A method for preparing long-acting antibacterial cellulose material
By reacting the halogenated vinyl carboxylic acid esters with organic amines on the cellulose material, the problems of poor antibacterial properties and durability and complex preparation of cellulose materials are solved, and low-cost and rapid long-term preparation of antibacterial cellulose materials are achieved. Suitable for multiple application areas.
Patent Information
- Application Number
- CN202411150255.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing cellulose materials lack long-term antibacterial properties, the preparation process is complex and costly, which limits its wide application in the field of antibacterial.
By infiltrating the cellulose material in an alkaline solution and reacting with vinyl halogenated carboxylic acid ester, surface esterified cellulose is formed, and then impregnated in an organic amine solution, the cellulose material is imparted with long-acting antibacterial properties.
This method is simple to operate, low cost, fast reaction, can impart long-term antibacterial properties to cellulose materials at room temperature, and antibacterial groups are not easy to fall off, and is suitable for textile, medical and food packaging fields.
Smart Images

Figure CN118653302B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cellulose modification, and in particular relates to a method for preparing a long-acting antibacterial cellulose material. Background Art
[0002] Cellulose is the most abundant biomass resource in nature. It has the advantages of wide sources, green, non-toxic, renewable, and biodegradable. It is one of the most sustainable natural polymer materials. Cellulose and its derivatives can be widely used in food, medicine, textiles, and building materials. However, cellulose does not have antibacterial properties, which to some extent limits the application of cellulose materials in the antibacterial field.
[0003] Antibacterial fiber materials can inhibit the growth and reproduction of microorganisms, thereby preventing the spread of diseases. There are many varieties of antibacterial fibers, which can generally be divided into two categories: one is natural fibers that have antibacterial properties or fibers made from fiber raw materials that have antibacterial properties, which can be called intrinsic antibacterial fibers; the other is fibers that have antibacterial properties obtained through physical addition or chemical reaction methods, which are generally called modified antibacterial fibers. Intrinsic antibacterial fibers are also called natural antibacterial fibers, such as hemp fibers and bamboo fibers, which have antibacterial properties. In addition, regenerated fibers made from these natural fiber raw materials also have antibacterial properties, such as chitosan fibers and seaweed fibers. Although they are no longer natural fibers strictly speaking, they can also be classified as natural antibacterial fibers.
[0004] Modified antibacterial fibers can be divided into co-spinning method, surface coating method, grafting modification method, etc. according to the preparation method.
[0005] The co-spinning method is a modified antibacterial fiber prepared by co-spinning an antibacterial agent and a matrix. In the early days, the antibacterial fibers mainly prepared by the co-spinning method included nylon, polyester, polypropylene, etc. The antibacterial agent matrix migrates to the surface to play an antibacterial role. It is mostly used in semi-permanent antibacterial products, such as medical and health care, clothing, and industrial decorative fabrics.
[0006] Surface coating is to immerse the fiber in a solution containing an antimicrobial agent, or to coat the antimicrobial agent on the fiber surface to prepare antimicrobial fiber. It is simple to operate, low cost, and has a wide range of selectable antimicrobial agents. It is mostly suitable for antimicrobial finishing of fabrics. However, since most antimicrobial agents only exist on the surface of the antimicrobial fiber, the durability and washing fastness of the antimicrobial effect are poor, and it is often used as disposable sanitary products such as medical dressings, protective clothing, etc.
[0007] The grafting modification method refers to the preparation of antibacterial fibers by chemically bonding antibacterial groups with the surface reactive groups of fibers. The antibacterial fibers are resistant to washing and have stable and long-lasting performance. The antibacterial fibers prepared by the grafting modification method mainly include cotton fibers, regenerated cellulose fibers, polyacrylonitrile fibers, etc., which are mostly used in permanent antibacterial products such as clothing and home textiles. It has been reported that quaternary ammonium salts containing terminal alcohols can be prepared by reacting dodecyl dimethyl tertiary amine with 3-chloropropanol to introduce reactive groups, and then the quaternary ammonium salt antibacterial agent can be grafted with cellulose fibers using a hydroxyl crosslinking agent to give cellulose fibers long-lasting antibacterial properties (Journal of Textile Science and Engineering, 2021, 38(3):36-41). In addition, the antibacterial agent polyhexamethylguanidine is covalently grafted onto the oxidized cotton fiber, and a Schiff base is formed between its terminal amine and the aldehyde group of the fiber, reducing the carbon-nitrogen double bond so that the polyhexamethylguanidine is covalently bound to the surface of the cotton fiber, which can also give the fiber long-lasting antibacterial properties (ACS Applied Materials & Interfaces, 2018, 10(44):38506-38516). However, although the grafting modification method can give cellulose fibers long-lasting antibacterial properties, this method has high requirements for antibacterial agents and a complicated reaction process, which makes the long-lasting antibacterial fiber expensive.
[0008] Therefore, in order to meet the needs of practical applications, developing a low-cost, simple and rapid method to impart long-term antibacterial properties to cellulose materials is of great significance to promote the widespread application of long-term antibacterial cellulose materials. Summary of the invention
[0009] In view of this, the present invention provides a method for preparing a long-lasting antibacterial cellulose material, which is a preparation method with simple operation, low cost and fast reaction, and can quickly impart long-lasting antibacterial properties to the cellulose material at room temperature, so as to solve the problems raised in the existing technology such as poor durability of the antibacterial performance of the fiber material and complex preparation process, thereby being more suitable for application.
[0010] In order to achieve the above object, the present invention adopts the following technical solution:
[0011] A method for preparing a long-acting antibacterial cellulose material comprises the following steps:
[0012] (1) soaking the cellulose material in an alkaline solution for later use;
[0013] (2) mixing the impregnated cellulose material with halogenated carboxylic acid vinyl ester or halogenated carboxylic acid anhydride to react and obtain a surface-esterified cellulose material;
[0014] (3) The surface-esterified cellulose material obtained by the reaction in step (2) is immersed in a solution containing an organic amine to obtain a cellulose material with long-lasting antibacterial properties.
[0015] It should be noted that in the above steps (1) to (3), there is no specific amount ratio in the impregnation / wetting process, as long as it can fully contact with the fiber. Excessive impregnation / wetting has no effect, but too little will cause incomplete reaction due to incomplete impregnation.
[0016] Optionally, the cellulosic material comprises at least one of cotton fiber, regenerated cellulose fiber, wood fiber, and pulp fiber.
[0017] Optionally, the pH of the alkaline solution in step (1) is 9.5-14.8.
[0018] Optionally, the halogenated carboxylic acid vinyl ester in step (2) includes at least one of vinyl chloroacetate, vinyl bromoacetate, vinyl chloropropionate, vinyl bromopropionate, and vinyl chlorobutyrate.
[0019] Optionally, the halogenated carboxylic acid anhydride in step (2) includes at least one of chloroacetic anhydride, bromoacetic anhydride, chloropropionic anhydride and bromopropionic anhydride.
[0020] Optionally, the organic amine in step (3) includes at least one of a primary amine, a secondary amine and a tertiary amine.
[0021] Optionally, the solvent in the solution containing organic amine includes at least one of methanol, ethanol, isopropanol, ether, acetone, chloroform, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethyl sulfoxide and water.
[0022] Optionally, the preferred concentration of the solution containing the organic amine is 1-5%.
[0023] The long-acting antibacterial cellulose material prepared by the above method can be widely used in the fields of textile, medical treatment and food packaging.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention grafts halogenated groups onto the surface of cellulose material through an ester exchange reaction between halogenated carboxylic acid vinyl ester and hydroxyl groups on the surface of cellulose material, and then converts the halogenated groups grafted onto the surface of cellulose into amine groups through amination of halogenated hydrocarbons, thereby fixing the amine groups with antibacterial properties on the surface of cellulose material through covalent bonds. The antibacterial groups are not easy to fall off, and the antibacterial properties of the cellulose material are not easy to decrease after repeated washing and other treatments, thereby giving the cellulose material long-lasting antibacterial properties.
[0026] (2) Compared with the traditional grafting modification method, the method of the present invention can impart long-lasting antibacterial properties to cellulose fibers through continuous impregnation. It is simpler to operate, consumes less chemicals, has lower costs, and has higher reaction efficiency, which can significantly reduce the production cost of antibacterial cellulose materials.
[0027] (3) The method disclosed in the present invention has mild reaction conditions and can react at room temperature without heating, thereby quickly imparting long-lasting antibacterial properties to the cellulose material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0029] Figure 1 This is a schematic diagram of the reaction for preparing long-lasting antibacterial cellulose materials using vinyl chloroacetate as an esterification agent.
[0030] Figure 2 This is the infrared spectrum of the surface chloroacetylated regenerated cellulose fiber sample in Example 2.
[0031] Figure 3 This is the infrared spectrum of the antibacterial fiber sample with quaternary ammonium salt groups on the surface in Example 2. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0034] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0035] In the description of the present invention, it is necessary to understand that the terms "middle", "upper", "lower", "ascending", "descending", "vertical", "face", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0036] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0037] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0038] The invention discloses a method for preparing a long-acting antibacterial cellulose material, comprising the following steps:
[0039] (1) soaking the cellulose material in an alkaline solution;
[0040] (2) mixing the impregnated cellulose material with halogenated carboxylic acid vinyl ester or halogenated carboxylic acid anhydride to react and obtain a surface-esterified cellulose material;
[0041] (3) The surface esterified cellulose material is immersed in a solution containing an organic amine to obtain a cellulose material with long-lasting antibacterial properties.
[0042] In some embodiments, according to the aforementioned preparation method, the cellulose material includes at least one of cotton fiber, regenerated cellulose fiber, wood fiber, and pulp fiber. Specifically, the cellulose material refers to a material whose material matrix contains cellulose macromolecules, and the surface of the cellulose material has exposed hydroxyl groups that can participate in subsequent reactions. The cellulose material can be soaked in the alkaline solution by dipping or by spraying the alkaline solution on the surface of the cellulose material.
[0043] In some embodiments, according to the aforementioned preparation method, the pH of the alkaline solution in the aforementioned step (1) is 9.5 to 14.8. Specifically, when the pH of the alkaline solution in step (1) is lower than 9.5, the transesterification reaction rate of the halogenated carboxylic acid vinyl ester and the hydroxyl groups on the surface of the cellulose material is significantly reduced, and the reaction time is significantly prolonged. When the pH of the alkaline solution in step (1) is higher than 14.8, there are more side reactions, resulting in increased reagent consumption and increased costs.
[0044] In some embodiments, according to the aforementioned preparation method, the halogenated carboxylic acid vinyl ester in the aforementioned step (2) includes at least one of vinyl chloroacetate, vinyl bromoacetate, vinyl chloropropionate, vinyl bromopropionate, and vinyl chlorobutyrate; and the halogenated carboxylic acid anhydride includes at least one of chloroacetic anhydride, bromoacetic anhydride, chloropropionic anhydride, and bromopropionic anhydride. Specifically, as the chain length of the halogenated carboxylic acid group increases, the reactivity of the esterifying agent decreases, the reaction efficiency decreases, and the reagent consumption increases, thereby increasing the cost.
[0045] In some embodiments, the organic amine in the aforementioned step (3) includes at least one of a primary amine, a secondary amine, and a tertiary amine. Specifically, the present invention grafts the halogenated group onto the surface of the cellulose material through an ester exchange reaction between a halogenated carboxylic acid vinyl ester and a hydroxyl group on the surface of the cellulose material or through an esterification reaction between a halogenated carboxylic acid anhydride and a hydroxyl group, and then converts the halogenated group grafted onto the surface of the cellulose into an amine group through an amination of the halogenated group, thereby fixing the amine group with antibacterial properties on the surface of the cellulose material by a covalent bond, and the antibacterial group is not easy to fall off, thereby giving the cellulose material long-lasting antibacterial properties.
[0046] In some embodiments, according to the aforementioned preparation method, the solvent in the solution containing the organic amine in the aforementioned step (3) includes at least one of methanol, ethanol, isopropanol, ether, acetone, chloroform, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, and water.
[0047] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0048] Example 1
[0049] (1) At room temperature, 2 g of regenerated cellulose fiber (1.33 dtex) was immersed in 100 mL of diethylamine aqueous solution (pH 11.0) for 1 min.
[0050] (2) At room temperature, the soaked regenerated cellulose fiber was taken out and placed in 100 mL of vinyl chloroacetate solution and stirred for 5 minutes to obtain surface chloroacetylated regenerated cellulose fiber;
[0051] (3) At room temperature, the surface chloroacetylated regenerated cellulose fiber was placed in 100 mL of 1% triethylamine methanol solution and stirred for 60 minutes. After being taken out, it was washed with 100 mL of pure water and dried in an oven at 80 degrees to obtain regenerated cellulose fiber with long-lasting antibacterial properties.
[0052] The antibacterial rates of the antibacterial cellulose samples against Staphylococcus aureus and Escherichia coli were measured by GB / T 20944.3-2008 and were 52% and 60%, respectively.
[0053] Example 2
[0054] The difference from Example 1 is that step (3) uses a 1% methanol solution of dodecyl dimethyl tertiary amine. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 and were 86% and 90%, respectively.
[0055] Example 3
[0056] The difference from Example 2 is that the antibacterial cellulose sample obtained in step (3) is repeatedly washed 5 times according to the experimental condition A1M in GB / T 12490. After repeated washing, the sample is tested according to GB / T 20944.3-2008, and the antibacterial rates of the sample against Staphylococcus aureus and Escherichia coli are 84% and 89%, respectively.
[0057] Example 4
[0058] The difference from Example 1 is that step (3) uses a 1% methanol solution of N,N-dimethylbenzylamine. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T20944.3-2008 and were 75% and 68%, respectively.
[0059] Example 5
[0060] The difference from Example 4 is that the antibacterial cellulose sample obtained in step (3) is washed repeatedly 10 times according to the experimental condition A1M in GB / T 12490. The antibacterial rates of the above sample against Staphylococcus aureus and Escherichia coli are measured by GB / T 20944.3-2008 to be 74% and 66%, respectively.
[0061] Example 6
[0062] The difference from Example 1 is that step (3) uses a 1% benzylamine tetrahydrofuran solution. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T20944.3-2008 and were 61% and 63%, respectively.
[0063] Example 7
[0064] The difference from Example 1 is that step (1) uses cotton fiber as raw material, and step (3) uses 1% methanol solution of dodecyl dimethyl tertiary amine. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 to be 83% and 86%, respectively.
[0065] Example 8
[0066] The difference from Example 1 is that step (1) uses pulp fiber as raw material, and step (3) uses 1% methanol solution of dodecyl dimethyl tertiary amine. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 to be 69% and 72%, respectively.
[0067] Example 9
[0068] The difference from Example 1 is that step (1) uses a sodium hydroxide aqueous solution with a pH of 14.8, and step (3) uses a 1% methanol solution of dodecyl dimethyl tertiary amine. The antibacterial rates of the antibacterial cellulose sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 to be 72% and 79%, respectively.
[0069] Example 10
[0070] The difference from Example 1 is that step (1) uses a dimethylaminopyridine aqueous solution with a pH of 9.5, and step (3) uses a 5% methanol solution of dodecyldimethylamine. The antibacterial rates of the above samples against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 to be 61% and 63%, respectively.
[0071] Embodiment 11
[0072] The difference from Example 10 is that step (3) uses 1% dodecyl dimethyl tertiary amine acetone solution. The antibacterial rates of the above sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 and were 65% and 62%, respectively.
[0073] Example 12
[0074] The difference from Example 10 is that step (3) uses a 1% chloroform solution of dodecyl dimethyl tertiary amine. The antibacterial rates of the above sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 and were 63% and 63%, respectively.
[0075] Embodiment 13
[0076] The difference from Example 10 is that chloroacetic anhydride is used as the esterification agent in step (2). The antibacterial rates of the above sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 and were 67% and 65%, respectively.
[0077] Embodiment 14
[0078] The difference from Example 10 is that bromoacetic anhydride is used as the esterification agent in step (2). The antibacterial rates of the above sample against Staphylococcus aureus and Escherichia coli were measured using GB / T 20944.3-2008 and were 60% and 61%, respectively.
[0079] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0080] Comparative Example 1
[0081] 2 g of regenerated cellulose fiber (1.33 dtex) was placed in 100 mL of 1% triethylamine methanol solution and stirred for 60 minutes. After being taken out, it was washed with 100 mL of pure water and dried in an oven at 80 degrees. The product was directly measured using GB / T20944.3-2008, and its antibacterial rates against Staphylococcus aureus and Escherichia coli were 2% and 3%, respectively.
[0082] From the above-mentioned embodiments, infrared spectra of the embodiments and comparative examples, it can be seen that the present invention first grafts the halogenated groups onto the surface of the cellulose material (such as Figure 2 As shown), the halogenated groups grafted onto the cellulose surface are then converted into amine groups by aminolysis of the halogenated groups (as shown Figure 3 As shown in the figure, the amine structure with antibacterial properties can be directly connected to the surface of the cellulose material through chemical bonds, thereby giving the cellulose material long-lasting antibacterial properties. The reaction can be completed quickly at room temperature, is easy to operate, consumes less chemicals, and is low in cost.
[0083] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a long-lasting antibacterial cellulose material, characterized in that: The following steps are involved: (1) soaking the cellulose material in an alkaline aqueous solution for later use; (2) mixing the impregnated cellulose material with halogenated carboxylic acid vinyl ester or halogenated carboxylic acid anhydride to react and obtain a surface-esterified cellulose material; (3) immersing the surface-esterified cellulose material obtained in step (2) in a solution containing an organic amine to obtain a cellulose material with long-lasting antibacterial properties; In step (1), the pH of the alkaline aqueous solution is 9.5-14.
8.
2. The method for preparing the long-acting antibacterial cellulose material according to claim 1, characterized in that: The cellulose material includes at least one of cotton fiber, regenerated cellulose fiber, wood fiber and pulp fiber.
3. The method for preparing the long-acting antibacterial cellulose material according to claim 1, characterized in that: In step (2), the halogenated carboxylic acid vinyl ester includes at least one of vinyl chloroacetate, vinyl bromoacetate, vinyl chloropropionate, vinyl bromopropionate, and vinyl chlorobutyrate.
4. The method for preparing the long-acting antibacterial cellulose material according to claim 1 or 3, characterized in that: In step (2), the halogenated carboxylic acid anhydride comprises at least one of chloroacetic anhydride, bromoacetic anhydride, chloropropionic anhydride and bromopropionic anhydride.
5. The method for preparing the long-acting antibacterial cellulose material according to claim 1, characterized in that: In step (3), the organic amine includes at least one of a primary amine, a secondary amine, and a tertiary amine.
6. The method for preparing the long-acting antibacterial cellulose material according to claim 1 or 5, characterized in that: In step (3), the solvent in the solution containing the organic amine includes at least one of methanol, ethanol, isopropanol, ether, acetone, chloroform, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethyl sulfoxide and water.
7. The method for preparing the long-acting antibacterial cellulose material according to claim 1, characterized in that: The concentration of the solution containing organic amine is 1-5%.