Desert sand mixed fiber concrete and preparation method thereof
By using desert sand and fly ash in desert areas, combined with polyethylene fiber and other materials, low-cost and low-carbon desert sand mixed fiber concrete is prepared, which solves the problems of high carbon emissions of traditional concrete and depletion of natural sand resources, and achieves the realization of It is a low-carbon, low-cost concrete alternative with excellent compressive and tensile properties.
Patent Information
- Application Number
- CN202411147091.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Traditional concrete emits high carbon emissions during the production process and the natural sand resources are depleted. It requires a low-carbon and low-cost concrete alternative that can effectively utilize desert sand resources in the northwest desert areas, reduce engineering costs, and ensure compressive strength and resistance. Tensile strength.
Using desert sand, fly ash, polyvinyl alcohol fiber and polyethylene fiber, low-cost and low-carbon desert sand mixed fiber concrete through specific ratios and treatment methods, use fly ash to reduce the amount of cement, and use it to Fiber reinforced materials improve the tensile strength and deformation ability of concrete.
A significant reduction in carbon footprint has been achieved, engineering costs have been reduced, the environment has been protected, and the compressive strength and excellent tensile deformation capacity of concrete have been ensured, and carbon emissions have been reduced by about 33%.
Smart Images

Figure CN118652090B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete preparation, and in particular to a desert sand mixed fiber concrete and a preparation method thereof. Background Art
[0002] At present, the western region is at the peak of urban infrastructure development. Fiber high-performance concrete has been widely used in the repair of existing concrete buildings, crack prevention and anti-seepage of dams and aqueducts, structural seismic resistance of steel-concrete hybrid structures, seismic nodes and seismic dampers, etc. Compared with ordinary concrete, high-performance concrete uses a large amount of cementitious materials and has a higher production cost. The natural sand used in traditional concrete is rock debris formed and accumulated in natural waters such as rivers and lakes. In recent years, the use of concrete has increased, and natural sand resources have been basically exhausted. Moreover, for the desert and sandy areas in the northwest, desert sand resources are very rich. If we can use local materials, use desert sand instead of river sand, and reasonably use cheap local resources to prepare lightweight, environmentally friendly and highly ductile concrete, it will be of great significance to reduce local engineering costs, protect the local environment and reasonably develop and utilize local natural resources.
[0003] In the process of the rapid development of infrastructure, the use of concrete cement and medium sand has increased. The CO2 implied in the carbon footprint of concrete mainly comes from cement. Although the carbon emissions per unit weight of concrete are not high, when multiplied by the huge consumption required for global infrastructure, the total carbon emissions will inevitably increase rapidly. Therefore, it is necessary to study a low-carbon desert sand concrete with a carbon footprint lower than the traditional content, and to ensure that the concrete has sufficient compressive strength, high tensile strength and excellent deformation capacity. Summary of the invention
[0004] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a desert sand mixed fiber concrete and a preparation method thereof. The low-cost and low-carbon desert sand mixed fiber concrete provided by the present invention fully utilizes desert sand resources and a high amount of fly ash to form a new type of low-carbon desert sand concrete with a carbon footprint lower than the traditional content. It can not only reduce the formation of carbon footprint, reduce engineering costs, protect the environment and save resources, but also ensure that the concrete has sufficient compressive strength, high tensile strength and excellent tensile deformation capacity.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A desert sand mixed fiber concrete is composed of the following raw materials in parts by weight:
[0007] 410-460 parts of desert sand, 500-600 parts of cement, 650-750 parts of fly ash, 300-340 parts of water, 9-10 parts of water reducer, 0.5 parts of thickener, 13-19.5 parts of polyvinyl alcohol fiber, 4.85-9.7 parts of polyethylene fiber;
[0008] Among them, the ratio of fly ash content in the total mass of fly ash and cement is 0.55~0.60;
[0009] The total volume content of the polyvinyl alcohol fiber and the polyethylene fiber is 2%, wherein the volume ratio of the polyvinyl alcohol fiber to the polyethylene fiber is 1-1.5:0.5-1.
[0010] In a preferred embodiment of the present invention, the ratio of fly ash content in the total mass of fly ash and cement is 0.55, and the volumetric content ratio of polyvinyl alcohol fiber to polyethylene fiber is 1:1.
[0011] In a preferred embodiment of the present invention, the PVA fiber is treated with surface oiling to facilitate pulling out before fiber breakage. The fiber has a diameter of 36.8 μm, a length of 9 mm, a tensile strength of 1851 MPa, an elastic modulus of 43 GPa, an elongation of 6.6%, and a density of 1.30 g / cm 3 .
[0012] In a preferred embodiment of the present invention, the PE fiber has a diameter of 25 μm, a length of 12 mm, a tensile strength of 2850 MPa, an elastic modulus of 116 GPa, an elongation of 2% to 3%, and a density of 0.97 g / cm 3 .
[0013] In a preferred embodiment of the present invention, the compressive strength of the desert sand hybrid fiber concrete is 22.42 MPa~65.34 MPa, the tensile strength is 3.61 MPa~6.30 MPa, and the tensile strain is 3.69%~7.13%, which fully utilizes the tensile deformation capacity of polyvinyl alcohol fiber and the high strength of polyethylene fiber, so that the desert sand hybrid fiber concrete has both high tensile strength and good tensile deformation resistance.
[0014] In a preferred embodiment of the present invention, the water reducer is a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3.
[0015] In a preferred embodiment of the present invention, the water reducer is a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3.
[0016] In a preferred embodiment of the present invention, the thickener is hydroxypropyl methylcellulose ether.
[0017] In a preferred embodiment of the present invention, the mud content of the desert sand is ≤2.1%, and the particle size is 74 μm~600 μm.
[0018] Another object of the present invention is to provide a method for preparing the low-cost and low-carbon desert sand hybrid fiber concrete as described in any one of the above, comprising the following steps:
[0019] Weigh the following raw materials in parts by weight: 410-460 parts of desert sand, 500-600 parts of cement, 650-750 parts of fly ash, 300-340 parts of water, 9-10 parts of water reducer, 0.5 parts of thickener, 13-19.5 parts of polyvinyl alcohol fiber, and 4.85-9.7 parts of polyethylene fiber;
[0020] 2 / 3 of the mass fractions of desert sand, cement and fly ash in the raw materials are mixed with water to obtain a first mixture, and the amount of cement in the concrete is reduced by increasing the amount of fly ash. The 100% desertified desert sand is used to replace the sand in the mechanism, which can not only reduce the formation of carbon footprint, reduce engineering costs, protect the environment and save resources, but also ensure that the concrete has sufficient compressive strength, high tensile strength and excellent deformation capacity;
[0021] Adding the remaining 1 / 3 of desert sand, cement and fly ash to the first mixture, and simultaneously adding a water reducing agent, to obtain a second mixture;
[0022] Then, a thickener is added to the second mixture, the mixture is stirred, and finally polyvinyl alcohol and polyethylene fibers are added and stirred to obtain low-cost and low-carbon desert sand hybrid fiber concrete.
[0023] In a preferred embodiment of the present invention, the obtained desert sand mixed fiber concrete is poured in a mold, demolded after pouring, and then placed in a curing box for curing for 3 to 28 days to obtain desert sand mixed fiber concrete of different ages.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The low-cost and low-carbon desert sand mixed fiber concrete provided by the present invention fully utilizes desert sand resources and a high amount of fly ash to form a new type of low-carbon desert sand concrete with a carbon footprint lower than the traditional content. The carbon footprint content of traditional concrete is generally high, mainly because a large amount of carbon dioxide emissions will be generated during the production process of its main component cement. The present invention reduces the amount of cement in the concrete by increasing the amount of fly ash added, and uses 100% desertified desert sand again to replace the sand in the mechanism, which can reduce the formation of carbon footprint, reduce engineering costs, protect the environment and save resources. Under the condition of ensuring that the concrete has sufficient compressive strength, it has higher tensile strength and excellent deformation ability.
[0026] The carbon footprint mainly includes the consumption of fuel oil, gas, cement, water, sand and gravel in production and transportation. First, the present invention uses desert sand to be directly used in the nearest tunnel, which greatly reduces the carbon footprint of sand and gravel such as machine-made sand transported from afar during mining and transportation. Secondly, the cement dosage used in the present invention is relatively small, and more fly ash is used to reuse the waste. Finally, the water-cement ratio of the present invention is relatively low, and the water-cement ratio is the ratio of water to cement + fly ash, which also reduces water consumption and carbon footprint in transportation. The carbon footprint content of traditional concrete is generally high, mainly because the production process of its main ingredient cement will generate a large amount of carbon dioxide emissions. The carbon footprint content of traditional concrete is about 1 ton of carbon dioxide emissions per ton of concrete, while the desert sand mixed fiber concrete prepared in this application contains only about 0.67 tons of carbon dioxide emissions per ton.
[0027] 3. The promotion of low-carbon desert sand concrete prepared by the present invention can not only reduce the formation of carbon footprint, reduce engineering costs, protect the environment and save resources, but also enable the rational development and reuse of environmentally friendly and easily available fly ash and desert sand resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1The present invention is a graph showing the compressive strength of desert sand hybrid fiber concrete of different ages as a function of fiber content, wherein the abscissa represents the ratio of polyvinyl alcohol fiber to polyethylene fiber content, and 1.5%, 0.5%, 1.25%, 0.75%, and 1% represent the volume content of fiber in 1L concrete, respectively. Among them, a-0.60-3d refers to Example 4 to Example 6, in which the ratio of fly ash content to the total mass of fly ash and cement is 0.60, corresponding to an age of 3 days; a-0.60-7d refers to Example 4 to Example 6, in which the ratio of fly ash content to the total mass of fly ash and cement is 0.60, corresponding to an age of 7 days; a-0.60-14d refers to Example 4 to Example 6, in which the ratio of fly ash content to the total mass of fly ash and cement is 0.60, corresponding to an age of 14 days; a- 0.60-28d refers to Example 4 to Example 6, in which the ratio of the fly ash content in the total mass of fly ash and cement is 0.60, corresponding to an age of 28 days; b-0.55-3d refers to Example 1 to Example 3, in which the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 3 days; b-0.55-7d refers to Example 1 to Example 3, in which the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 7 days; b-0.55-14d refers to Example 1 to Example 3, in which the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 14 days; b-0.55-28d refers to Example 1 to Example 3, in which the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 28 days.
[0029] Figure 2It is a curve diagram of the change of tensile strength of desert sand hybrid fiber concrete of different ages prepared by the present invention with fiber content, and the abscissa represents the ratio of polyvinyl alcohol fiber to polyethylene fiber content, wherein a-0.60-3d refers to Example 4 to Example 6-the ratio of fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 3 days; a-0.60-7d refers to Example 4 to Example 6-the ratio of fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 7 days; a-0.60-14d refers to Example 4 to Example 6-the ratio of fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 14 days; a-0.60-28d refers to Example 4 to Example 6-fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of The ratio of the fly ash content in the total mass of fly ash and cement is 0.60, corresponding to an age of 28 days; b-0.55-3d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 3 days; b-0.55-7d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 7 days; b-0.55-14d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 14 days; b-0.55-28d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 28 days.
[0030] Figure 3It is a curve diagram of the change of the ultimate tensile strain of the desert sand hybrid fiber concrete of different ages prepared by the present invention with the fiber content, and the abscissa represents the ratio of the content of polyvinyl alcohol fiber to that of polyethylene fiber, wherein a-0.60-3d refers to Example 4 to Example 6-the ratio of the fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 3 days; a-0.60-7d refers to Example 4 to Example 6-the ratio of the fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 7 days; a-0.60-14d refers to Example 4 to Example 6-the ratio of the fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of 14 days; a-0.60-28d refers to Example 4 to Example 6-fly ash content in the total mass of fly ash and cement is 0.60-corresponding to the age of The ratio of the fly ash content in the total mass of fly ash and cement is 0.60, corresponding to an age of 28 days; b-0.55-3d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 3 days; b-0.55-7d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 7 days; b-0.55-14d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 14 days; b-0.55-28d means that in Example 1 to Example 3, the ratio of the fly ash content in the total mass of fly ash and cement is 0.55, corresponding to an age of 28 days.
[0031] Figure 4 It is the tensile failure form of the desert sand hybrid fiber concrete of the present invention, wherein, a-1 group-28d-63 cracks refers to Example 4-corresponding to the age of 28 days-63 cracks appear on the belly of the tensile specimen after tensile failure; a-2 group-28d-68 cracks refers to Example 5-corresponding to the age of 28 days-68 cracks appear on the belly of the tensile specimen after tensile failure; a-3 group-28d-27 cracks refers to Example 6-corresponding to the age of 28 days-27 cracks appear on the belly of the tensile specimen after tensile failure; b-1 group-3d-80 cracks refers to Example 1-corresponding to the age of 3 days-80 cracks appear on the belly of the tensile specimen after tensile failure; b-1 group-7d-56 cracks The cracks refer to Example 1, which has 56 cracks appearing on the belly of the tensile specimen after being tensilely damaged at the corresponding age of 7 days; b-1 group - 14d-60 cracks refer to Example 1, which has 60 cracks appearing on the belly of the tensile specimen after being tensilely damaged at the corresponding age of 14 days; b-1 group - 28d-53 cracks refer to Example 1, which has 53 cracks appearing on the belly of the tensile specimen after being tensilely damaged at the corresponding age of 28 days; b-2 group - 28d-46 cracks refer to Example 2, which has 46 cracks appearing on the belly of the tensile specimen after being tensilely damaged at the corresponding age of 28 days; b-3 group - 28d-71 cracks refer to Example 3, which has 71 cracks appearing on the belly of the tensile specimen after being tensilely damaged at the corresponding age of 28 days.
[0032] Figure 5 This is a typical 28d tensile strain-stress diagram of Example 5 of the present invention when the fly ash content is 0.60. The five curves represent five different samples, which are tensile samples made by mixing the same proportion. DETAILED DESCRIPTION
[0033] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0035] The cement is P·O42.5 (low alkali) grade ordinary Portland cement produced by Shijiazhuang Jinyu Concrete Co., Ltd., with a density of 3.14 g / cm 3 The test results of cement physical indicators and cement chemical indicators are shown in the table below, both of which meet the requirements of GB 175-2007 "General Portland Cement".
[0036] The fly ash used is Class F Grade I fly ash produced by Shijiazhuang Jinyu Concrete Co., Ltd. The main characteristic parameters of the fly ash are shown in the table below.
[0037] Desert sand was taken from the Tengger Desert, PVA fiber and PE fiber were purchased from Yong'an Baohualin Industrial Development Co., Ltd., and the water reducer was purchased from Shanghai Chenqi Chemical Technology Co., Ltd. The water reducer was a high-efficiency polycarboxylate water reducer and water with a weight ratio of 3:1, and the model of the high-efficiency polycarboxylate water reducer was DH-4005: the thickener was purchased from Jinzhou Fuqiang Fine Chemical Co., Ltd., and the thickener was a thickener (hydroxypropyl methylcellulose ether), and the hydroxypropyl methylcellulose ether was a thickener with a viscosity of 200,000.
[0038] Cement physical index test results
[0039]
[0040] Cement chemical index test results
[0041]
[0042] Main characteristic parameters of fly ash
[0043]
[0044] Example 1
[0045] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0046] Weigh the following raw materials in parts by weight: 570 parts of cement, 684 parts of fly ash, 445 parts of desert sand, 310 parts of water, 9.9 parts of water reducer, 19.5 parts of polyvinyl alcohol fiber, polyvinyl alcohol fiber is referred to as PVA, 4.85 parts of polyethylene fiber, polyethylene fiber is referred to as PE, 0.5 parts of hydroxypropyl methylcellulose ether, the water reducer is a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3, wherein the ratio of fly ash to the total mass of fly ash and cement is 0.55, and the volume ratio of PVA to PE is 1.5%:0.5%.
[0047] Pour 2 / 3 of the raw materials, desert sand, cement and fly ash, into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0048] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0049] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0050] Example 2
[0051] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0052] The following raw materials were weighed in parts by weight: 570 parts of cement, 684 parts of fly ash, 445 parts of desert sand, 310 parts of water, 9.9 parts of water reducer, 16.25 parts of PVA fiber, 7.28 parts of PE fiber, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.55, and the volume ratio of PVA to PE was 1.25%:0.75%.
[0053] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0054] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0055] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0056] Example 3
[0057] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0058] The following raw materials were weighed in parts by weight: 570 parts of cement, 684 parts of fly ash, 445 parts of desert sand, 310 parts of water, 9.9 parts of water reducer, 13 parts of PVA fiber, 9.7 parts of PE fiber, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.55, and the volume ratio of PVA to PE was 1%:1%.
[0059] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0060] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0061] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0062] Example 4
[0063] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0064] The following raw materials were weighed in parts by weight: 500 parts of cement, 750 parts of fly ash, 445 parts of desert sand, 325 parts of water, 9.2 parts of water reducer, 19.5 parts of PVA fiber, 4.85 parts of PE fiber, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.60, and the volume ratio of PVA to PE was 1.5%:0.5%.
[0065] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0066] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0067] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0068] Example 5
[0069] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0070] The following raw materials were weighed in parts by weight: 500 parts of cement, 750 parts of fly ash, 445 parts of desert sand, 325 parts of water, 9.2 parts of water reducer, 16.25 parts of PVA fiber, 7.28 parts of PE fiber, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.60, and the volume ratio of PVA to PE was 1.25%:0.75%.
[0071] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0072] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0073] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0074] Example 6
[0075] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0076] The following raw materials were weighed in parts by weight: 500 parts of cement, 750 parts of fly ash, 445 parts of desert sand, 325 parts of water, 9.2 parts of water reducer, 13 parts of PVA fiber, 9.7 parts of PE fiber, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylate water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.60, and the volume ratio of PVA to PE was 1%:1%.
[0077] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0078] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0079] Add hydroxypropyl methylcellulose ether to the second mixture and stir for 30 seconds. Finally, slowly add PVA fiber and PE fiber and disperse them. The whole process takes about 5 minutes. After the fiber is added, switch to high-speed rotation for 2 minutes to 3 minutes to obtain low-cost and low-carbon desert sand mixed fiber concrete.
[0080] Comparative Example 1
[0081] A method for preparing desert sand mixed fiber concrete comprises the following steps:
[0082] The following raw materials were weighed in parts by weight: 570 parts of cement, 684 parts of fly ash, 445 parts of desert sand, 310 parts of water, 9.9 parts of water reducer, and 0.5 parts of hydroxypropyl methylcellulose ether. The water reducer was a high-efficiency polycarboxylic acid water reducer and water in a weight ratio of 1:3. The ratio of fly ash to the total mass of fly ash and cement was 0.55.
[0083] Pour 2 / 3 of the desert sand, cement and fly ash in the raw materials into a JJ-5 mixing drum, stir for 30 seconds, then add all the water, and stir for another 30 seconds to obtain a first mixture.
[0084] The remaining 1 / 3 of desert sand, cement and fly ash are mixed evenly in a feeding basin and then slowly added to the first mixture obtained in step (2). During this period, water reducing agent is continuously added. The whole process takes about 2 minutes to obtain a second mixture.
[0085] Hydroxypropyl methylcellulose ether was added to the second mixture and stirred for 30 seconds to obtain low-cost and low-carbon desert sand hybrid fiber concrete.
[0086] Comparative Example 2
[0087] The preparation method is the same as that of Example 1, except that: PVA fiber is added in a volumetric dosage of 2%.
[0088] Comparative Example 3
[0089] The preparation method is the same as that of Example 1, except that the ratio of fly ash content in the total mass of fly ash and cement is 0.68.
[0090] Results Analysis
[0091] The present invention has conducted a total of 7 groups of tests. The raw material composition information of Examples 1-6 and Comparative Example 1 is shown in Table 1. The size of the uniaxial compression test piece is 70.7 mm*70.7 mm*70.7 mm, and the uniaxial tensile test piece is a dumbbell-shaped thin plate mold with a size of 330 mm*60 mm*13 mm. The effects of different fly ash content on the compressive strength and tensile properties of desert sand hybrid fiber concrete were studied. The effects of different fiber content on the tensile properties of desert sand hybrid fiber concrete were also explored. In the accompanying drawings and the following description, 0.55 and 0.60 refer to the ratio of fly ash mass to cementitious material. Cementitious material refers to fly ash mass + cement mass. The carbon footprint test method of the present invention is a prior art. For specific test methods, refer to Sun Zhanxing et al., "Research on the Application of Carbon Footprint Difference in Concrete Production".
[0092] The size of the compression test specimen is a cube with a side length of 70.7 mm. The specimens that have reached the predetermined curing age are taken out of the curing box, the surface moisture is wiped off, and the YAW6206 microcomputer-controlled electro-hydraulic servo pressure testing machine is used for the test. The computer controls the continuous uniform load to be applied. The loading rate is 0.5 MPa / s according to the size specified in GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". Three specimens are prepared in each group, and the results are obtained by taking the average value.
[0093] The tensile test specimen is a dumbbell-shaped thin plate. The specimen size is 330×60×13 mm in accordance with JC / T 2461-2018 "Test Method for Mechanical Properties of High Ductility Fiber Reinforced Cement-based Composite Materials". The test was carried out using a WDW-300 microcomputer-controlled electronic universal testing machine. When installing the specimen, eccentric stress conditions should be avoided. The loading speed is 0.15 mm / min. Five specimens are prepared in each group, and the results are averaged.
[0094] Figure 1 The graph of the compressive strength of desert sand hybrid fiber concrete of different ages prepared by the present invention with the change of fiber content shows that the compressive strength of group b is improved by 46%~68%, 38%~57%, 30%~35%, and 18%~23% respectively compared with group a at the corresponding ages of 3d, 7d, 14d, and 28d, and the improvement rate gradually decreases. This is because the activity of cement is higher than that of fly ash in the hydration reaction, which makes the cement hydration reaction cycle shorter than that of fly ash. Therefore, in the early stage of the hydration reaction, fly ash mainly plays the role of filling gaps and hindering the cement hydration reaction, making the compressive strength of group b about 50% higher than that of group a. With the increase of the curing age, the content of cement that has not been hydrated gradually decreases, while the hydration reaction of fly ash gradually accelerates, so that the improvement rate of the compressive strength of group b compared with group a gradually decreases and stabilizes at about 20%. When the age reaches 28 days, the change rate of compressive strength of groups a and b with fiber content is less than 4% and 1%, respectively, and the change range is not large, indicating that the change of fiber content in the later stage has little effect on the compressive strength.
[0095] Figure 2 The graph of the tensile strength of the desert sand mixed fiber concrete of different ages prepared by the present invention with the change of fiber content shows that at 28d in groups a and b, as the proportion of PE fiber content increases, the tensile strength shows a trend of first decreasing and then increasing. This may be due to the fact that when the fiber ratio is PVA:PE=1.5%:0.5%, the proportion of PVA fibers treated with surface oil is relatively large, which not only helps the dispersion of the fibers, but also reduces the chemical bonding between the matrix and the fibers, increases the friction bonding between the matrix and the fibers, and causes more fibers to be pulled out and damaged, consuming more energy. When the fiber ratio is PVA:PE=1.25%:0.75%, although the strain hardening behavior can still be exerted, the bridging ability is smaller than that of the other two groups of fibers, so the tensile strength is smaller. When the fiber ratio is PVA:PE=1%:1%, the number of PE fibers that play a bridging role is relatively large, and because PE fibers mainly play a role through high elastic modulus and tensile strength, the fibers are evenly dispersed by bridging external loads, so their tensile strength is improved.
[0096] When the fiber volume content is not more than 2%, the concrete mixture is not prone to fiber agglomeration and non-dispersion, which makes the PVA fiber well dispersed. The PVA fiber after surface oiling is evenly dispersed and has stronger crack development ability. The concrete is referred to as ECC; the characteristics of strain hardening and multi-crack cracking are controlled by small-size fibers, and the peak tensile strength of the material is determined by large-size fibers. The mixing of multi-size fibers can alleviate the limitations of single-size fibers to a certain extent. The mixing of multiple types of fibers can well improve the mechanical properties of the material. The presence of long fibers in ECC can improve its tensile properties, but long fibers will cause problems such as difficult pumping and easy pipe clogging during injection construction. The ultimate tensile strain of desert sand PVA-ECC with single PVA fiber is less than 3%, which does not meet the ultimate tensile strain condition of ECC; when the relative volume content of PE fiber is 0.5%, the mixed fiber desert sand ECC has excellent mechanical properties and deformation properties. With the increase of the volume content of PE fiber, it has no obvious improvement effect on the mechanical properties and deformation properties of mixed fiber desert sand ECC, and the price of PE fiber is several times that of PVA fiber of the same quality. Mixed fibers are the same type of fibers, but with different fiber sizes, such as length, dendrites or aspect ratio, which can alleviate the limitations of single-size fibers to a certain extent. Among them, the shorter PVA fibers mainly play a role in the initial loading stage, responsible for the generation, development and penetration of microcracks in the initial loading stage, and improve the tensile strength of the material in the early stage. The longer PE fibers mainly play a role in the later stage of loading, bridging the macroscopic wide cracks of the specimen and improving the toughness of the material in the later stage.
[0097] Figure 3 The graph of the change of tensile strain of desert sand hybrid fiber concrete of different ages prepared by the present invention with the fiber content shows that under the same fiber content and age conditions, the tensile strength and tensile strain of group B are higher than those of group A. This is mainly because fly ash plays a lubricating role in the matrix, and the interface bonding ability between the matrix and the fiber is reduced, so that the high strength effect of the fiber cannot be exerted, that is, too high fly ash content will reduce the tensile strength and tensile strain of ECC.
[0098] Table 1 is a table of raw material composition information of Examples 1 to 6 of the present invention and Comparative Example 1, unit: weight parts / g
[0099]
[0100] Table 2 Physical and mechanical properties of PVA and PE fibers
[0101]
[0102] Note: The test standards for PVA fiber and PE fiber are both FZ / T 52023-2012.
[0103] Table 3 Compression and tensile mechanical properties of Examples 1 to 6 and Comparative Example 1
[0104]
[0105] Table 3 shows the compressive and tensile mechanical properties of Examples 1 to 6 of the present invention and Comparative Example 1. From the analysis of compressive strength, when the fly ash content is 0.55, the 28d compressive strength is greater than 60MPa; when the fly ash content is 0.60, the 28d compressive strength is greater than 50MPa, which has good compressive strength. From the results of Examples 1-6 and Comparative Example 1, it can be seen that the later compressive strength of fiber-added concrete is improved compared with that of non-fiber-added concrete, and the proportion of different types of fibers has little effect on the later compressive strength of desert sand mixed fiber concrete. It can be found that the low-cost and low-carbon desert sand mixed fiber concrete of the present invention still has a high compressive strength after using desert sand and a high amount of fly ash.
[0106] From the tensile strength analysis, when the fly ash content is 0.55, the 28d tensile strength is greater than 6.0 MPa, and when the fly ash content is 0.60, the 28d tensile strength is greater than 4.0 MPa. It can be found that the low-cost and low-carbon desert sand hybrid fiber concrete of the present invention has a high tensile strength.
[0107] From the tensile strain analysis, the 28d tensile strain of fly ash with a dosage of 0.60 is greater than 3.5%, while the 28d tensile strain of fly ash with a dosage of 0.55 is as high as over 5.5%, which is about 300-500 times that of ordinary concrete and several times that of ordinary fiber concrete.
[0108] Figure 4 and Figure 5 They are respectively the tensile failure form of the desert sand hybrid fiber concrete of the present invention and the typical 28d tensile strain-stress diagram. Figure 4 , Figure 5 It can be found that the low-cost, low-carbon desert sand hybrid fiber concrete of the present invention has good multi-crack cracking ability and strain relationship, which can greatly prevent the occurrence of concrete damage and block falling due to tension, thereby improving the safety of the structure. In comparative example 2, the ultimate tensile strain of desert sand PVA-ECC with only PVA fiber is less than 3%, which does not meet the ECC ultimate tensile strain condition, and the deformation performance is lower than that of the sample mixed with PVA / PE fiber. In comparative example 3, when the fly ash content is 0.68, its compressive strength, tensile strength and tensile strain are greatly reduced, and the crack control ability is reduced.
[0109] In summary, the low-cost and low-carbon desert sand mixed fiber concrete provided by the present invention fully utilizes desert sand resources and a high amount of fly ash to form a new type of low-carbon desert sand concrete with a carbon footprint lower than the traditional content. The carbon footprint content of traditional concrete is generally high, mainly because a large amount of carbon dioxide emissions will be generated during the production process of its main component cement. The present invention reduces the amount of cement in the concrete by increasing the amount of fly ash added, and uses 100% desertified desert sand to replace the sand in the mechanism. It can not only reduce the formation of carbon footprint, reduce engineering costs, protect the environment and save resources, but also ensure that the concrete has sufficient compressive strength, high tensile strength and excellent deformation capacity.
[0110] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0111] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A desert sand mixed fiber concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 410-460 parts of desert sand, 500-600 parts of cement, 650-750 parts of fly ash, 300-340 parts of water, 9-10 parts of water reducer, 0.5 parts of thickener, 13-19.5 parts of polyvinyl alcohol fiber, 4.85-9.7 parts of polyethylene fiber; Among them, the ratio of fly ash content in the total mass of fly ash and cement is 0.55; The total volume ratio of the polyvinyl alcohol fiber to the polyethylene fiber in the concrete is 2%, wherein the volume ratio of the polyvinyl alcohol fiber to the polyethylene fiber is 1:
1.
2. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The polyvinyl alcohol fiber has an average diameter of 36.8 μm, an average length of 9 mm, a tensile strength of 1851 MPa, an elastic modulus of 43 GPa, an elongation of 6.6%, and a density of 1.30 g / cm 3 .
3. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The polyethylene fiber has an average diameter of 25 μm, an average length of 12 mm, a tensile strength of 2850 MPa, an elastic modulus of 116 GPa, an elongation of 2% to 3%, and a density of 0.97 g / cm 3 .
4. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The desert sand mixed fiber high performance concrete has a compressive strength of 33.27 MPa to 65.34 MPa, a tensile strength of 4.39 MPa to 6.30 MPa, and a tensile strain of 6.78% to 7.13%.
5. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer and water in a weight ratio of 1:
3.
6. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The thickener is hydroxypropyl methylcellulose ether.
7. The desert sand hybrid fiber concrete according to claim 1, characterized in that: The desert sand has a mud content of ≤2.1% and a particle size of 74 μm to 600 μm.
8. A method for preparing desert sand hybrid fiber concrete according to any one of claims 1 to 7, characterized in that: The following steps are involved: Weigh the following raw materials in parts by weight: 410-460 parts of desert sand, 500-600 parts of cement, 650-750 parts of fly ash, 300-340 parts of water, 9-10 parts of water reducer, 0.5 parts of thickener, 13-19.5 parts of polyvinyl alcohol fiber, and 4.85-9.7 parts of polyethylene fiber; Mixing 2 / 3 of the desert sand, cement and fly ash in the raw materials with water to obtain a first mixture; Adding the remaining 1 / 3 of desert sand, cement and fly ash to the first mixture, and simultaneously adding a water reducing agent, to obtain a second mixture; Then, a thickener is added to the second mixture and stirred, and finally polyvinyl alcohol fiber and polyethylene fiber are added and stirred to obtain desert sand hybrid fiber high performance concrete.
9. The method for preparing desert sand hybrid fiber concrete according to claim 8, characterized in that: The obtained desert sand hybrid fiber high performance concrete is poured in a mold, demolded after pouring, and then placed in a curing box for curing for 3 to 28 days to obtain desert sand hybrid fiber high performance concrete of different ages.
Citation Information
Patent Citations
Desert aeolian sand high-ductility cement-based composite material and preparation method thereof
CN114634338A
Ultrahigh-ductility double-doped fiber concrete and preparation method thereof
CN115108785A
3D printing desert sand ultra-high ductility concrete and preparation method thereof
CN115893959A