Environmentally friendly polyurethane adhesive and preparation process thereof
By using renewable raw materials such as castor oil and modified polymerization technology, environmentally friendly polyurethane adhesives with excellent water resistance and bonding strength are prepared, which solves the problems of poor performance and environmental pollution of traditional polyurethane adhesives, and provides More environmentally friendly and economical solutions.
Patent Information
- Application Number
- CN202411153452.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The main raw materials of existing polyurethane adhesives come from non-renewable petroleum resources, resulting in high environmental pollution and economic costs, and their performance such as water resistance, solvent resistance, film strength, etc. are poor.
Renewable raw materials such as castor oil instead of traditional petroleum-based and coal-based raw materials, and by preparing polyurethane prepolymers and chain extenders, combined with hydroxyethyl methacrylate, butyl methacrylate, etc., it is modified to form an environmentally friendly polyurethane adhesive. The mixture improves its water resistance, aging resistance and bonding strength.
It has achieved a reduction in dependence on the environment and fossil resources from the source, significantly improved the water resistance, aging resistance and bonding strength of polyurethane adhesives, providing a more environmentally friendly and economical solution.
Smart Images

Figure CN118652648B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to an environmentally friendly polyurethane adhesive and a preparation process thereof. Background Art
[0002] Waterborne polyurethane is a polymer that can be dispersed in water. It is a polymer material with water as the dispersion medium, which is formed by chain extension of diisocyanate, polymer diol, hydrophilic diol, small molecule diol or diamine. At present, waterborne polyurethane has been widely used in adhesives, coatings, leather finishing agents, fabric treatment agents, etc., among which it is most widely used in the field of adhesives. However, the main raw materials of polyurethane adhesives, isocyanate and polyol, usually come from non-renewable petroleum resources. On the one hand, the use of fossil raw materials such as petroleum-based and coal-based will release a large amount of carbon dioxide and a variety of volatile organic compounds, which will harm the environment and human health; on the other hand, the price of fossil raw materials fluctuates greatly, and it is estimated that oil may be exhausted in the future. Therefore, from the environmental and economic perspectives, the development of renewable raw materials as a green substitute for fossil raw materials has become an urgent problem to be solved.
[0003] Most of the current polyurethane adhesives are linear thermoplastic polyurethanes. Since their coatings are not cross-linked and have low molecular weight, their water resistance, solvent resistance, film strength and other properties are still relatively poor.
[0004] To this end, the present invention discloses an environmentally friendly polyurethane adhesive and a preparation process thereof. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides an environmentally friendly polyurethane adhesive and a preparation process thereof, which adopts renewable raw materials (such as castor oil) to replace traditional petroleum-based, coal-based and other fossil raw materials, thereby reducing environmental pollution and dependence on fossil resources from the source. The prepared environmentally friendly polyurethane adhesive has excellent water resistance, aging resistance and bonding strength.
[0006] The first object of the present application is to provide an environmentally friendly polyurethane adhesive, comprising a component A and a component B, wherein the weight ratio of the component A to the component B is 100:5-8;
[0007] The component A comprises the following raw materials in parts by weight:
[0008] 100 parts of polyurethane prepolymer, 5-6 parts of chain extender, 10-20 parts of hydroxyethyl methacrylate, 5-8 parts of butyl methacrylate, 0.1-0.2 parts of initiator, 40-50 parts of diluent;
[0009] The B component includes the following raw materials in parts by weight:
[0010] 10-20 parts of curing agent, 40-50 parts of diluent, 10-20 parts of leveling agent;
[0011] The preparation process of the chain extender is as follows: dissolving nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, reacting at 35-40° C. under nitrogen protection for 1.5-2 hours, and removing methanol after the reaction to obtain the chain extender.
[0012] In some embodiments, the method for preparing the polyurethane prepolymer comprises the following steps:
[0013] Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain the polyurethane prepolymer.
[0014] In some embodiments, the initiator is potassium persulfate.
[0015] In some embodiments, the curing agent is any one of triethylamine and dimethylethanolamine.
[0016] In some embodiments, the diluent is acetone.
[0017] In some embodiments, the leveling agent is γ-aminopropyltriethoxysilane.
[0018] The second object of the present application is to provide a preparation process of the above-mentioned environmentally friendly polyurethane adhesive, comprising the following steps:
[0019] S1. Preparation of polyurethane prepolymer
[0020] Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain a polyurethane prepolymer;
[0021] S2. Preparation of chain extender
[0022] Dissolve nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, and react at 35-40°C under nitrogen protection for 1.5-2h. After the reaction is completed, remove methanol to obtain a chain extender;
[0023] S3. Preparation of component A
[0024] Prepare materials according to the weight composition of each raw material of component A; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add a diluent and mix thoroughly; then add butyl methacrylate and an initiator for polymerization reaction to obtain component A;
[0025] S4. Preparation of component B
[0026] Prepare materials according to the weight proportion of each raw material in component A; fully mix the curing agent, diluent and leveling agent at room temperature to obtain component B; when using, mix component A and component B in a weight ratio of 100:5-8 to obtain an environmentally friendly polyurethane adhesive.
[0027] In some embodiments, in step S3, the polyurethane prepolymer and the chain extender are reacted at 75-80° C. under nitrogen protection for 2-3 hours.
[0028] In some embodiments, in step S3, the polymerization reaction is carried out at 70-75° C. under nitrogen protection for 2-3 hours.
[0029] In some embodiments, when used, component A and component B are mixed in a weight ratio of 100:5-8 to obtain an environmentally friendly polyurethane adhesive.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The environmentally friendly polyurethane adhesive described in the present application uses renewable raw materials (such as castor oil) instead of traditional petroleum-based, coal-based and other fossil raw materials, thereby reducing environmental pollution and dependence on fossil resources from the source.
[0032] 2. The environmentally friendly polyurethane adhesive prepared in the present application is prepared through the preparation of polyurethane prepolymer, the synthesis of chain extender and subsequent end-capping and polymerization reactions, and is modified by using butyl methacrylate to improve the water resistance, aging resistance and bonding strength of the adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0034] Figure 1 This is a process flow chart of a preparation process of an environmentally friendly polyurethane adhesive described in this application;
[0035] Figure 2 This is the infrared spectrum of the chain extender described in this application. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0037] As used herein, "and / or" includes the term of all combinations of any one or more associated listed items. The terms used herein are only used to describe specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It is further understood that "including", when used in this specification, specifies the stated features, integers, steps, operations, elements and / or compositions, but does not exclude the existence or addition of one or more other features, integers, steps, operations, elements, compositions and / or combinations thereof.
[0038] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It is further understood that terms, such as defined in commonly used dictionaries, are interpreted in accordance with their meanings in the context of the relevant art and are not idealized or overly formal meanings unless explicitly defined as such herein.
[0039] The exemplary invention described herein may appropriately lack any one or more element limitations that are not specifically disclosed herein. Therefore, the terms "comprise", "include", "contain", etc. should be understood broadly and non-restrictively. In addition, the terminology used herein is used as a description, not a limitation, and it is unintentional to use these terminology expressions that do not include any equivalent characteristics, but only describe some of their characteristics, but various modifications are possible within the scope of the present invention according to the rights. Therefore, although the present invention has been specifically disclosed by preferred embodiments and optional features, the modifications disclosed herein to embody the changes of the present invention may be recorded by those skilled in the art, and such modifications and changes will be considered to be within the scope of the present invention.
[0040] An environmentally friendly polyurethane adhesive comprises a component A and a component B, wherein the weight ratio of the component A to the component B is 100:5-8;
[0041] The component A comprises the following raw materials in parts by weight:
[0042] 100 parts of polyurethane prepolymer, 5-6 parts of chain extender, 10-20 parts of hydroxyethyl methacrylate, 5-8 parts of butyl methacrylate, 0.1-0.2 parts of initiator, 40-50 parts of diluent;
[0043] The B component includes the following raw materials in parts by weight:
[0044] 10-20 parts of curing agent, 40-50 parts of diluent, 10-20 parts of leveling agent.
[0045] In some embodiments, the method for preparing the polyurethane prepolymer comprises the following steps:
[0046] Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain the polyurethane prepolymer.
[0047] Specifically, the polyurethane prepolymer is prepared by reacting castor oil, isophorone diisocyanate and polyethylene glycol 600 in specific proportions and under specific conditions. The isocyanate group therein has high reactivity and can react with a variety of active hydrogen-containing compounds to form a cross-linked structure, further constructing a polymer network structure and improving the strength and performance of the adhesive.
[0048] In some embodiments, the preparation method of the chain extender comprises the following steps: adding nadic anhydride and tris(hydroxymethyl)aminomethane to methanol at a molar ratio of 1:1, reacting at 35-40°C under nitrogen protection for 1.5-2h, and removing methanol after the reaction to obtain the chain extender. The chemical reaction process of the chain extender is as follows:
[0049]
[0050] Specifically, the chain extender reacts with the isocyanate group in the polyurethane prepolymer through its functional group to extend the polyurethane molecular chain and form a longer linear or branched structure. In the present invention, the chain extender is prepared by the reaction of nadic anhydride and trishydroxymethylaminomethane, and its functional group can efficiently react with the isocyanate group to achieve the extension of the molecular chain, further improve the molecular weight and crosslinking density of the adhesive, and thus enhance its mechanical properties. In the present application, the weight of the chain extender is 5-6 parts, and can specifically be any value of 5 parts, 6 parts, and 5.5 parts, as long as it meets the requirement of 5-6 parts. Figure 2 As shown, at 1552 cm -1 The absorption peak at 1054 cm corresponds to the formation vibration of NH, indicating the presence of carbamate groups (-NHCOO-) in the chain extender. -1 and 1643 cm -1 The absorption peaks at and belong to the stretching vibrations of the acyclic anhydride and the C=C group, respectively, indicating the presence of the acyclic anhydride and the C=C group in the chain extender. Therefore, it can be explained that the present application can prepare a chain extender having a carbamate group (-NHCOO-) by reacting nadic anhydride and trishydroxymethylaminomethane.
[0051] In the present application, the hydroxyl group of hydroxyethyl methacrylate can react with the isocyanate group to form a stable carbamate bond, thereby avoiding unnecessary reactions between the isocyanate group and water, moisture in the air, etc., which may affect the performance of the adhesive. At the same time, the introduction of hydroxyethyl methacrylate also provides a reaction site for the subsequent polymerization reaction. The weight of hydroxyethyl methacrylate is 10-20 parts, and can be any value of 10 parts, 20 parts, or 15 parts, as long as it meets the requirement of 10-20 parts.
[0052] In some embodiments, the initiator is potassium persulfate. The initiator decomposes at high temperature to produce free radicals, which can attack the double bonds in the monomer molecules and initiate a chain polymerization reaction. In the present application, potassium persulfate is used as an initiator, and the free radicals produced by its decomposition can effectively initiate the polymerization reaction of the monomer. The weight portion of the initiator is 0.1-0.2 parts, specifically any value of 0.1 parts, 0.2 parts, and 0.15 parts, as long as it meets the requirement of 0.1-0.2 parts.
[0053] In some embodiments, the diluent is acetone. The diluent is generally a low-viscosity organic solvent that can dissolve or disperse the polymer components in the adhesive, reduce its viscosity and improve fluidity. In the present invention, acetone is used as a diluent, and its good solubility and volatility can meet the construction requirements and quickly evaporate to form a film.
[0054] In some embodiments, the curing agent is any one of triethylamine and dimethylethanolamine. The curing agent usually contains a group (such as an amine group) that can react with a functional group (such as a hydroxyl group, an amino group, etc.) in a polyurethane prepolymer, and can react quickly with the polyurethane prepolymer after coating to form a strong cross-linked structure. In the present invention, triethylamine or dimethylethanolamine is used as a curing agent, which can react with the isocyanate group in the polyurethane prepolymer to achieve rapid curing. The weight of the curing agent is 10-20 parts, and can specifically be any value of 10 parts, 20 parts, and 11 parts, as long as it meets the requirement of 10-20 parts.
[0055] In some embodiments, the leveling agent is a γ-aminopropyltriethoxysilane leveling agent: the leveling agent usually has a low surface tension, can form a uniform thin film on the surface of the coating, reduce the interfacial tension between the coating and the air or substrate, and enable the coating to automatically level and remove bubbles during the drying process. The leveling agent plays a role in improving the surface flatness of the coating in the adhesive system, making the coating smoother and more uniform, and improving the aesthetics and adhesion. The weight of the leveling agent is 10-20 parts, specifically any value of 10 parts, 20 parts, and 11 parts, as long as it meets the requirement of 10-20 parts.
[0056] Butyl methacrylate has many outstanding advantages such as excellent light resistance and outdoor exposure durability. When polyurethane is modified with butyl methacrylate, the advantages of the two can be complemented. That is, by modifying polyurethane with butyl methacrylate, the low water resistance and low gloss of a single polyurethane film can be improved, while the shortcomings of a single butyl methacrylate such as hot stickiness and cold brittleness and poor solvent resistance can also be improved. In the present application, the weight of butyl methacrylate is 5-8 parts, and can be any value of 5 parts, 6 parts, and 8 parts, as long as it meets the requirements of 5-8 parts.
[0057] like Figure 1 The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0058] S1. Preparation of polyurethane prepolymer
[0059] Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain a polyurethane prepolymer;
[0060] S2. Preparation of chain extender
[0061] Dissolve nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, and react at 35-40°C under nitrogen protection for 1.5-2h. After the reaction is completed, remove methanol to obtain a chain extender;
[0062] S3. Preparation of component A
[0063] Prepare materials according to the weight composition of each raw material of component A; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add a diluent and mix thoroughly; then add butyl methacrylate and an initiator for polymerization reaction to obtain component A;
[0064] S4. Preparation of component B
[0065] The materials are prepared according to the weight proportion of each raw material of component A; the curing agent, the diluent and the leveling agent are fully mixed at room temperature to obtain component B; when in use, the components A and B are mixed according to a weight ratio of 100:5-8 to obtain an environmentally friendly polyurethane adhesive.
[0066] In the following examples, the initiator is potassium persulfate; the diluent is acetone; and the leveling agent is γ-aminopropyltriethoxysilane.
[0067] Embodiment 1: The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0068] S1. Preparation of polyurethane prepolymer
[0069] Castor oil, isophorone diisocyanate and polyethylene glycol 600 were mixed in a molar ratio of 1:1:1, and reacted at 75° C. under nitrogen protection for 4 hours. The reaction was completed to obtain a polyurethane prepolymer;
[0070] S2. Preparation of chain extender
[0071] According to the molar ratio of 1:1, nadic anhydride and tris(hydroxymethyl)aminomethane were dissolved in a methanol solution, and reacted at 35°C under nitrogen protection for 1.5 hours. After the reaction was completed, methanol was removed to obtain a chain extender;
[0072] S3. Preparation of component A
[0073] Prepare the materials according to the weight composition of each raw material of component A, including 100 parts of polyurethane prepolymer, 5 parts of chain extender, 10 parts of hydroxyethyl methacrylate, 5 parts of butyl methacrylate, 0.1 parts of initiator and 40 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add the diluent and mix thoroughly; then add butyl methacrylate and the initiator for polymerization reaction to obtain component A;
[0074] S4. Preparation of component B
[0075] Prepare the materials according to the weight composition of each raw material of component A, including 10 parts of curing agent (triethylamine), 40 parts of diluent, and 10 parts of leveling agent; fully mix the curing agent, diluent, and leveling agent at room temperature to obtain component B.
[0076] An environmentally friendly polyurethane adhesive comprises a component A and a component B. When in use, the weight ratio of the component A to the component B is 100:5.
[0077] Embodiment 2: The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0078] S1. Preparation of polyurethane prepolymer
[0079] Castor oil, isophorone diisocyanate and polyethylene glycol 600 were mixed in a molar ratio of 1:1:1, and reacted at 80° C. under nitrogen protection for 5 hours. The reaction was completed to obtain a polyurethane prepolymer;
[0080] S2. Preparation of chain extender
[0081] According to the molar ratio of 1:1, nadic anhydride and tris(hydroxymethyl)aminomethane were dissolved in a methanol solution, and reacted at 40°C under nitrogen protection for 2 hours. After the reaction, methanol was removed to obtain a chain extender;
[0082] S3. Preparation of component A
[0083] Prepare the materials according to the weight composition of each raw material of component A, including 100 parts of polyurethane prepolymer, 6 parts of chain extender, 20 parts of hydroxyethyl methacrylate, 8 parts of butyl methacrylate, 0.2 parts of initiator and 50 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add the diluent and mix thoroughly; then add butyl methacrylate and the initiator for polymerization reaction to obtain component A;
[0084] S4. Preparation of component B
[0085] Prepare the materials according to the weight proportion of each raw material of component A, including 20 parts of curing agent (triethylamine), 50 parts of diluent, and 20 parts of leveling agent; fully mix the curing agent, diluent, and leveling agent at room temperature to obtain component B.
[0086] An environmentally friendly polyurethane adhesive comprises a component A and a component B. When in use, the weight ratio of the component A to the component B is 100:8.
[0087] Embodiment 3: The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0088] S1. Preparation of polyurethane prepolymer
[0089] Castor oil, isophorone diisocyanate and polyethylene glycol 600 were mixed in a molar ratio of 1:1:1, and reacted at 75° C. under nitrogen protection for 5 hours. The reaction was completed to obtain a polyurethane prepolymer;
[0090] S2. Preparation of chain extender
[0091] Dissolve nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, and react at 35°C under nitrogen protection for 2 hours. After the reaction is completed, remove methanol to obtain a chain extender;
[0092] S3. Preparation of component A
[0093] Prepare the materials according to the weight composition of each raw material of component A, including 100 parts of polyurethane prepolymer, 5 parts of chain extender, 20 parts of hydroxyethyl methacrylate, 5 parts of butyl methacrylate, 0.2 parts of initiator and 40 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add the diluent and mix thoroughly; then add butyl methacrylate and the initiator for polymerization reaction to obtain component A;
[0094] S4. Preparation of component B
[0095] Prepare the materials according to the weight proportion of each raw material of component A, including 10 parts of curing agent (triethylamine), 50 parts of diluent, and 10 parts of leveling agent; fully mix the curing agent, diluent, and leveling agent at room temperature to obtain component B.
[0096] An environmentally friendly polyurethane adhesive comprises a component A and a component B. When in use, the weight ratio of the component A to the component B is 100:6.
[0097] Embodiment 4: The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0098] S1. Preparation of polyurethane prepolymer
[0099] Castor oil, isophorone diisocyanate and polyethylene glycol 600 were mixed in a molar ratio of 1:1:1, and reacted at 77° C. under nitrogen protection for 4.5 hours. The reaction was completed to obtain a polyurethane prepolymer;
[0100] S2. Preparation of chain extender
[0101] According to the molar ratio of 1:1, nadic anhydride and tris(hydroxymethyl)aminomethane were dissolved in a methanol solution, and reacted at 37°C under nitrogen protection for 1.8 hours. After the reaction was completed, methanol was removed to obtain a chain extender;
[0102] S3. Preparation of component A
[0103] Prepare the materials according to the weight composition of each raw material of component A, including 100 parts of polyurethane prepolymer, 5.5 parts of chain extender, 15 parts of hydroxyethyl methacrylate, 7 parts of butyl methacrylate, 0.15 parts of initiator and 45 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add the diluent and mix thoroughly; then add butyl methacrylate and the initiator for polymerization reaction to obtain component A;
[0104] S4. Preparation of component B
[0105] Prepare the materials according to the weight proportion of each raw material of component A, including 15 parts of curing agent (dimethylethanolamine), 45 parts of diluent, and 15 parts of leveling agent; fully mix the curing agent, diluent, and leveling agent at room temperature to obtain component B.
[0106] An environmentally friendly polyurethane adhesive comprises a component A and a component B. When in use, the weight ratio of the component A to the component B is 100:7.
[0107] Embodiment 5: The preparation process of the environmentally friendly polyurethane adhesive comprises the following steps:
[0108] S1. Preparation of polyurethane prepolymer
[0109] Castor oil, isophorone diisocyanate and polyethylene glycol 600 were mixed in a molar ratio of 1:1:1, and reacted at 80° C. under nitrogen protection for 4 hours. The reaction was completed to obtain a polyurethane prepolymer;
[0110] S2. Preparation of chain extender
[0111] According to the molar ratio of 1:1, nadic anhydride and tris(hydroxymethyl)aminomethane were dissolved in a methanol solution, and reacted at 40°C under nitrogen protection for 1.5 hours. After the reaction was completed, methanol was removed to obtain a chain extender;
[0112] S3. Preparation of component A
[0113] Prepare the materials according to the weight composition of each raw material of component A, including 100 parts of polyurethane prepolymer, 6 parts of chain extender, 10 parts of hydroxyethyl methacrylate, 6 parts of butyl methacrylate, 0.2 parts of initiator and 48 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add the diluent and mix thoroughly; then add butyl methacrylate and the initiator for polymerization reaction to obtain component A;
[0114] S4. Preparation of component B
[0115] Prepare the materials according to the weight composition of each raw material of component A, including 17 parts of curing agent (dimethylethanolamine), 48 parts of diluent, and 18 parts of leveling agent; fully mix the curing agent, diluent, and leveling agent at room temperature to obtain component B.
[0116] An environmentally friendly polyurethane adhesive comprises a component A and a component B. When in use, the weight ratio of the component A to the component B is 100:6.
[0117] The environmentally friendly polyurethane adhesives of Examples 1-5 are cured at 60-80° C. for 24-48 hours.
[0118] Comparative Example 1
[0119] A polyurethane adhesive comprises a component A and a component B, a chain extender is 2,2-dihydroxymethyl propionic acid, and other conditions are consistent with those in Example 1.
[0120] Comparative Example 2
[0121] A polyurethane adhesive comprises a component A and a component B.
[0122] During the preparation of component A,
[0123] Prepare the materials according to the weight proportion of each raw material of component A, including 100 parts of polyurethane prepolymer, 5 parts of chain extender, 10 parts of hydroxyethyl methacrylate and 40 parts of diluent; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping, and then add the diluent to obtain component A.
[0124] The remaining conditions are the same as those in Example 1.
[0125] The polyurethane adhesives of Examples 1-5 and Comparative Examples 1-2 were tested according to the following performance items, and the results are summarized in the following Table 1:
[0126] Water resistance test:
[0127] Pour a certain amount of adhesive into the mold, place the mold in a 60℃ oven until the mass no longer changes, and cut a 4cm 2 The adhesive film of different sizes (mass is recorded as m0, at 25°C, is immersed in deionized water for 24 hours, taken out, and the water on the surface of the film is wiped dry with filter paper, and its mass is recorded as m1. The water absorption rate of the adhesive film is calculated by the following formula: Water absorption rate of the adhesive film (%) = (m1-m0) / m0×100%.
[0128] Bond strength test
[0129] Sample preparation method: Apply the adhesive emulsion on an aluminum sheet with a size of 100mm×25mm, with a coating size of approximately 20mm×25mm. After drying naturally in the air for 2 hours, overlap the two aluminum sheets at the emulsion coating position and stick them together. Fix them with clips and put them in an oven at 80°C to dry for 48 hours. Then test the tensile strength in a universal material testing machine and evaluate the bonding strength with the maximum tensile strength.
[0130] The tensile strength is tested under the following aging test, and the tensile strength refers to GB / T 528-2008.
[0131] 1. High and low temperature humidity alternating aging test
[0132] The test was carried out according to the standard methods of GB / T2423.1-2008 and GB / T 2790-1995. The specific test steps are as follows: the test sample at room temperature was placed in a high-low temperature and humidity cycle test chamber under the specified conditions, and placed at 80℃ and 95%RH for 4 hours, then cooled to -40℃ within 2 hours, and then placed at -40℃ for 4 hours, and then heated to 80℃ and 95%RH within 2 hours. The test cycles were 240, 480, 720, and 960 hours respectively.
[0133] 2. UV aging test
[0134] Reference standards ASTMG 154-12a "Operation Standard for Fluorescent UV Exposure Equipment for Nonmetallic Materials" and ASTM G151-10 "Standard Practice for Exposure of Nonmetallic Materials in Accelerated Test Devices Using Laboratory Light Sources", the UV wavelength is 313nm. One cycle is 4 hours under UV conditions and 4 hours under condensation conditions, the temperature is 60°C, and the irradiance is 0.71±0.02W / m 2 / nm, the condensation temperature is 50±3℃, and the test cycles are 240, 480, 720, and 960h.
[0135] Table 1
[0136]
[0137] From Table 1, it can be found that the polyurethane adhesives prepared in Examples 1-5 have a water absorption rate of less than 1%, showing excellent water resistance, and a bonding strength greater than 1500N, showing excellent bonding performance; and in high and low temperature aging tests and UV aging tests, the tensile strength has basically no change (or slightly decreases), showing excellent aging resistance.
[0138] In comparative example 1, the polyurethane adhesive prepared by adding a small molecule chain extender has a certain degree of decline in water absorption, bonding strength and aging tests. This may be related to the fact that the molecular weight of the prepolymer obtained after chain extension with the small molecule chain extender is relatively small.
[0139] In Comparative Example 2, no butyl methacrylate or initiator was added to carry out polymerization reaction, and no butyl methacrylate was used to modify the polyurethane prepolymer, resulting in a significant decrease in the water absorption rate, bonding strength and aging test of the adhesive.
[0140] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. An environmentally friendly polyurethane adhesive, characterized in that: Comprising component A and component B, wherein the weight ratio of component A to component B is 100:5-8; The component A comprises the following raw materials in parts by weight: 100 parts of polyurethane prepolymer, 5-6 parts of chain extender, 10-20 parts of hydroxyethyl methacrylate, 5-8 parts of butyl methacrylate, 0.1-0.2 parts of initiator, 40-50 parts of diluent; The B component includes the following raw materials in parts by weight: 10-20 parts of curing agent, 40-50 parts of diluent, 10-20 parts of leveling agent; The preparation process of the chain extender is as follows: dissolving nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, reacting at 35-40° C. under nitrogen protection for 1.5-2 hours, and removing methanol after the reaction to obtain the chain extender; The preparation method of the polyurethane prepolymer comprises the following steps: Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain the polyurethane prepolymer.
2. The environmentally friendly polyurethane adhesive according to claim 1, characterized in that: The initiator is potassium persulfate.
3. The environmentally friendly polyurethane adhesive according to claim 1, characterized in that: The curing agent is any one of triethylamine and dimethylethanolamine.
4. The environmentally friendly polyurethane adhesive according to claim 1, characterized in that: The diluent is acetone.
5. The environmentally friendly polyurethane adhesive according to claim 1, characterized in that: The leveling agent is γ-aminopropyltriethoxysilane.
6. A process for preparing the environmentally friendly polyurethane adhesive according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of polyurethane prepolymer Castor oil, isophorone diisocyanate and polyethylene glycol 600 are mixed in a molar ratio of 1:1:1, and reacted at 75-80° C. under nitrogen protection for 4-5 hours. The reaction is completed to obtain a polyurethane prepolymer; S2. Preparation of chain extender Dissolve nadic anhydride and tris(hydroxymethyl)aminomethane in a methanol solution at a molar ratio of 1:1, and react at 35-40°C under nitrogen protection for 1.5-2h. After the reaction is completed, remove methanol to obtain a chain extender; S3. Preparation of component A Prepare materials according to the weight composition of each raw material of component A; react the polyurethane prepolymer and the chain extender; after the reaction, add hydroxyethyl methacrylate for end-capping; after the end-capping, add a diluent and mix thoroughly; then add butyl methacrylate and an initiator for polymerization reaction to obtain component A; S4. Preparation of component B Prepare materials according to the weight proportion of each raw material in component A; fully mix the curing agent, diluent and leveling agent at room temperature to obtain component B; when using, mix component A and component B in a weight ratio of 100:5-8 to obtain an environmentally friendly polyurethane adhesive.
7. The preparation process according to claim 6, characterized in that: In step S3, the polyurethane prepolymer and the chain extender are reacted at 75-80° C. under nitrogen protection for 2-3 hours.
8. The preparation process according to claim 6, characterized in that: In step S3, the polymerization reaction is carried out at 70-75° C. under nitrogen protection for 2-3 hours.
9. The preparation process according to claim 6, characterized in that: When in use, component A and component B are mixed in a weight ratio of 100:7 to obtain an environmentally friendly polyurethane adhesive.