpholine diethyl) ether, p-toluenesulfonyl isocyanate and gamma-glycidyl ether by optimizing formulation and preparation method Components such as oxypropyl trimethoxysilane are prepared to produce electronic glue with good flexibility, surface drying time and shear strength.

Benefits of technology

The flexibility, surface drying time and shear strength of electronic glue is achieved, and the application reliability and production efficiency of electronic glue is improved, ensuring stability at extreme temperatures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an electronic adhesive containing modified butadiene and a preparation method thereof, belonging to the technical field of electronic adhesives, comprising 20-25 parts of modified polyester polyol, 13 parts of toluene diisocyanate, 0.8 parts of bis(2-morpholine diethyl) ether, 30 parts of modified butadiene, 1.1 parts of p-toluenesulfonyl isocyanate, 1.1 parts of γ-glycidyl ether oxypropyl trimethoxy silane, 1.1 parts of antioxidant, and 0.25 parts of defoamer; the antioxidant is antioxidant 1010, and the defoamer is BYK-24043. The electronic adhesive of the invention has good flexibility and takes into account good surface drying time and shear strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic adhesives and relates to an electronic adhesive containing modified butadiene and a preparation method thereof. Background Art

[0002] Electronic glue is an adhesive specially used in the electronics industry. It has a series of properties to meet the special requirements of electronic equipment during manufacturing and use.

[0003] In the prior art, a patent application with application number CN202410160227.6 and patent name "Method for preparing high-hardness polyurethane electronic adhesive" discloses that high-hardness polyurethane electronic adhesive is prepared by the reaction of substances, thereby improving the hardness, waterproofness and mechanical properties of the electronic adhesive. However, it ignores the fact that when the electronic adhesive is used, it not only requires a certain hardness, but also a certain flexibility. At present, when the electronic adhesive is in use, because the electronic product is heated, heat will be transferred to the electronic adhesive. If the hardness is only increased, it will be difficult to ensure the stability of the electronic adhesive at extreme temperatures, and it will be difficult to improve the reliability of the electronic adhesive in long-term operation.

[0004] In addition, the electronic glue also needs to increase the surface drying time, which can improve the production efficiency when the electronic glue is used in the production of electronic products. Otherwise, if it only has flexibility, the production efficiency is too low, which greatly affects the application of the electronic glue. Moreover, if only flexibility is considered without considering the shear strength, the reliability of the electronic glue will be affected. Therefore, flexibility, surface drying time and shear strength need to be considered so that the electronic glue can be better applied.

[0005] Based on the above research, it is necessary to provide an electronic adhesive containing modified butadiene. Summary of the invention

[0006] The purpose of the present invention is to provide an electronic adhesive containing modified butadiene and a preparation method thereof. In order to provide an electronic adhesive that can comprehensively meet the requirements of flexibility, surface drying time and shear strength, the existing electronic adhesives can often only improve one of their properties. This application optimizes the electronic adhesive formula and improves the preparation method of the electronic adhesive, so that the prepared electronic adhesive has better flexibility, better surface drying time, and improved shear strength.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] The invention comprises 20-25 parts of modified polyester polyol, 13 parts of toluene diisocyanate, 0.8 parts of bis(2-morpholine diethyl) ether, 30 parts of modified butadiene, 1.1 parts of p-toluenesulfonyl isocyanate, 1.1 parts of γ-glycidyl ether oxypropyl trimethoxy silane, 1.1 parts of antioxidant and 0.25 parts of defoaming agent;

[0009] The antioxidant is antioxidant 1010, and the defoaming agent is BYK-24043;

[0010] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0011] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0012] Preferably, the hydroxyl value of the modified polyester polyol is 50-55 mg KOH / g.

[0013] Preferably, the molecular weight of maleic anhydride polybutadiene is 3300-3500. By selecting maleic anhydride polybutadiene with a suitable molecular weight, the modified butadiene will not be too brittle due to excessive molecular chain length during preparation, which will affect the flexibility, surface drying time and shear strength of the electronic adhesive.

[0014] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.2-1.5.

[0015] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.5.

[0016] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.2.

[0017] A method for preparing electronic adhesive containing modified butadiene comprises the following steps:

[0018] S1: The modified polyester polyol, antioxidant and defoamer are mixed, heated to 70°C, maintained for 4 hours, then heated to 100°C, maintained for 1 hour, and then placed in a vacuum environment of -0.2Mpa for 3 hours;

[0019] S2: At 100°C, add modified butadiene, stir, cool to 70°C, maintain for 1 hour, add toluene diisocyanate, 70°C, maintain for 1 hour, then vacuum for 30 minutes, add bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention adopts a combination of modified polyester polyol and modified butadiene, and coordinates them with other components. In the synthesis, 1,4-butanediol is selected as the polyester polyol to react with suberic acid and epsilon-caprolactone. Because two -OH groups of 1,4-butanediol have a suitable distance, they can cooperate well with suberic acid and epsilon-caprolactone in the synthesis, so that their groups can interact with each other. Suberic acid, 1,4-butanediol and epsilon-caprolactone with a mass ratio of 3.5:1.8:0.9 can make the -OH of the modified polyester polyol have a certain retention. The modified butadiene and the -OH of the modified polyester polyol synergistically act, so that the prepared electronic adhesive has better flexibility, better surface drying time and better shear strength. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0023] The phenolic epoxy resin is commercially available or prepared by the following method: F-44 epoxy resin is a phenolic epoxy resin with a high epoxy value and good mechanical properties. The following is a detailed preparation method of F-44 epoxy resin:

[0024] Raw material preparation: Bisphenol A: As one of the main raw materials, bisphenol A is the starting material of epoxy resin. Epichlorohydrin: reacts with bisphenol A to form epoxy resin. NaOH: acts as a catalyst to promote the reaction. Reaction process: Mix bisphenol A and epichlorohydrin under stirring to dissolve bisphenol A. At a certain temperature, add the required amount of alkali (NaOH) to the mixture, maintain the reaction after the first drop of alkali, and recover epichlorohydrin. Add the remaining alkali to the reaction solution, maintain the reaction, and then add an appropriate amount of benzene to dissolve the resin solution, stir and let stand to separate.

[0025] Put the resin benzene solution on the upper layer into a stirring pot, stir, heat, maintain, and stand, remove the undissolved part of the bottom layer, then stir again, heat to make the resin benzene solution boil and reflux, remove the water from time to time until no bubbles appear, then maintain reflux, then cool, stand, and filter. Put the filtrate into a debenzening pot, first debenzene under normal pressure, then debenzene under reduced pressure, until no benzene liquid comes out, and obtain a light yellow liquid resin.

[0026] Post-treatment: The resin solution after the reaction is cooled and filtered to remove impurities. The solvent is removed by reduced pressure distillation to obtain pure phenolic epoxy resin.

[0027] Flexibility test: Apply the electronic glue to a suitable substrate, or directly use the electronic glue as an adhesive to bond two substrates together. After the electronic glue is cured, cut it into rectangular or circular pole pieces of specific size according to the test requirements. Wind the cut pole piece into a single-layer cylinder. Make sure the winding is tight and without gaps. Use double-sided tape or other appropriate fixing methods to stick the ends of the wound cylindrical pole piece to the test fixture. Place the cylindrical pole piece in the test equipment and apply pressure along the cylindrical radial direction. You can use a universal testing machine and other equipment for precise control. Stop pressurizing when the applied pressure reaches the preset value, and record the pressure value and the deformation distance of the cylindrical pole piece in the pressure direction. Evaluate the flexibility of the electronic glue based on the distance of deformation of the cylindrical pole piece under pressure. Measure the distance between the upper and lower pressure surfaces of the cylindrical pole piece under pressure, and take the reciprocal of the distance as a quantitative indicator of flexibility. The better the flexibility, the larger the value of this quantitative indicator.

[0028] Shear strength test: On an aluminum substrate with an area of ​​25.4mm*101.6mm, a glass sheet with an area of ​​3mm*3mm is bonded. The bonding surface of the glass sheet is fully coated with glue, and the thickness of the glue layer is 0.1~0.2mm. It is illuminated by a 365mm LED light source. After curing, the Dage chip thrust machine is used to test the edge of the glass sheet until it is broken. The speed is 6mm / min, and the shear strength at this time is recorded in MPa.

[0029] The test method for surface drying time can refer to GB / T 13477.5-2002.

[0030] In the following examples, the hydroxyl value of the modified polyester polyol is 50-55 mg KOH / g. The molecular weight of the maleic anhydride polybutadiene is 3300-3500.

[0031] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0032] The invention comprises 20-25 parts of modified polyester polyol, 13-14 parts of toluene diisocyanate, 0.8-0.85 parts of bis(2-morpholine diethyl) ether, 30-35 parts of modified butadiene, 1.1-1.2 parts of p-toluenesulfonyl isocyanate, 1.1-1.2 parts of γ-glycidyl ether oxypropyl trimethoxy silane, 1.1-1.2 parts of antioxidant and 0.25-0.3 parts of defoaming agent;

[0033] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0034] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0035] Preferably, the hydroxyl value of the modified polyester polyol is 50-55 mg KOH / g.

[0036] Preferably, the molecular weight of the maleated polybutadiene is 3300-3500.

[0037] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.2-1.5.

[0038] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.5.

[0039] Preferably, the mass ratio of the modified butadiene to the modified polyester polyol is 1.2.

[0040] A method for preparing electronic adhesive containing modified butadiene comprises the following steps:

[0041] S1: The modified polyester polyol, antioxidant and defoamer are mixed, heated to 70°C, maintained for 4 hours, then heated to 100°C, maintained for 1 hour, and then placed in a vacuum environment of -0.2Mpa for 3 hours;

[0042] S2: At 100°C, add modified butadiene, stir, cool to 70°C, maintain for 1 hour, add toluene diisocyanate, 70°C, maintain for 1 hour, then vacuum for 30 minutes, add bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0043] Preferably, the preparation method of the modified butadiene is: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are added to a reaction kettle in sequence, the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, so as to obtain the modified butadiene.

[0044] Preferably, the preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and they are added to the water-separating condensation flask under the protection of nitrogen, heated to 140°C, and the water-separating condensation flask is used for water separation. The temperature at the opening of the water-separating condensation flask is controlled at 97°C. After 1 hour, the temperature is raised to 160°C and reacted for 10 hours. Based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added, and the temperature is raised to 180°C and reacted for 8 hours to obtain the modified polyester polyol.

[0045] Example 1: The preparation method is:

[0046] S1: 200 g of modified polyester polyol, 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 Mpa for 3 h;

[0047] S2: At 100°C, add 300g of modified butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0048] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0049] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0050] Example 2: The preparation method is:

[0051] S1: 230 g of modified polyester polyol, 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 Mpa for 3 h;

[0052] S2: At 100°C, add 300g of modified butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0053] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0054] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0055] Example 3: The preparation method is:

[0056] S1: 250 g of modified polyester polyol, 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 Mpa for 3 h;

[0057] S2: At 100°C, add 300g of modified butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0058] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0059] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0060] Comparative Example 1: The preparation method is:

[0061] S1: 180 g of modified polyester polyol, 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 Mpa for 3 h;

[0062] S2: At 100°C, add 300g of modified butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0063] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added to the water-separating condensation flask under the protection of nitrogen, and heated to 140° C. The water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97° C. After 1 hour, the temperature is increased to 160° C. for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180° C. for reaction for 8 hours to obtain the modified polyester polyol;

[0064] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0065] Comparative Example 2: The preparation method is:

[0066] S1: 200 g of modified polyester polyol, 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 Mpa for 3 h;

[0067] S2: At 100°C, add 300g of butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0068] The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added into a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, and the suberic acid, 1,4-butanediol and ε-caprolactone are added into the water-separating condensation flask under the protection of nitrogen, and the suberic acid, 1,4-butanediol and ε-caprolactone are added into the water-separating condensation flask, and the suberic acid, 1,4-butanediol and ε-caprolactone are heated to 140°C, and the water-separating condensation flask is used for water separation, and the temperature at the opening of the water-separating condensation flask is controlled at 97°C. After 1 hour, the temperature is increased to 160°C for reaction for 10 hours, and 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, and the temperature is increased to 180°C for reaction for 8 hours to obtain the modified polyester polyol.

[0069] Comparative Example 3: The preparation method is:

[0070] S1: 200 g of di-ester polyol (purchased from Oleon, CAS: 177591-11-6), 11 g of antioxidant (antioxidant: antioxidant 1010) and 2.5 g of defoamer (defoamer: BYK-24043) were mixed, heated to 70°C, maintained for 4 h, then heated to 100°C, maintained for 1 h, and then placed in a vacuum environment of -0.2 MPa for 3 h;

[0071] S2: At 100°C, add 300g of modified butadiene, stir, cool to 70°C, maintain for 1h, add 130g of toluene diisocyanate, 70°C, maintain for 1h, then vacuum for 30 minutes, add 8g of bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add 11g of p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add 11g of γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.

[0072] The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

[0073] Flexibility test Shear strength (Mpa) Dry time min Example 1 3mm 8.0 3-10 Example 2 4mm 7.0 15-20 Example 3 5mm 7.6 15-25 Comparative Example 1 8mm 4.0 30-40 Comparative Example 2 10mm 4.6 30-40 Comparative Example 3 12mm 2.3 30-40

[0074] The present invention adopts a combination of modified polyester polyol and modified butadiene, and coordinates them with other components. In the synthesis, 1,4-butanediol is selected as the polyester polyol to react with suberic acid and epsilon-caprolactone. Because two -OH groups of 1,4-butanediol have a suitable distance, they can cooperate well with suberic acid and epsilon-caprolactone in the synthesis, so that their groups can interact with each other. Suberic acid, 1,4-butanediol and epsilon-caprolactone with a mass ratio of 3.5:1.8:0.9 can make the -OH of the modified polyester polyol have a certain retention. The modified butadiene and the -OH of the modified polyester polyol synergistically act, so that the prepared electronic adhesive has better flexibility, better surface drying time and better shear strength.

[0075] Comparative Example 4: The difference from Example 1 is that the acid value of the modified butadiene is greater than 0.9 mgKOH / g. The flexibility test is 7 mm, the shear strength (Mpa) is 5.0 Mpa, and the surface drying time is 20-25 min.

[0076] By comparing Example 1 and Comparative Example 4, we found that the acid value of modified butadiene affects the flexibility of the electronic adhesive and further affects the surface drying time. The possible reason is that the acid value is too high, the synergistic effect of the modified polyester polyol and the modified butadiene is poor, and the flexibility and surface drying time of the prepared electronic adhesive are worse than those in Example 1.

[0077] Therefore, the combination of modified polyester polyol and modified butadiene is used, and it is matched with other components to prepare an electronic adhesive with good flexibility, good surface drying time, and good shear strength. The surface drying time of the electronic adhesive is within a suitable range, which can improve the production efficiency and the shear strength of the electronic adhesive when the electronic adhesive is used in the production of electronic products, and improve the reliability of the electronic adhesive.

[0078] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. An electronic adhesive containing modified butadiene, characterized in that: According to the mass components, The invention comprises 20-25 parts of modified polyester polyol, 13 parts of toluene diisocyanate, 0.8 parts of bis(2-morpholine diethyl) ether, 30 parts of modified butadiene, 1.1 parts of p-toluenesulfonyl isocyanate, 1.1 parts of γ-glycidyl ether oxypropyl trimethoxy silane, 1.1 parts of antioxidant and 0.25 parts of defoaming agent; The antioxidant is antioxidant 1010, and the defoaming agent is BYK-24043; The preparation method of the modified polyester polyol is as follows: suberic acid, 1,4-butanediol and ε-caprolactone are added to a water-separating condensation flask under the protection of nitrogen, the mass ratio of suberic acid, 1,4-butanediol and ε-caprolactone is 3.5:1.8:0.9, heated to 140°C, the water-separating condensation flask is used for water separation, the temperature at the opening of the water-separating condensation flask is controlled at 97°C, after 1 hour, the temperature is increased to 160°C for reaction for 10 hours, based on the total mass of suberic acid, 1,4-butanediol and ε-caprolactone, 0.0002% of 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorus is added, the temperature is increased to 180°C for reaction for 8 hours, and the modified polyester polyol is obtained; The preparation method of modified butadiene is as follows: maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide are sequentially added into a reaction kettle, wherein the mass ratio of maleic anhydride polybutadiene, phenolic epoxy resin and benzyl triethylbenzene ammonium bromide is 1:9:0.01, and the mixture is heated to 150-160° C., and the acid value is less than or equal to 0.9 mgKOH / g, thereby obtaining the modified butadiene.

2. The electronic adhesive containing modified butadiene according to claim 1, characterized in that: The hydroxyl value of the modified polyester polyol is 50-55 mg KOH / g.

3. The electronic adhesive containing modified butadiene according to claim 1, characterized in that: The molecular weight of the maleic anhydride polybutadiene is 3300-3500.

4. The electronic adhesive containing modified butadiene according to claim 1, characterized in that: The mass ratio of the modified butadiene to the modified polyester polyol is 1.2-1.

5.

5. The electronic adhesive containing modified butadiene according to claim 1, characterized in that: The mass ratio of the modified butadiene to the modified polyester polyol is 1.

5.

6. The electronic adhesive containing modified butadiene according to claim 1, characterized in that: The mass ratio of the modified butadiene to the modified polyester polyol is 1.

2.

7. A method for preparing an electronic adhesive containing modified butadiene according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: The modified polyester polyol, antioxidant and defoamer are mixed, heated to 70°C, maintained for 4 hours, then heated to 100°C, maintained for 1 hour, and then placed in a vacuum environment of -0.2Mpa for 3 hours; S2: At 100°C, add modified butadiene, stir, cool to 70°C, maintain for 1 hour, add toluene diisocyanate, 70°C, maintain for 1 hour, then vacuum for 30 minutes, add bis(2-morpholinediethyl) ether, then vacuum for 30 minutes, add p-toluenesulfonyl isocyanate, then vacuum for 30 minutes, add γ-glycidyloxypropyltrimethoxysilane, and under a nitrogen protective atmosphere, prepare electronic glue.