Low alloy ultra-high strength steel HF1800 and its preparation method

By optimizing the composition and heat treatment process in low alloy ultra-high strength steel, the Nb-rich MC-type carbide and Fe-Ni solid solution was formed, and the problem of insufficient toughness and heat resistance of existing steels when improving yield strength was solved, and the problem of insufficient toughness and heat resistance of existing steels was achieved. Higher strength, toughness and heat resistance to meet the needs of modern industrial equipment.

CN118639139BActive Publication Date: 2024-12-03JIANGSU CHUANGNENG IND EQUIP TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411109784.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing low alloy ultra-high strength steels such as D6AC, D406A, and 30Cr3 are difficult to maintain fracture toughness and plasticity when improving yield strength, and are insufficient heat resistance, which cannot meet the needs of modern industrial equipment for higher strength, toughness and heat resistance. .

Method used

C: 0.30%~0.40%, Si: 1.5%~2.0%, Mn: 0.1%~0.3%, Ni: 3.5%~4.2%, Cr: 0.5%~1.0%, Mo: 0.5%~1.0%, Nb : 0.05% to 0.3% of the component combination, and Nb-rich MC-type carbide and Fe-Ni solid solution are formed through heat treatment to ensure uniform solid solution of alloy elements in the steel matrix, forming a semi-common structure to improve strength and toughness, and through The forging process optimizes the maintenance of material properties.

Benefits of technology

It achieves the improvement of steel yield strength, fracture toughness and heat resistance while ensuring plasticity, meet modern industrial needs, and maintain low production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639139B_ABST
    Figure CN118639139B_ABST
Patent Text Reader

Abstract

The present invention discloses a low alloy ultra-high strength and toughness steel HF1800 and a preparation method thereof, S1, casting raw materials into round ingots, the components and mass percentage contents of the raw materials are: C: 0.30% to 0.40%, Si: 1.5% to 2.0%, Mn: 0.1% to 0.3%, Ni: 3.5% to 4.2%, Cr: 0.5% to 1.0%, Mo: 0.5% to 1.0%, Nb: 0.05% to 0.3%, and the rest are Fe and other inevitable impurity elements; S2, electroslag remelting the round ingot to obtain an electroslag steel ingot; S3, forging into a forging blank; S4, after solution treatment, annealing treatment is performed to obtain low alloy ultra-high strength and toughness steel HF1800. The advantages of the present invention are: through reasonable component design and preparation process, Ni, Si, Mn, especially Cr elements are fully and evenly dissolved in the matrix, the hardness and strength of the matrix are improved, and the fracture toughness and elongation after fracture of the steel can also be guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal materials, and in particular to low-alloy ultra-high strength and toughness steel HF1800 and a preparation method thereof. Background Art

[0002] Low alloy ultra-high strength steel has been the largest ultra-high strength steel used in aerospace, petrochemical, marine equipment and other fields due to its low alloy content, excellent strength and toughness combination, and low production cost. Typical examples include D6AC, D406A, 30Cr3, etc. This type of steel was generally developed and promoted in the 1960s-1980s. Its alloy element content does not exceed 10%, the annealed uniaxial tensile elongation is greater than 15%, the cross-sectional shrinkage is greater than 45%, the yield strength after tempering can reach more than 1400MPa, and the fracture toughness can still reach 80MPa·m 1 / 2 Excellent strengthening and toughness combined with good plasticity and low production and processing costs make low-alloy ultra-high strength and toughness steel the best choice for various load-bearing structural parts.

[0003] However, with the development of various industrial equipment technologies such as aerospace, the original low-alloy ultra-high strength steel can no longer meet the demand. First, the yield strength needs to be further increased to above 1550MPa to achieve a new level of strength leap; second, while the strength is increased, the fracture toughness must still be maintained at 80 MPa·m 1 / 2 , and even further increased to 90MPa·m 1 / 2 ; Third, it should have a certain heat resistance and be able to maintain its performance for a medium to long term within 200°C.

[0004] The traditional D6AC, D406A and 30Cr3 cannot meet the above requirements. This is because D6AC, D406A and 30Cr3 mainly rely on carbon solid solution strengthening or carbide precipitation to improve hardness and strength. However, while improving hardness and strength, they will sacrifice a certain toughness and plasticity, limiting their ability to achieve extremely high strengthening levels.

[0005] Therefore, it is very necessary to develop an ultra-high strength and toughness steel that can further improve its strength, fracture toughness and heat resistance to meet the needs of downstream industries while ensuring plasticity and maintaining a low production cost. Summary of the invention

[0006] The object of the present invention is to provide a low alloy ultra-high strength and toughness steel HF1800 and a preparation method thereof which can further improve its strength, fracture toughness and heat resistance while ensuring plasticity.

[0007] To achieve the above object, the technical solution adopted by the present invention is: low alloy ultra-high strength and toughness steel HF1800, including: raw materials composed of the following components and mass percentages: C: 0.30% to 0.40%, Si: 1.5% to 2.0%, Mn: 0.1% to 0.3%, Ni: 3.5% to 4.2%, Cr: 0.5% to 1.0%, Mo: 0.5% to 1.0%, Nb: 0.05% to 0.3%, and the rest are Fe and other inevitable impurity elements;

[0008] The matrix of the low alloy ultra-high strength and toughness steel HF1800 in the original state is mainly ferrite, and a large amount of Cr carbides are dispersed in the matrix. The tensile properties of the low alloy ultra-high strength and toughness steel HF1800 in the original state are: tensile strength: 1400MPa-1480MPa, yield strength: 800MPa-1100MPa, elongation after fracture: 16%-18%;

[0009] The matrix metallographic structure of the low alloy ultra-high strength and toughness steel HF1800 after quenching and tempering is composed of martensite, carbide and residual austenite, and alloy elements such as Cr, Ni, Si, and Mn are uniformly dissolved in the matrix. The carbide is Nb-rich MC-type carbide, distributed in a nearly spherical shape, and the Nb-rich MC-type carbide wraps the inclusions, so that the size of the inclusions remains at the nanoscale. The Nb-rich MC-type carbide combines with the matrix to form a semi-coherent morphology. The properties of the low alloy ultra-high strength and toughness steel HF1800 in the heat-treated state are: elongation after fracture>20%, cross-sectional shrinkage>45%, yield strength>1550MPa, fracture toughness>90 MPa·m 1 / 2 After being kept at 200℃ for 10h, the yield strength is >1200MPa.

[0010] Furthermore, in the aforementioned low alloy ultra-high strength and toughness steel HF1800, the average particle size of carbides is 200nm to 400nm.

[0011] The preparation method of the low alloy ultra-high strength and toughness steel HF1800 comprises the following steps:

[0012] S1, melting the above raw materials and casting them into ingots with a diameter of 200 mm to 420 mm;

[0013] S2, electroslag remelting the round ingot obtained in S1 at a melting rate of 5.0 kg / min to 8.0 kg / min to obtain an electroslag steel ingot, wherein the diameter of the electroslag steel ingot is 200 mm to 530 mm;

[0014] S3, forging the electroslag steel ingot obtained in S2, and before forging, homogenizing and heating the electroslag steel ingot to 1180° C. to 1220° C., and keeping the temperature for 24 h to 32 h, and cooling after forging to obtain a forging blank;

[0015] S4. The forging blank obtained in S3 is first heated to 930°C to 980°C for solution treatment, and then annealed at a temperature of 680°C to 730°C to obtain low alloy ultra-high strength and toughness steel HF1800.

[0016] Furthermore, in the preparation method of the aforementioned low alloy ultra-high strength and toughness steel HF1800, in which, in S1, vacuum induction melting or electric furnace combined with out-of-furnace refining is selected for melting, and the melting temperature is 1480°C to 1520°C.

[0017] Furthermore, in the aforementioned method for preparing low alloy ultra-high strength and toughness steel HF1800, the homogenization heating temperature of the electroslag ingot in S3 is determined according to the mass percentage of Nb:

[0018] 0.05%≤Nb<0.1%, homogenization heating temperature is 1180℃;

[0019] 0.1%≤Nb<0.15%, homogenization heating temperature is 1190℃;

[0020] 0.15%≤Nb<0.2%, homogenization heating temperature is 1200℃;

[0021] 0.2%≤Nb<0.25%, homogenization heating temperature is 1210℃;

[0022] 0.25%≤Nb≤0.3%, homogenization heating temperature is 1220℃.

[0023] Furthermore, in the preparation method of the aforementioned low-alloy ultra-high strength and toughness steel HF1800, in which, in S3, the initial forging temperature is 1150°C, the final forging temperature is 900°C, and during the forging process, the furnace heating temperature between fires is 30°C lower than the homogenization heating temperature before forging, and the furnace insulation time between fires is 1h to 2h.

[0024] Furthermore, in the preparation method of the aforementioned low-alloy ultra-high strength and toughness steel HF1800, in which, in S3, the octagonal crystal is first broken along the axial direction of the electroslag steel ingot to open the blank, and the first fire forging is carried out: upsetting, drawing, and upsetting to form a square billet, and then the second fire forging is carried out after returning to the furnace for heating and insulation: drawing, upsetting, drawing, and finishing to obtain a round bar forging blank.

[0025] Furthermore, in the aforementioned method for preparing the low alloy ultra-high strength and toughness steel HF1800, in which, in S3, after the forging is completed, the forging blank is first air-cooled to a surface temperature below 500°C, and then buried in sand and cooled to a surface temperature below 200°C before sand removal.

[0026] Furthermore, in the preparation method of the aforementioned low-alloy ultra-high strength and toughness steel HF1800, in S4, a solid solution treatment is first performed: the forging billet is heated to 930°C~980°C at a heating rate of 50°C / h, kept warm for 120min~180min, and then removed from the furnace and water-cooled to below 150°C, and then annealing is performed: the forging billet is heated to 680°C~730°C at a heating rate of 50°C / h, kept warm for 6h, cooled to 400°C with the furnace, and then removed from the furnace and air-cooled, and the time interval between annealing and solid solution removal is no more than 3h.

[0027] The advantages of the present invention are as follows: through reasonable component design and preparation process, the present invention allows Ni, Si, Mn, and especially Cr elements to be fully and evenly dissolved in the matrix, thereby improving the strength of the matrix and ensuring the fracture toughness of the steel. By increasing the content of Ni and Si and reducing the content of Cr, on the one hand, Ni forms a Fe-Ni solid solution in the steel through substitution solid solution, and the residual austenite formed by the Fe-Ni solid solution after quenching ensures that the steel has excellent toughness. On the other hand, Ni inhibits the precipitation of Cr carbides and prevents the Cr carbides from reducing the toughness of the steel after combining with Si. On the other hand, Ni can complement a large amount of Si to promote the formation of a more evenly distributed nano-scale precipitation phase. These precipitation phases have a significant strengthening effect on the material, but because of their small size and even distribution, they will not become the source of stress concentration inside the material, thereby making the steel have good toughness.

[0028] Nb is a very strong carbide-forming element in steel. The formed MC carbide has the highest thermal stability. Nb-rich MC carbide will wrap inclusions. On the one hand, it prevents the inclusions from becoming large in size. On the other hand, the interface structure with the matrix is ​​improved to a semi-coherent structure, so that the fracture toughness of the steel will not decrease after the strength is increased. When homogenizing and heating before forging, heating is required according to the mass percentage of Nb, because the Nb content will affect the phase transformation kinetics and cooling sensitivity of the steel.

[0029] The low alloy ultra-high strength steel HF1800 of the present invention has an elongation after fracture of more than 20%, a cross-sectional shrinkage of more than 45%, a yield strength of more than 1550 MPa, and a fracture toughness of more than 90 MPa·m after heat treatment. 1 / 2 After being kept at 200℃ for 10h, the yield strength is >1200MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a 1000-fold metallographic structure photograph of the original state (solution annealing state) of the low-alloy ultra-high strength and toughness steel HF1800 described in Example 1 of the present invention.

[0031] Figure 2It is the XRD phase analysis spectrum of the low alloy ultra-high strength and toughness steel HF1800 in the original state (solution annealing state) described in Example 1 of the present invention.

[0032] Figure 3 This is a scanning electron microscope photograph of the original state (solution annealing state) of the low-alloy ultra-high strength and toughness steel HF1800 described in Example 1 of the present invention.

[0033] Figure 4 It is a metallographic structure photograph of the low alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 1 of the present invention at 200 times the size.

[0034] Figure 5 It is the XRD phase analysis spectrum of the low alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 1 of the present invention.

[0035] Figure 6 This is a scanning electron microscope photograph of the original state (solution annealing state) of the low-alloy ultra-high strength and toughness steel HF1800 described in Example 1 of the present invention.

[0036] Figure 7 It is a superimposed distribution diagram of alloy elements in the original state (solution annealing state) of the low-alloy ultra-high strength and toughness steel HF1800 described in Example 1 of the present invention in the EDS image.

[0037] Figure 8 It is an element mapping diagram of various alloy elements in the original state (solution annealing state) of the low-alloy ultra-high strength and toughness steel HF1800 described in Example 1 of the present invention in the EDS image.

[0038] Fig. 9 It is a superimposed distribution diagram of alloy elements in the EDS image of the low alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 1 of the present invention.

[0039] Fig.10 It is an element mapping diagram of various alloy elements in the EDS image of the low-alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 1 of the present invention.

[0040] Fig.11 It is a scanning image of Nb-rich MC-type carbides in the low-alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 4 of the present invention.

[0041] Fig.12 This is a composition analysis diagram of Nb-rich MC-type carbides in the low-alloy ultra-high strength and toughness steel HF1800 heat-treated state (900° C. quenching + 250° C. tempering) described in Example 4 of the present invention. DETAILED DESCRIPTION

[0042] The composition and mass percentage of low alloy ultra-high strength and toughness steel HF1800 are: C: 0.30% ~ 0.40%, Si: 1.5% ~ 2.0%, Mn: 0.1% ~ 0.3%, Ni: 3.5% ~ 4.2%, Cr: 0.5% ~ 1.0%, Mo: 0.5% ~ 1.0%, Nb: 0.05% ~ 0.3%, and the rest are Fe and other inevitable impurity elements. After heat treatment, low alloy ultra-high strength and toughness steel HF1800 contains Nb-rich MC-type carbides, which wrap inclusions and prevent them from growing. The precipitation of carbides in low alloy ultra-high strength and toughness steel HF1800 is suppressed, and it is mainly Mo carbides.

[0043] The C element is the element that can most directly improve the strength of steel. The strength of steel can be improved by increasing the C content and then forming carbides through solid solution strengthening. However, the C content should not be too high, otherwise it will lead to a decrease in the toughness of the steel. In this embodiment, the mass percentage of C is controlled at 0.30% to 0.40%. This C content is higher than the C content in traditional D6AC, D406A, and 30Cr3, which can improve the strength and hardness of the low-alloy ultra-high strength and toughness steel HF1800 described in the present invention. In order to prevent the decrease in toughness, it is necessary to add the Ni element.

[0044] Ni is the most important alloying element that improves the strength of steel without reducing its toughness. Ni forms Fe-Ni solid solution in steel by substitution solid solution. Fe-Ni solid solution with a large amount of Ni solid solution forms more residual austenite after quenching, which makes the steel have excellent toughness. Increasing the Ni content can make more Cr be dissolved in austenite, reducing the number of Cr atoms that can be used to form carbides, inhibiting the precipitation of Cr carbides, thereby reducing the formation of hardening phases and further maintaining the toughness of steel. In this embodiment, the mass percentage content of Ni is controlled at 3.5% to 4.2%, which can not only better inhibit the precipitation of Cr carbides, but also ensure the stability of austenite. It can not only make up for the toughness of steel reduced due to increased C content, but also improve the toughness of steel.

[0045] Si plays many roles in alloy steel. On the one hand, increasing the Si content can improve the strength of steel through solid solution strengthening; on the other hand, it can also improve the tempering resistance of steel structure by increasing the Si content, so that the steel has better thermal stability. However, in steel mainly composed of Cr carbides, too high Si content will lead to a significant decrease in the plasticity and toughness of the steel, so in traditional steel, Si should not exceed 1.0%. However, in this embodiment, by greatly increasing the Ni content, the precipitation of Cr carbides is reduced, and the combination between Si and Cr carbides can be reduced. In addition, in a high Ni environment, increasing the Si content can promote the formation of more uniformly distributed nano-scale precipitation phases. These precipitation phases have a significant strengthening effect on the material, but because of their small size and uniform distribution, they will not become the source of stress concentration inside the material, thereby maintaining good toughness. In this embodiment, the mass percentage content of Si is controlled at 1.5% to 2.0%, which can improve the strength of the steel while also improving the combination with Ni, and promote the formation of more uniformly distributed nano-scale precipitation phases.

[0046] Mn is a common alloy element for improving the hardenability of steel, but it has a slight effect on the toughness of steel. In the present invention, the content of Ni and Si is relatively high, and the hardenability of steel is guaranteed. In this embodiment, the mass percentage content of Mn is controlled at 0.1% to 0.3%.

[0047] Cr is an important carbide-forming element in steel. It is the main source of M element in M23C6 type carbide. Studies have shown that if medium-high carbon steel is to be strengthened by Si element, the Cr element needs to be controlled at a low level to inhibit the precipitation of Cr carbides to avoid a significant reduction in the toughness of the steel. In this embodiment, the mass percentage content of the Cr element is controlled at 0.5% to 1.0%.

[0048] Mo is a strong carbide-forming element in steel and is the main source of M in M2C carbides. Appropriate addition of Mo can, on the one hand, preferentially fix a large number of C atoms and reduce the precipitation of Cr carbides. On the other hand, Mo-rich carbides have better thermal stability and can improve the heat resistance of steel. In this embodiment, the mass percentage content of Mo is controlled at 0.5% to 1.0%.

[0049] Nb is a very strong carbide-forming element in steel, and the formed MC-type carbide has the highest thermal stability; at the same time, even a trace amount of Nb element dissolved in the steel matrix can play a strong role in refining austenite grains, thereby improving the strength and toughness of the steel. In this embodiment, the mass percentage content of Nb element is controlled at 0.05% to 0.3%.

[0050] By optimizing the ratio of Ni, Si and Mn components, increasing the content of Si and Ni elements and reducing the content of Cr elements, the Cr elements are fully and evenly dissolved in the matrix, which improves the strength of the matrix and ensures the fracture toughness of the steel. At the same time, the precipitation of high Cr carbides is very small, mainly evenly distributed and fine Mo-rich M2C carbides and Nb-rich MC carbides. The size of these two carbides is between 0.3μm and 2μm, which has a better strengthening effect on steel than high Cr carbides. More importantly, Nb-rich MC carbides will wrap inclusions, which prevent inclusions from becoming large in size on the one hand, and improve the interface structure with the matrix to a semi-coherent structure on the other hand, so that the toughness of the steel will not decrease after the strength is increased.

[0051] The preparation method of the low alloy ultra-high strength and toughness steel HF1800 comprises the following steps:

[0052] S1. After the raw materials are melted, they are cast into ingots with a diameter of 200 mm to 500 mm. The composition and mass percentage of the raw materials are as follows: C: 0.30% to 0.40%, Si: 1.5% to 2.0%, Mn: 0.1% to 0.3%, Ni: 3.5% to 4.2%, Cr: 0.5% to 1.0%, Mo: 0.5% to 1.0%, Nb: 0.05% to 0.3%, and the rest are Fe and other inevitable impurity elements; in this step, vacuum induction melting method or electric furnace combined with refining outside the furnace is used for melting, and the melting temperature is 1480°C to 1520°C;

[0053] S2, electroslag remelting the round ingot obtained in S1 at a melting rate of 5.0 kg / min to 8.0 kg / min to obtain an electroslag steel ingot, wherein the diameter of the electroslag steel ingot is 200 mm to 420 mm;

[0054] S3, forging the electroslag steel ingot obtained in S2, homogenizing and heating the electroslag steel ingot to 1180℃~1220℃ before forging, and keeping it warm for 24h~32h before forging into a billet, the initial forging temperature is 1150℃, and the final forging temperature is 900℃. During the forging process, the billet is firstly opened by smacking the octagonal crystal along the axis direction of the electroslag steel ingot, and the first fire forging is carried out: upsetting, drawing, upsetting to form a square billet, and then the billet is returned to the furnace for heating and keeping warm, and the second fire forging is carried out: drawing, upsetting, drawing, and finishing to obtain a round bar forging billet, the heating temperature of the return furnace between fires is 30℃ lower than the homogenization heating temperature before forging, and the return furnace keeping warm time between fires is 1h~2h. After the forging billet is forged, it is first air-cooled to a surface temperature below 500℃, and then buried in sand and cooled to a surface temperature below 200℃ before sanding;

[0055] In this step, the homogenization heating temperature of the electroslag ingot is determined according to the mass percentage of Nb: 0.05%≤Nb<0.1%, the homogenization heating temperature is 1180℃; 0.1%≤Nb<0.15%, the homogenization heating temperature is 1190℃; 0.15%≤Nb<0.2%, the homogenization heating temperature is 1200℃; 0.2%≤Nb<0.25%, the homogenization heating temperature is 1210℃; 0.25%≤Nb≤0.3%, the homogenization heating temperature is 1220℃.

[0056] S4. The forging billet obtained in S3 is first subjected to solid solution treatment: the forging billet is heated to 930℃~980℃ at a heating rate of 50℃ / h, kept warm for 120min~180min, cooled in water to below 150℃ and then discharged from the water, and then annealed: the forging billet is heated to 680℃~730℃ at a heating rate of 50℃ / h, kept warm for 6h, cooled to 400℃ with the furnace and then discharged from the furnace and air-cooled to obtain low alloy ultra-high strength and toughness steel HF1800. The time interval between annealing and solid solution treatment shall not exceed 3h. Example 1

[0057] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.08%, and smelted in a 1.5t vacuum induction furnace with a smelting temperature set at 1500°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0058] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0059] The electroslag ingot is heated to 1180°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0060] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1150℃ and kept warm for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0061] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to a surface temperature of about 200°C or less before sand removal.

[0062] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 150 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800. Example 2

[0063] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.16%, and smelted in a 1.5t vacuum induction furnace with the smelting temperature set at 1510°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0064] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0065] The electroslag ingot is heated to 1200°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0066] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1170℃ for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0067] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to a surface temperature of about 200°C or less before sand removal.

[0068] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 150 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800. Example 3

[0069] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.08%, and smelted in a 1.5t vacuum induction furnace with a smelting temperature set at 1500°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0070] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0071] The electroslag ingot is heated to 1180°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0072] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1150℃ and kept warm for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 170mm is obtained.

[0073] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to a surface temperature of about 200°C or less before sand removal.

[0074] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 120 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800. Example 4

[0075] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.08%, and smelted in a 10t electric furnace with the smelting temperature set at 1520°C. After smelting in an electric furnace → refining outside the furnace, they were cast into three round ingots with a diameter of 420mm. The round ingots were polished and used as raw materials for electroslag remelting.

[0076] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 530mm. The stable melting rate was set to 8.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 1300mm and a weight of 2.4t was obtained.

[0077] The electroslag ingot was heated to 1180°C and kept at this temperature for 32 hours. It was then cooled to 1150°C in the heating furnace and kept at this temperature for 1.5 hours before being taken out of the furnace for forging.

[0078] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of 590mm and a height of about 700mm. After being returned to the furnace and heated to 1150℃ and kept warm for 2h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 280mm is obtained.

[0079] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to below 200°C before sand removal.

[0080] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 180 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800.

[0081] Table 1 Tensile properties test of original state (solution annealing state) of Examples 1-4

[0082] . Comparative Example 1

[0083] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.16%, and smelted in a 1.5t vacuum induction furnace with the smelting temperature set at 1510°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0084] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0085] The electroslag ingot is heated to 1180°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0086] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1170℃ for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0087] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to below 200°C before sand removal.

[0088] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 150 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800.

[0089] In Comparative Example 1, the mass percentage content of Nb is 0.16%. According to actual production requirements, the homogenization heating temperature before forging should be 1200°C. However, in this comparative example, the homogenization heating temperature before forging is 1180°C. Comparative Example 2

[0090] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3.8%, Cr: 1.5%, Mo: 0.8%, and Nb: 0.08%, and smelted in a 1.5t vacuum induction furnace with the smelting temperature set at 1510°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0091] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0092] The electroslag ingot is heated to 1180°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0093] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1170℃ for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0094] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to below 200°C before sand removal.

[0095] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 150 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800.

[0096] In Comparative Example 2, the mass percentage content of Cr is 1.5%, which exceeds the range of Cr required in the present invention. Comparative Example 3

[0097] The raw materials were prepared according to the mass percentage of C: 0.35%, Si: 1.8%, Mn: 0.2%, Ni: 3%, Cr: 0.8%, Mo: 0.8%, and Nb: 0.08%, and smelted in a 1.5t vacuum induction furnace with the smelting temperature set at 1510°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0098] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0099] The electroslag ingot is heated to 1180°C and kept at this temperature for 24 hours. It is then cooled to 1150°C in the heating furnace and kept at this temperature for 1 hour before being taken out of the furnace and forging begins.

[0100] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1170℃ for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0101] After the round bar forging billet is air-cooled to a surface temperature of about 500°C, it is transferred to sand burying and cooled to below 200°C before sand removal.

[0102] The round bar forgings are subjected to solution treatment and annealing treatment. During solution treatment, the cooled round bar forgings are heated to 950°C at a heating rate of 50°C / h and kept at this temperature for 150 minutes, then taken out of the furnace and water-cooled to below 150°C before being discharged from the water. Annealing treatment is then carried out, and the time interval between annealing and solution treatment does not exceed 3 hours. During annealing treatment, the round bar forgings are heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, then cooled to 400°C with the furnace and taken out of the furnace for air cooling to obtain low alloy ultra-high strength and toughness steel HF1800.

[0103] In Comparative Example 3, the mass percentage content of Ni is 3%, which is smaller than the range of Ni specified in the present invention. Comparative Example 4

[0104] The raw materials were prepared according to the mass percentage of C: 0.30%, Si: 1.1%, Mn: 0.7%, Ni: 1.0%, Cr: 3.0%, Mo: 0.7%, V: 0.1%, and smelted in a 1.5t vacuum induction furnace with a smelting temperature set at 1500°C. After smelting → refining, they were cast into round ingots with a diameter of 300mm, which were polished and used as raw materials for electroslag remelting.

[0105] A 3t protective atmosphere electroslag remelting furnace was used to remelt a steel ingot with a diameter of 420mm. The stable melting rate was set at 6.0kg / min. After cutting off the bottom plate and the necking, an electroslag steel ingot with a height of about 960mm and a weight of 1.05t was obtained.

[0106] The electroslag ingot is heated to 1150°C and kept at this temperature for 24 hours before being taken out of the furnace and forging begins.

[0107] In the forging process, the octagonal crystals are first beaten along the axis of the electroslag steel ingot to form a billet, and then upsetting and drawing are carried out. The first fire is upsetting → drawing → upsetting to a square billet with a cross-sectional side length of about 450mm and a height of about 500mm. After being returned to the furnace and heated to 1170℃ for 1.5h, the second fire forging is carried out, and after drawing → upsetting → drawing → finishing, a round bar forging billet with an average cross-sectional diameter of about 220mm is obtained.

[0108] The round bar forging billet is air cooled to room temperature.

[0109] The round bar forging blank is annealed. The round bar forging blank is heated to 700°C at a heating rate of 50°C / h, and kept at this temperature for 6 hours, and then cooled to 400°C in the furnace and air-cooled to obtain a 30Cr3 steel bar.

[0110] Comparative Example 4 is 30Cr3 which is currently widely used in the market. In Comparative Example 4, the V element replaces the Nb element specified in the present invention.

[0111] Performance Testing

[0112] After heat treatment of Examples 1 to 4 and Comparative Examples 1 to 3 using a heat treatment system of 900°C quenching + 250°C tempering, and heat treatment of Comparative Example 4 using a heat treatment system of 880°C quenching + 220°C tempering, the room temperature tensile properties of the steels of Examples 1 to 4 and Comparative Examples 1 to 4 were tested in accordance with Part 1: Room Temperature Test Method of GB / T228-2010 "Tensile Test of Metallic Materials" (since Comparative Example 4 is a steel with a different composition from that of Examples 1 to 4 and Comparative Examples 1 to 3, and Comparative Example 4 is a commonly used steel on the market, its commonly used heat treatment system is 880°C quenching + 220°C tempering).

[0113] Table 2 Comparison of room temperature mechanical properties test

[0114] serial number Heat treatment system Tensile strength (MPa) Yield strength (MPa) Elongation after break (%) Sectional shrinkage (%) Example 1 900℃ quenching + 250℃ tempering 1920 1580 20.2 48.8 Example 2 900℃ quenching + 250℃ tempering 1933 1591 22.1 49.3 Example 3 900℃ quenching + 250℃ tempering 1947 1563 20.4 50.2 Example 4 900℃ quenching + 250℃ tempering 1934 1574 21.7 47.0 Comparative Example 1 900℃ quenching + 250℃ tempering 1942 1568 15.3 38.3 Comparative Example 2 900℃ quenching + 250℃ tempering 1972 1595 13.1 33.9 Comparative Example 3 900℃ quenching + 250℃ tempering 1822 1484 21.3 42.3 Comparative Example 4 880℃ quenching + 220℃ tempering 1710 1413 16.0 49.2

[0115] As can be seen from Table 2, after heat treatment, the elongation and area reduction performance of Comparative Examples 1 and 2 are significantly reduced to varying degrees compared with Examples 1-4. Comparative Example 1 uses a high Nb content but a low pre-forging heating temperature. When the Nb content is high and the pre-forging heating temperature does not match the Nb content, the coarse Nb-rich primary carbides produced during the smelting process cannot be fully decomposed, causing the coarse Nb-rich primary carbides to be dissolved into the matrix. On the one hand, the effect of Nb on the grain refinement of austenite is limited, thereby affecting the strength and toughness of the steel. On the other hand, the incompletely dissolved coarse carbides will cause the toughness of the steel to drop sharply. Comparative Example 2 uses a higher Cr content than the range specified in the present invention. Too high a Cr content will affect the form of various carbides in the steel, resulting in high Cr M 23 C 6 The precipitation and existence of type carbides will affect the plasticity and toughness of steel.

[0116] Compared with Examples 1-4, the tensile strength and yield strength of Comparative Example 3 are significantly reduced. Comparative Example 3 uses a lower Ni content than the range specified in the present invention. Ni is the most important alloy element that improves the strength of steel without reducing the toughness of steel. Ni forms Fe-Ni solid solution in steel by substitution solid solution. Fe-Ni solid solution with a large amount of Ni solid solution forms more residual austenite after quenching, which makes the steel have excellent toughness. Increasing the Ni content can make more Cr be dissolved in austenite, reducing the number of Cr atoms that can be used to form carbides, inhibiting the precipitation of Cr carbides, thereby reducing the formation of hardening phases, and further maintaining the toughness of steel. When the Ni content is reduced, more residual austenite cannot be formed and the precipitation of Cr carbides cannot be inhibited, thereby reducing the tensile strength and yield strength of steel. Comparative Example 4 is 30Cr3, which is the most representative ultra-high strength steel on the market. Its tensile strength and yield strength are significantly lower than those of Examples 1-4. The V element is a very important carbide-forming element. The V element is generally added to the previous generation of low-alloy ultra-high-toughness steels represented by 30Cr3 in Comparative Example 4 as a means to improve the strength of the steel. However, studies have found that the VC formed by the V element is a non-coherent interface with the matrix, and the V element is more likely to form VN and other inclusions with sharp corners, which greatly reduces the toughness of the steel. Therefore, in order to ensure the toughness of the steel, the amount of V element added is not high, which limits its effect on improving the strength of the steel. By using Nb element instead of V element, through reasonable metallurgical and forging process design, Nb can play an important role in solid solution strengthening and second phase strengthening of steel by solid solution and formation of tiny special Nb-rich MC-type carbides. When added in trace amounts, the strength of the steel can be greatly improved while ensuring the toughness of the steel.

[0117] In Comparative Example 4, the Nb element was replaced by the V element. The ability of the V element to promote grain refinement is weaker than that of the Nb element. The carbides formed by the Nb element in the steel have a smaller size and higher thermal stability. These nano-scale Nb carbides can effectively pin dislocations and improve the precipitation strengthening effect of the steel. However, the carbides of the V element have no significant pinning effect on dislocations and have a weaker precipitation strengthening effect.

[0118] The comparison results of room temperature mechanical properties test show that the low alloy ultra-high strength and toughness steel HF1800 described in the present invention can only obtain excellent mechanical properties under the design of a reasonable composition ratio range and a matching preparation process, and its performance is significantly ahead of 30Cr3.

[0119] After heat treatment of Examples 1 to 4 using a heat treatment system of 900°C quenching + 250°C tempering and heat treatment of Comparative Example 4 using a heat treatment system of 880°C quenching + 220°C tempering, the room temperature tensile properties of the steels of Examples 1 to 4 and Comparative Example 4 after being kept at 200°C for 10 hours were tested in accordance with Part 1: Room Temperature Test Method of GB / T228-2010 "Tensile Test of Metallic Materials" (since Comparative Example 4 is a steel with a different composition from that of Examples 1 to 4, and Comparative Example 4 is a commonly used steel on the market, its commonly used heat treatment system is 880°C quenching + 220°C tempering).

[0120] Table 3 Comparison of mechanical properties at room temperature after 10h insulation at 200℃

[0121] serial number Heat treatment system Tensile strength (MPa) Yield strength (MPa) Elongation after break (%) Sectional shrinkage (%) Example 1 900℃ quenching + 250℃ tempering 1471 1243 14.6 45.1 Example 2 900℃ quenching + 250℃ tempering 1458 1212 13.7 43.1 Example 3 900℃ quenching + 250℃ tempering 1490 1258 14.9 44.0 Example 4 900℃ quenching + 250℃ tempering 1488 1245 15.1 42.7 Comparative Example 4 880℃ quenching + 220℃ tempering 1262 1013 15.3 44.2

[0122] It can be seen from Table 3 that after heat treatment and long-term heat preservation at 200°C, the tensile strength of Examples 1-4 is greater than 1400MPa and the yield strength is greater than 1200MPa. Comparative Examples 1-3 are not prepared under the composition ratio range and the preparation process matched with the present invention, and their mechanical properties at room temperature are relatively poor, so they are not included in this comparison. After long-term heat preservation at 200°C, the tensile strength of 30Cr3 in Comparative Example 4 significantly decreases to below 1300MPa and the yield strength significantly decreases to below 1100MPa. The test results show that the low-alloy ultra-high strength and toughness steel HF1800 described in the present invention has better high-temperature stability.

[0123] After heat treatment of Examples 1 to 4 and Comparative Examples 1 to 3 using a heat treatment system of 900°C quenching + 250°C tempering, and heat treatment of Comparative Example 4 using a heat treatment system of 880°C quenching + 220°C tempering, the fracture toughness of the steels of Examples 1 to 4 and Comparative Examples 1 to 4 was tested in accordance with GB / T21143-2014 "Uniform Test Method for Quasi-static Fracture Toughness of Metallic Materials" (since Comparative Example 4 is a steel with a different composition from that of Examples 1 to 4 and Comparative Examples 1 to 3, and Comparative Example 4 is a commonly used steel on the market, its commonly used heat treatment system is 880°C quenching + 220°C tempering).

[0124] Table 4 Fracture toughness performance test comparison

[0125] ,

[0126] It can be seen from Table 4 that the fracture toughness KIC of Examples 1-4 after heat treatment exceeds 90 MPa·m 1 / 2 .

[0127] The fracture toughness of comparative example 1 after heat treatment is only 43 MPa·m 1 / 2 , indicating that the mismatch between the Nb content and the pre-forging heating temperature affects the microstructure and phase transformation process of the steel, resulting in a significant decrease in the fracture toughness of the steel. In Comparative Example 2, the Cr content exceeding the specified range of the present invention is used, which will make the grains too fine, and after heat treatment, the fracture toughness of the steel will drop to 77 MPa·m 1 / 2 Although the fracture toughness of comparative example 3 after heat treatment reaches 90 MPa·m 1 / 2 However, as shown in Table 2, the strength of Comparative Example 3 is insufficient due to the low Ni content. The fracture toughness of 30Cr3 in Comparative Example 4 after heat treatment is 83 MPa·m 1 / 2 It is much lower than that of Examples 1 to 4. The fracture toughness test results show that the composition range and corresponding preparation process of the low alloy ultra-high strength and toughness steel HF1800 described in the present invention are necessary conditions for achieving the required fracture toughness performance.

[0128] Figure 1 The metallographic structure is 1000 times that of the original state (solution annealing state) of Example 1 of the present invention. The metallographic structure photo shows that the structure of the material is fine and uniform. After high-temperature annealing, the supersaturated martensite structure formed by solid solution has been fully decomposed, and a large number of precipitated carbides are dispersed in the matrix. The distribution of carbides does not show the characteristics of precipitation along the original austenite grain boundaries. Figure 2 This is the XRD phase analysis of the original state (solution annealing state) of Example 1 of the present invention. The results show that the matrix structure is ferrite and the residual austenite content is extremely low. Due to the extremely low content of residual austenite, the residual austenite cannot be displayed during the XRD phase analysis. Figure 3 This is a scanning electron microscope photograph of the original state (solution annealing state) of Example 1 of the present invention. The scanning electron microscope photograph shows that the average size of the carbide particles formed by high temperature annealing is about 200nm-400nm.

[0129] Figure 4 The metallographic structure is 200 times that of the heat-treated state (900°C quenching + 250°C tempering) of Example 1 of the present invention. The metallographic structure photo shows that the heat-treated state of HF1800 consists of lath-shaped tempered martensite, carbides and residual austenite. Compared with the original state, the amount of carbides is greatly reduced. Figure 5 This is the XRD phase analysis of the heat-treated state of Example 1 of the present invention. The spectrum analysis shows that the vast majority of the phase composition of the steel is body-centered cubic martensite, and the residual austenite content is relatively low, only 1.76%, indicating that the hardenability of the steel is good. Figure 6This is a scanning electron microscope photo of the heat-treated state of Example 1 of the present invention. Compared with the original state, the amount of carbides in the heat-treated state is sharply reduced, and the spheroidization morphology is very obvious, indicating that through the implementation of the quenching process, the carbides precipitated by high-temperature annealing have been fully dissolved back into the matrix. The average size of the carbides in the heat-treated state is about 200nm-400nm.

[0130] Figure 7 and Figure 8 Combined together is the EDS surface analysis diagram of the alloy element distribution of the low alloy ultra-high strength and toughness steel HF1800 in the original state (solution annealing state) described in Example 1 of the present invention. Fig. 9 and Fig.10 Combined with this is the EDS surface analysis diagram of the alloy element distribution of the low alloy ultra-high strength steel HF1800 heat-treated state (900°C quenching + 250°C tempering) described in Example 1 of the present invention. EDS surface analysis shows that most of the carbides in the original state of HF1800 are carbides formed by Cr. Existing studies have shown that the main type of Cr carbides is M 23 C 6 Type. In the heat-treated HF1800, the carbides are mainly formed by Mo, and the Cr element has been evenly dissolved in the matrix through the reasonable composition ratio and process of the present invention, which enhances the strength of the matrix without affecting the toughness of the material. It should be pointed out that due to the close peak values ​​of the component energy spectra of Mo and Nb, and the limitation of the resolution of EDS surface scanning, the overall distribution of the component information of the very low content Nb element cannot be obtained under the surface scanning. In fact, the Mo carbides obtained by EDS surface analysis are mostly Nb-rich MC type carbides in EDS point analysis at a higher resolution multiple.

[0131] Fig.11 and Fig.12 They are respectively the morphology of Nb-rich MC carbides in Example 4 of the present invention and the EDS point scanning component analysis. From the morphological point of view, the Nb-rich MC carbides are mainly distributed in the matrix rather than on the grain boundaries in a nearly spherical form, indicating that these carbides are secondary carbides rather than primary carbides left over from the metallurgical process. The precipitation of MC carbides can not only improve the strength of the steel, but also will not cause the degradation of the grain boundaries and thus affect the toughness of the steel. Compared with the previous generation of alloys such as 30Cr3 that are strengthened by carbonitrides formed by the V element in a non-coherent relationship with the matrix, the Nb-rich MC carbides form a semi-coherent relationship with the matrix, which obviously has a more significant advantage in ensuring the fracture toughness of the steel.

[0132] EDS point scanning composition analysis shows that inclusions formed by elements such as oxygen and titanium are encapsulated in Nb-rich MC carbides. Inclusions in steel can easily grow into micron-sized impurity phases, thereby severely degrading the performance of the steel. The present invention forms this new type of Nb-rich MC carbide in steel through optimized component configuration and reasonable process design, which encapsulates inclusions so that their size can only remain at the nanoscale, and at the same time improves the interface structure to a semi-coherent form, so that it cannot affect the toughness and other properties of the steel. The new type of Nb-rich MC carbide encapsulating inclusions plays a very critical role in improving the strength of steel while ensuring the fracture toughness of steel.

[0133] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. Low alloy ultra-high strength steel HF1800, characterized by: It is composed of the following components in mass percentage: C: 0.30% to 0.40%, Si: 1.5% to 2.0%, Mn: 0.1% to 0.3%, Ni: 3.5% to 4.2%, Cr: 0.5% to 1.0%, Mo: 0.5% to 1.0%, Nb: 0.05% to 0.3%, and the rest are Fe and other inevitable impurity elements; The matrix of the low alloy ultra-high strength and toughness steel HF1800 in the original state is mainly ferrite, and a large amount of Cr carbides are dispersed in the matrix. The tensile properties of the low alloy ultra-high strength and toughness steel HF1800 in the original state are: tensile strength: 1400MPa-1480MPa, yield strength: 800MPa-1100MPa, elongation after fracture: 16%-18%; The matrix metallographic structure of the low alloy ultra-high strength and toughness steel HF1800 after quenching and tempering heat treatment consists of martensite, carbide and residual austenite, Cr, Ni, Si, Mn alloy elements are uniformly dissolved in the matrix, the carbide is Nb-rich MC type carbide, distributed in a nearly spherical shape, the Nb-rich MC type carbide wraps the inclusions so that the size of the inclusions remains at the nanoscale, the Nb-rich MC type carbide is combined with the matrix to form a semi-coherent morphology, and the properties of the low alloy ultra-high strength and toughness steel HF1800 in the heat-treated state are: elongation after fracture>20%, section shrinkage>45%, yield strength>1550MPa, fracture toughness>90 MPa·m 1 / 2 After being kept at 200℃ for 10h, the yield strength is >1200MPa.

2. The low alloy ultra-high strength and toughness steel HF1800 according to claim 1 is characterized in that: The average particle size of the carbides is 200nm to 400nm.

3. The method for preparing the low alloy ultra-high strength and toughness steel HF1800 according to any one of claims 1 to 2, characterized in that: Here are the steps: S1, melting the above raw materials and casting them into ingots with a diameter of 200 mm to 420 mm; S2, electroslag remelting the round ingot obtained in S1 at a melting rate of 5.0 kg / min to 8.0 kg / min to obtain an electroslag steel ingot, wherein the diameter of the electroslag steel ingot is 200 mm to 530 mm; S3, forging the electroslag steel ingot obtained in S2, and before forging, homogenizing and heating the electroslag steel ingot to 1180° C. to 1220° C., and keeping the temperature for 24 h to 32 h, and cooling after forging to obtain a forging blank; S4. The forging blank obtained in S3 is first heated to 930°C to 980°C for solution treatment, and then annealed at a temperature of 680°C to 730°C to obtain low alloy ultra-high strength and toughness steel HF1800.

4. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: In S1, vacuum induction melting or electric furnace combined with off-furnace refining is used for melting, and the melting temperature is 1480°C to 1520°C.

5. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: The homogenization heating temperature of the electroslag ingot in S3 is determined according to the mass percentage of Nb: 0.05%≤Nb<0.1%, homogenization heating temperature is 1180℃; 0.1%≤Nb<0.15%, homogenization heating temperature is 1190℃; 0.15%≤Nb<0.2%, homogenization heating temperature is 1200℃; 0.2%≤Nb<0.25%, homogenization heating temperature is 1210℃; 0.25%≤Nb≤0.3%, homogenization heating temperature is 1220℃.

6. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: In S3, the initial forging temperature is 1150°C and the final forging temperature is 900°C. During the forging process, the heating temperature between fires is 30°C lower than the homogenization heating temperature before forging, and the holding time between fires is 1h to 2h.

7. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: In S3, the octagonal crystal is firstly crushed along the axis direction of the electroslag steel ingot to form a billet, and the first fire forging is carried out: upsetting, drawing, upsetting to form a square billet, and then the second fire forging is carried out after returning to the furnace for heating and heat preservation: drawing, upsetting, drawing, and finishing to obtain a round bar forging billet.

8. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: In S3, after forging, the forging blank is first air-cooled to a surface temperature below 500°C, and then buried in sand and cooled to a surface temperature below 200°C before sand removal.

9. The method for preparing low alloy ultra-high strength and toughness steel HF1800 according to claim 3, characterized in that: In S4, a solution treatment is first performed: the forging billet is heated to 930°C-980°C at a heating rate of 50°C / h, kept at this temperature for 120min-180min, and then removed from the furnace and water-cooled to below 150°C. Then, an annealing treatment is performed: the forging billet is heated to 680°C-730°C at a heating rate of 50°C / h, kept at this temperature for 6h, and then removed from the furnace and air-cooled after cooling to 400°C. The time interval between annealing and solution cooling is no more than 3h.

Citation Information

Cited By

  • High-hardness impact-resistant ultrahigh-strength low alloy steel and production method thereof

    CN121737595A