Negative electrode material and preparation method thereof, and electrochemical device
By using negative electrode materials containing silicon and carbon materials in lithium-ion batteries, combined with specific pore structure distribution and carbon cladding, the problems of poor conductivity and volume expansion of traditional negative electrode materials are solved, and the battery's magnification and cycling stability are improved. Especially in high and low temperature environments.
Patent Information
- Application Number
- CN202411131889.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Traditional graphite negative electrode materials cannot meet the performance requirements of high specific capacity and high voltage lithium-ion batteries, and the silicon carbon negative electrode materials have poor conductivity, uneven dispersion, and are prone to side reactions with the electrolyte, resulting in unsatisfactory volume expansion and electrochemical performance. .
Using negative electrode materials containing silicon and carbon materials, the lithium ion transmission efficiency and diffusion capacity can be adjusted through specific pore structure distribution characteristics (pore structures of 2nm~20nm and 20nm~80nm) and carbon cladding layer, and the lithium ion transmission efficiency and diffusion capacity can be improved, and the conductivity and cycling stability can be improved. sex.
It achieves the reduction of volume expansion, improves conductivity, rate performance and cycle stability, and improves the high and low temperature performance and storage performance of the battery.
Smart Images

Figure CN118658984B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and specifically to a negative electrode material and a preparation method thereof, and an electrochemical device. Background Art
[0002] In recent years, lithium-ion batteries have been widely used in various fields. With the breakthroughs in the research and development of positive electrode materials such as high specific capacity and high voltage, traditional graphite-based negative electrode materials can no longer meet the performance requirements of the next generation of lithium-ion batteries, and negative electrode materials with higher capacity and better performance are urgently needed to be developed. Compared with graphite, elemental silicon is considered to be an ideal negative electrode material that can replace graphite due to its higher theoretical specific capacity and suitable operating voltage. However, the large volume expansion in the alloying reaction / de-alloying reaction of elemental silicon with lithium will cause the capacity of electrochemical devices (e.g., lithium-ion batteries) to decay rapidly.
[0003] In the related art, silicon is dispersed in porous carbon materials to prepare silicon-carbon negative electrode materials in order to alleviate the volume expansion of silicon. However, the conductivity of the above-mentioned silicon-carbon negative electrode materials is poor, silicon is unevenly dispersed in the porous carbon materials, the amount of silicon deposited in the porous carbon materials is low, and it is easy to react with the electrolyte to dissolve the active ingredients inside the silicon-carbon negative electrode materials, etc., resulting in the volume expansion and electrochemical performance of the silicon-carbon negative electrode materials are still not ideal and need to be improved. Summary of the invention
[0004] The present application provides a negative electrode material that can reduce volume expansion, improve conductivity, rate performance and cycle stability.
[0005] In addition, the embodiments of the present application also provide a method for preparing the aforementioned negative electrode material and an electrochemical device comprising the aforementioned negative electrode material.
[0006] The embodiment of the present application provides a negative electrode material, which includes a silicon-containing material and a carbon-containing material. The negative electrode material has a pore structure, and the pore structure has the following distribution characteristics:
[0007] The negative electrode material is tested by the BET method, and it is found that the negative electrode material has a first pore structure with a pore size of 2nm~20nm and a second pore structure with a pore size of 20nm~80nm, the pore volume of the first pore structure is V1, the pore volume of the second pore structure is V2, and the specific surface area of the negative electrode material is S, wherein 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g.
[0008] The present invention also provides a method for preparing a negative electrode material, which comprises the following steps:
[0009] Screening the silicon source by particle size, cleaning and drying to obtain the core;
[0010] The core is added into a deionized water solution of a surfactant, and nano-silicon dioxide and ball milling beads are added to perform ball milling to obtain a negative electrode material precursor;
[0011] Carbon coating the negative electrode material precursor to obtain a negative electrode material matrix; and
[0012] The negative electrode material matrix is subjected to alkaline solution to remove the nano-silicon dioxide to obtain the negative electrode material, wherein the negative electrode material has a pore structure, and the pore structure has the following distribution characteristics:
[0013] The negative electrode material is tested by the BET method, and it is found that the negative electrode material has a first pore structure with a pore size of 2nm~20nm and a second pore structure with a pore size of 20nm~80nm, the pore volume of the first pore structure is V1, the pore volume of the second pore structure is V2, and the specific surface area of the negative electrode material is S, wherein 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g.
[0014] An embodiment of the present application further provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet includes a negative electrode active substance, and the negative electrode active substance includes the negative electrode material as described above.
[0015] Compared with the prior art, the negative electrode material provided in the embodiment of the present application has a specific pore structure distribution characteristic, wherein the ratio of the total pore volume of the first pore structure and the second pore structure in the negative electrode material to the specific surface area of the negative electrode material ((V1+V2) / S) represents the homogenized depth value of the pore structure of the negative electrode material. The appropriate homogenized depth value of the pore structure ((V1+V2) / S), the pore volume ratio of the first pore structure to the second pore structure (V1 / V2) and the specific surface area (S) of the negative electrode material can improve the lithium ion transmission efficiency by adjusting the diffusion flux and diffusion depth of the electrolyte and the slurry in the negative electrode material, thereby improving the rate performance of the negative electrode material; at the same time, due to the appropriate pore structure, the negative electrode material can still maintain good lithium ion diffusion capacity under high and low temperature environments, showing excellent high and low temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A process flow chart of the method for preparing the negative electrode material provided in an embodiment of the present application.
[0017] Figure 2This is a schematic diagram of the structure of the electrochemical device provided in an embodiment of the present application. DETAILED DESCRIPTION
[0018] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0019] The embodiment of the present application provides a negative electrode material, which includes a silicon-containing material and a carbon-containing material. The negative electrode material has a pore structure, and the pore structure has the following distribution characteristics: the negative electrode material is tested by the BET method, and it is measured that the negative electrode material has a first pore structure with a pore diameter of 2nm~20nm and a second pore structure with a pore diameter of 20nm~80nm, the pore volume of the first pore structure is V1, the pore volume of the second pore structure is V2, and the specific surface area of the negative electrode material is S, wherein 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g.
[0020] The ratio of the total pore volume of the first pore structure and the second pore structure in the negative electrode material to the specific surface area of the negative electrode material is 0.1μm≥(V1+V2) / S≥0.01μm. This ratio is the homogenized depth value of the pore structure of the negative electrode material. The pore structures of different pore diameters are standardized and determined, which reflects the diffusion depth of the electrolyte in the negative electrode material and affects the speed of lithium ion transmission in the pores of the pore structure of the negative electrode material. When the depth value is too large (greater than 0.1μm), the electrolyte infiltration efficiency is low and the lithium ion transmission efficiency is greatly reduced; when the depth value is too small (less than 0.01μm), it will cause the electrolyte infiltration to be out of control, and the electrolyte will quickly enter the interior of the negative electrode material, causing oxidation of the active material and excessive gas production, leading to problems such as reduced structural stability, cycle stability and rate performance of the negative electrode material. Therefore, by regulating the ratio of the pore structure volume and specific surface area of the negative electrode material within the above range, a suitable pore structure depth value can be obtained, which helps to balance the lithium ion transmission performance and promote the transmission of lithium ions inside the negative electrode material, thereby improving the stability and rate performance of the negative electrode material.
[0021] Controlling the pore volume ratio (V1 / V2) of the first pore structure to the second pore structure in the negative electrode material within the range of 0.01~0.8 can effectively adjust the hydrophilicity of the negative electrode material particles and further improve the low temperature performance and rate performance of the negative electrode material. This is because the pore volume distribution within the above range can effectively expand the lithium ion transmission interface while shortening the lithium ion transmission path, thereby reducing the lithium ion transmission resistance, improving the lithium ion transmission efficiency, and improving the rate performance of the negative electrode material. In addition, in a low temperature environment with low lithium ion transmission efficiency, the negative electrode material can still maintain good lithium ion diffusion capacity and exhibit excellent low temperature performance. In addition, a reasonable pore volume distribution can simultaneously adjust the wettability of the negative electrode material in polar and non-polar solvents.
[0022] As mentioned above, the pore volume distribution will affect the wettability of the electrolyte and polar solvents. Specifically, with the 20nm pore size structure as the boundary, the first pore structure with a pore size of 2nm~20nm includes micropores (2~5nm) and mesopores (5nm~20nm) close to the size of micropores. The existence of the first pore structure slows down the electrolyte infiltration speed and greatly increases the specific surface area of the negative electrode material. However, if the proportion of the first pore structure is too high, it will lead to particle agglomeration, reduced rate performance, and electrolyte degradation, which will further cause the pore structure to close, resulting in excessive local thickness of SEI, affecting the lithium ion transmission path. The second pore structure with a pore size in the range of 20nm~80nm includes mesopores (20nm~50nm) and macropores close to the size of mesopores (50nm~80nm). The existence of the second pore structure is conducive to balancing the specific surface area of the negative electrode material, improving the wetting efficiency, improving the uniformity of electrolyte degradation, forming a stable and uniform SEI, and optimizing the lithium ion transmission path; however, if the second pore structure accounts for too much, it may cause the slurry to diffuse rapidly in the negative electrode material when preparing the electrochemical device, and react with the active components, thereby causing particle pulverization during the cycle and reducing the cycle performance; if the second pore structure accounts for too little, it will reduce the electrolyte wetting efficiency and is not conducive to alleviating the volume expansion effect during the charge and discharge process. Therefore, controlling V1 / V2 in the range of 0.01~0.8 is also conducive to balancing the electrolyte wetting speed of the negative electrode material.
[0023] The specific surface area S of the negative electrode material ranges from 10.0 m 2 / g≥S≥0.1m 2 / g, the specific surface area S is a key factor in the material transfer and reaction between the negative electrode material and the electrolyte. The specific surface area within the above range can provide more active reaction sites and channels for the negative electrode material, which is beneficial to the adsorption and diffusion rate of lithium ions, accelerates the charge and discharge rate, and improves the performance of the prepared battery.
[0024] Therefore, the V1, V2 and S of the negative electrode material are controlled in the following ranges: 0.1 μm ≥ (V1 + V2) / S ≥ 0.01 μm, 0.8 ≥ V1 / V2 ≥ 0.01, 10.0 μm 2 / g≥S≥0.1m 2 / g, by homogenizing the pore structure depth value, it can be found that the electrolyte infiltration efficiency is optimal within the depth range of 0.01μm~0.1μm, which is beneficial to balance the uniformity of electrolyte degradation, form a stable and uniform SEI, and optimize the lithium ion transmission path, thereby improving the stability and rate performance of the negative electrode material.
[0025] Furthermore, the pore volume of the first pore structure and the second pore structure in the pore structure can be adjusted to meet the above pore structure. In some embodiments, the pore volume V1 can be 0.5 cm 3 / g≥V1≥0.001cm 3 / g, V1 within the above range can shorten the lithium ion transmission path, which is beneficial to improve the diffusion rate of lithium ions inside the negative electrode material; the pore volume V2 can be 5.0cm 3 / g≥V2≥0.01cm 3 / g, V2 in the above range provides sufficient space for electrolyte infiltration and volume expansion of negative electrode materials, increases the adsorption and release rate of lithium ions, and improves the structural stability of the negative electrode materials.
[0026] The negative electrode material having the above-mentioned pore structure determines the hydrophilicity and lipophilicity of the negative electrode material, which will affect the dispersibility of the negative electrode material in the slurry during the battery preparation process and the infiltration depth of the electrolyte into the negative electrode material during the electrochemical reaction, thereby affecting the performance of the battery prepared by the final negative electrode material. In the embodiment of the present application, the negative electrode material has the above-mentioned pore structure, which can improve the solid-liquid reaction efficiency on the surface of the negative electrode material, including the diffusion efficiency, ion diffusion flux and diffusion depth of lithium ions, thereby improving the storage performance and rate performance of the battery prepared by the negative electrode material under high and low temperature conditions.
[0027] In some embodiments, the particle size D50 of the anode material may range from 2.0 μm to 15.0 μm, and further may be from 4.0 μm to 10.0 μm. Exemplarily, the particle size D50 of the anode material may be 2.0 μm, 3.0 μm, 4.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm, 10.0 μm, 11.0 μm, 12.0 μm, 13.0 μm, 14.0 μm or 15.0 μm, etc. Controlling the particle size of the anode material within the above range helps to ensure the consistency of the anode material, thereby improving the performance stability of the anode material; it can also increase the specific surface area of the anode material, which helps to improve the transmission rate of lithium ions in the anode material and the reaction activity of the electrode; at the same time, it reduces the particle size of the anode material being too low (less than 2 μm), thereby reducing the volume expansion of the anode material during light charge and discharge processes, which is beneficial to maintaining the structural stability and cycle life of the anode material.
[0028] In some embodiments, the anode material may mainly include silicon-containing materials and carbon-containing materials, and the phases may mainly include elemental silicon, silicon oxides, silicates or elemental carbon-based materials, etc. Among them, the total mass of the silicon-containing materials and carbon-containing materials may account for 40% to 97.5% of the total mass of the anode material, and further may be 40% to 90%, and further may be 40% to 80%. Exemplarily, it may be 40%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%, etc. Limiting the total mass ratio of the silicon-containing materials and carbon-containing materials ensures that the composition of the anode powder material is within a certain range, which helps to control the chemical composition of the anode material and ensure the stable and reliable performance of the anode material in the electrochemical device.
[0029] In some embodiments, the chemical general formula of the silicon oxide is SiO x , where 0 < x ≤ 2. Exemplarily, x may be 0.05, 0.11, 0.21, 0.26, 0.31, 0.41, 0.51, 0.59, 0.61, 0.69, 0.71, 0.74, 0.76, 0.79, 0.89, 0.99, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2, etc., which is not limited herein. Further, 0 < x < 1. The silicon oxide may be a material formed by silicon particles dispersed in SiO2, or a material having a tetrahedral structural unit, where the silicon atom is located at the center of the tetrahedral structural unit, and the silicon atom and / or oxygen atom is located at the four vertices of the tetrahedral structural unit.
[0030] In some embodiments, the mass of carbon element accounts for 1.5% to 45.5% of the total mass of the negative electrode material, and may further be 5% to 40%, and may be 1.5%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 45.5%, etc. For example, a silicon-containing material is used as a core, and a carbon coating layer is formed on the surface of the core to form the main part of the negative electrode material. On the one hand, the carbon coating layer is beneficial to hinder the direct contact between the active silicon in the core and the slurry, inhibit the occurrence of side reactions, thereby reducing the excessive growth of SEI, reducing the loss of active silicon and active lithium, and improving the capacity and initial efficiency of the negative electrode material; on the second hand, the silicon-based core has the problem of poor conductivity, and the carbon coating layer is conducive to the formation of a conductive network, which can improve the conductivity of the negative electrode material, and the coating layer ensures the contact of the conductive network during the cycle, reduces the production of active substances such as "dead silicon" that are separated from the conductive network, and improves the cycle performance of the negative electrode material; on the third hand, the carbon coating layer can provide a stable physical interface to inhibit excessive expansion of particles, and can also serve as a SEI growth skeleton to form a stable SEI layer, further stabilize the solid-liquid interface, inhibit expansion, and improve safety; on the fourth hand, the coating layer can further regulate the surface pore structure, and by adjusting the coating process parameters, regulate the specific surface area to achieve improvements in rate performance and high and low temperature performance. At the same time, it can also reasonably construct an expansion buffer space to reduce the deformation of the negative electrode material.
[0031] In some embodiments, the negative electrode material may further include one or more doping elements. Specifically, the doping elements may include at least one of hydrogen, oxygen, lithium, magnesium, aluminum, nitrogen, phosphorus, sulfur, boron, fluorine, molybdenum, sodium, potassium, calcium, titanium, niobium, lanthanum, tin, selenium and cerium. Doping the negative electrode material with elements can optimize the structure and performance of the negative electrode material and improve the cycle life and safety of the negative electrode material. Doping elements (such as doping with hydrogen, oxygen, lithium, nitrogen, phosphorus, boron, sulfur, fluorine, sodium, potassium, calcium, titanium, niobium, tin, selenium or cerium) can improve the electrochemical properties of the negative electrode material, including increasing the storage capacity of lithium ions, increasing the conductivity and reducing the electrode polarization, thereby improving the performance and cycle life of the battery; some doping elements (magnesium, aluminum or lanthanum, etc.) can slow down the volume expansion of the negative electrode material during the insertion / extraction of lithium ions, reduce the loss of the material and structural damage, thereby improving the cycle life of the negative electrode material.
[0032] In some embodiments, the content of the doping element in the negative electrode material may be 25ppm to 120000ppm, further may be 50ppm to 80000ppm, further may be 100ppm to 50000ppm, illustratively may be 25ppm, 50ppm, 100ppm, 500ppm, 1000ppm, 5000ppm, 10000ppm, 30000ppm, 50000ppm, 75000ppm, 80000ppm, 100000ppm or 120000ppm, etc. Controlling the content of the doping element in the negative electrode material within the above range may optimize the structure and performance of the negative electrode material. If the content is too low (lower than 25ppm), the purpose of optimizing the electrochemical performance may not be achieved, resulting in reduced storage capacity, reduced conductivity, reduced structural stability, etc. of the negative electrode material. If the content is too high (higher than 120000ppm), the electrochemical performance of the negative electrode material may be deteriorated, the structural stability may be impaired, the cost may be increased, and other problems may occur.
[0033] In some embodiments, the oil absorption value of the negative electrode material can be 25 mL / 100 g to 85 mL / 100 g, and further can be 35 mL / 100 g to 75 mL / 100 g, and can be 25 mL / 100 g, 35 mL / 100 g, 45 mL / 100 g, 55 mL / 100 g, 65 mL / 100 g, 75 mL / 100 g or 85 mL / 100 g, etc. The test method can be to drip the oil into the negative electrode material at a constant rate, and stir at a constant speed at the same time, the viscosity of the mixture of oil and negative electrode material gradually increases and a peak value appears, and the oil absorption value of the negative electrode material is calculated by the amount of oil dripped at 70% of the maximum torque. The oil absorption value of the negative electrode material in the above range is conducive to the production and processing of the negative electrode material and the process operation, and can also ensure the stability and safety of the battery while maintaining the performance and cycle life of the prepared battery.
[0034] In some embodiments, the pH value of the negative electrode material may be 7.5 to 12.0, and may further be 9 to 11, and may be 7.5, 8, 9, 10, 11 or 12, etc. According to GB / T 24533-2019, the pH value of the negative electrode material in water is tested for stability. The pH value of the negative electrode material may affect the interfacial reaction and interaction between the electrode and the electrolyte. The pH value in the above range is conducive to improving the stability and cycle life of the negative electrode material, and is convenient for control and quality management during the production of the negative electrode material.
[0035] In some embodiments, the integral area of the isothermal adsorption hysteresis loop of the negative electrode material can be 1.0×10 -4 ~5.0×10 -2. The isotherm curve obtained by testing the pore size distribution of the negative electrode material according to the GB / T 21650.3-2011 method was used to calculate the integral area of the isothermal adsorption hysteresis loop of the negative electrode material. The test process was as follows: at liquid nitrogen (77K, -196°C), N2 reached adsorption equilibrium and desorption equilibrium at different relative pressures. The integral area of the isothermal adsorption hysteresis curve is an important parameter for evaluating the pore structure and specific surface area of the negative electrode material. Further controlling the values of the pore structure and specific surface area of the negative electrode material within the above range will help optimize the performance of the negative electrode material.
[0036] In some embodiments, the pore size range of the negative electrode material can be 0.5nm~300nm, further can be 2nm~150nm, further can be 2nm~80nm. According to the isotherms of the adsorption branch and the desorption branch, the pore size distribution of the negative electrode material is obtained by the BJH, HK, and DFT models. The pore size range of the negative electrode material is 0.5nm~300nm, wherein a smaller pore size can provide a higher specific surface area, while a larger pore size is conducive to the penetration and diffusion of ions.
[0037] Compared with the prior art, the negative electrode material provided in the embodiment of the present application has the following beneficial effects:
[0038] 1. The negative electrode material has a pore structure with nanoscale pore size distribution (the first pore structure and the second pore structure). Reasonable pore size structure distribution can balance the pore volume and specific surface area of the negative electrode material to obtain a suitable pore structure depth, thereby controlling the electrolyte infiltration efficiency of the negative electrode material, balancing the uniformity of electrolyte degradation, forming a stable and uniform SEI, optimizing the lithium ion transmission path, and alleviating volume expansion, thereby improving the capacity, rate performance, structural stability, cycle efficiency, storage performance and electrochemical performance of the negative electrode material under high and low temperature conditions.
[0039] 2. The carbon coating layer on the surface of the negative electrode material can reduce the loss of active silicon and active lithium, and improve the capacity and initial efficiency of the negative electrode material; the carbon coating layer is also conducive to the formation of a conductive network, which can improve the conductivity and cycle performance of the negative electrode material; and the carbon coating layer can provide a stable physical interface, construct an expansion buffer space, inhibit excessive expansion of particles, reduce the deformation of the negative electrode material, and improve safety; in addition, the carbon coating layer can control the filling of nano-scale pore structure by adjusting the carbon coating, change the pore volume and pore area of the negative electrode material, thereby further regulating the specific surface area of the negative electrode material, and realizing the improvement of the rate performance and high and low temperature performance of the negative electrode material.
[0040] See also Figure 1 As shown, the method for preparing the negative electrode material provided in the embodiment of the present application specifically comprises the following steps:
[0041] Step S1, screening the silicon source by particle size, cleaning and drying to obtain the core.
[0042] Specifically, the silicon source raw material is pre-treated, including selecting the silicon source, grading it, and then screening for a suitable particle size. The silicon source is ultrasonically cleaned with deionized water and alcohol respectively, and then centrifuged and vacuum dried. After drying, it is sieved and scattered to obtain the kernel. It can be understood that the cleaning process is not limited to ultrasonic cleaning, and any method that can achieve the cleaning of the raw material; the drying process is not limited to vacuum drying, and any method that can achieve the drying of the raw material.
[0043] In some embodiments, the silicon source may include at least one of elemental silicon, silicon monoxide, silicon dioxide, and silicate, etc. Different silicon sources have different crystal structures, morphologies, and chemical properties. By selecting a suitable silicon source, the properties of silicon-based materials can be regulated.
[0044] In some embodiments, the cleaning time can be 30 min to 360 min; the centrifugation time can be 60 min to 120 min. Within the above range, the silicon source can be cleaned, the soluble salts and small molecular organic matter on the surface of the silicon source can be washed away, the impurity content can be reduced, and the occurrence of surface side reactions can be reduced.
[0045] In some embodiments, the drying time may be 3 hours to 48 hours, and the drying temperature may be 45° C. to 80° C. Low-temperature vacuum drying can effectively control the degree of oxidation on the surface of the material and regulate the reaction interface.
[0046] In this step, the screening of the particle size of the silicon source raw material can control the specific surface area of the material, thereby controlling the subsequent reaction efficiency, and can also ensure high consistency of the specific surface area between the raw material particles, which is beneficial to the uniformity of the subsequent preparation process and effectively reduces the differences between the negative electrode material particles.
[0047] In step S2, the core is doped with elements by plasma to obtain an element-doped core. The doped elements may include at least one of hydrogen, oxygen, lithium, magnesium, aluminum, nitrogen, phosphorus, sulfur, boron, fluorine, molybdenum, sodium, potassium, calcium, titanium, niobium, lanthanum, tin, selenium and cerium.
[0048] Specifically, plasma is used for element doping. A solid-state doping source may be used as a metal element doping source, and a corresponding compound gas-phase doping source may be used as a non-metallic doping source.
[0049] First, the reaction chamber is evacuated to a pressure of ≤0.1Pa; when the pressure meets the requirements, the state is maintained for about 30 minutes, and argon and hydrogen mixed gas is introduced, the mixing ratio is 1:1, and the mixed gas flow rate can be 500mL / min~3000mL / min. After the argon is introduced, the pressure is controlled to 1000~8000Pa through the vacuum valve; the plasma is turned on for plasma treatment. The core sample is doped. After the plasma emits light, the doping source (solid state) is immersed in the plasma (the immersion depth is adjusted according to the melting and boiling points of different elements to ensure that the doping source maintains a solid shape), and the doping reaction is carried out. The reaction time can be 6.0h~48.0h, and the doping amount is controlled; the gas phase doping source can be directly introduced into the reaction chamber, the gas phase flow rate can be 300mL / min~1500mL / min, and the pressure is controlled at 2000Pa~10000Pa, and the doping reaction treatment is carried out, and the treatment time is 1.0h~24.0h. The above two physical phase doping sources can also be used in combination.
[0050] After doping is completed, hydrogen is introduced at a rate of 500mL / min~1000mL / min, the pressure is controlled at 100Pa~1000Pa, and the treatment time is 15min~60min. Using hydrogen treatment, hydrogen atoms are introduced into these defects or active points through reduction, saturating surface defects and reducing different active points, thereby coordinating the degradation efficiency of the electrolyte, optimizing the core surface reaction interface, reducing excessive degradation of the core material and uneven expansion force, which is beneficial to improving the high and low temperature storage performance, rate and cycle performance of the final negative electrode material.
[0051] After the above treatment is completed, the material is discharged and subjected to high-temperature heat treatment. The temperature of the high-temperature heat treatment is controlled at 350-950°C and the treatment time is controlled at 2.0-24.0h. After the high-temperature heat treatment is completed, the material is broken up and sieved.
[0052] The core is doped by plasma, which has high uniformity, rapid reaction and wide temperature controllable range. The doping source is bombarded by high-energy plasma ions, so that the doping source ions are stripped from the block to form highly active particles, and doped by combining plasma with the core, which can achieve low-temperature doping and high doping efficiency, effectively improve the utilization rate of doping elements, and realize the electrochemical performance of doping elements.
[0053] Step S3, adding the element-doped core into a deionized water solution of a surfactant, and adding nano-silicon dioxide and ball milling beads for ball milling to obtain a negative electrode material precursor.
[0054] Specifically, the surfactant is first dissolved in an appropriate amount of deionized water to prepare a liquid phase dispersion, which is then added to the core in a certain proportion, and then nano-silicon dioxide is added. Finally, the material is processed for pore structure using high-energy ball milling. After the ball milling is completed, centrifugal dehydration treatment can be performed, and it can be dried in an Ar gas atmosphere.
[0055] Among them, dissolving the surfactant in an appropriate amount of deionized water to prepare a liquid phase dispersion can ensure that the surfactant can be fully dissolved and evenly dispersed in the deionized water, which is beneficial to increase the contact area between the surfactant and the core and promote the reaction. Using deionized water for dissolution can reduce the interference of impurities in the water on the reaction and ensure the repeatability and accuracy of the production process.
[0056] In some embodiments, the surfactant may include one of an alkaline solution and an organic oxidant. Using an alkaline solution or an organic oxidant as a surfactant is beneficial to promoting the interaction between the silicon source and nano-silicon dioxide to form a desired nanostructure. The alkaline solution can provide an alkaline environment to promote the surface activation of the silicon source, while the organic oxidant can provide oxygen atoms to promote the oxidation reaction of the silicon source and trigger chemical reactions on the surface of the silicon source. These reactions help to regulate the interaction between the silicon source and nano-silicon dioxide to achieve the desired nanoscale pore structure regulation and optimization.
[0057] In some embodiments, the particle size of nano-silica can be less than or equal to 80 nm. The use of nano-silica in the above particle size range can cause the silicon particles to collide and rub during the ball milling process through the action of mechanical force and thermal energy, so that micropores and mesoporous structures with a pore size less than or equal to 80 nm are formed on the surface of the material, and a unique pore size distribution is formed.
[0058] In some embodiments, the mass ratio of the core, surfactant, deionized water, nano-silica and ball milling beads is 1: (0.1~0.5): (1~5): (0.01~0.05): (0.3~2). The mass ratio of the core, water and surfactant can be 1: 1~5: 0.1~0.5; the mass ratio of the core to the ball milling beads can be 1: 0.3~2; finally, nano-silica with a particle size of less than 80nm is added according to a mass ratio of 1: 0.01~0.05 to the core. Different material ratios will affect the reaction conditions and energy transfer efficiency during ball milling, and also affect the size distribution, uniform surface structure and electrochemical properties of the negative electrode material precursor. Within the above-defined range, by precisely controlling the mass ratio of the core, surfactant, deionized water, nano-silica and ball milling beads, the appropriate ratio of various components in the reaction process can be ensured to achieve the desired reaction path and product quality.
[0059] In some embodiments, the ball milling time may be 30 min to 90 min, further may be 30 min to 60 min, illustratively may be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min or 90 min, etc. The ball milling time is controlled within the above range to fully achieve the desired material structure control and particle size refinement.
[0060] In some embodiments, the drying temperature may be set at 60-120° C. and the drying time may be 24-72 hours. Under these conditions, moisture in the material can be removed while maximally maintaining the structural integrity and stability of the material.
[0061] The nanoparticles are ball-milled together with the large particle materials using ball milling technology, so that the nanoparticles are adsorbed on the surface of the large particle core, so that the nanoparticles form a layer of coverage on the core surface. The covering layer can be used as a template, and the nanoparticles are subsequently removed through certain treatment or removal methods, such as sintering or dissolution, to form a prototype with a pore structure to achieve the regulation of the pore structure. At the same time, the ball milling process is optimized, the ball-to-material ratio of the ball milling is greatly reduced, and the excessive reduction of the particle size can be reduced.
[0062] Step S4, carbon-coating the negative electrode material precursor to obtain a negative electrode material matrix.
[0063] Specifically, after placing the negative electrode material precursor obtained in step S3 in a deposition reaction chamber, a protective gas is introduced into the reaction chamber to exhaust the oxygen in the deposition reaction chamber. When the oxygen concentration drops below 1 ppm, the oxygen is exhausted for 30 minutes, and then the coating source gas is introduced. The flow rate and time are adjusted according to different coating sources. After the coating is completed, the coating source gas is stopped, and the coating layer can be further heat treated.
[0064] In some embodiments, carbon coating may include placing the cathode material precursor in a reaction device and introducing a coating source gas for chemical vapor deposition. Chemical vapor deposition can achieve uniformity, controllability, high efficiency, high surface activity and good packaging of the carbon layer on the material surface, thereby improving the performance and application potential of the cathode material.
[0065] In some embodiments, the coating source gas may include at least one of methane, ethane, acetylene, ethylene, and propane to provide carbon atoms for depositing the carbon layer during the coating process.
[0066] In some embodiments, the temperature of the carbon coating can be 450°C to 1000°C, and the time can be 1h to 48.0h. By adjusting the temperature and time, the carbon coating process can be controlled and optimized to ensure the formation and stability of the carbon layer.
[0067] In some embodiments, the flow rate of the coating source gas can be 300 mL / min to 3000 mL / min. Controlling the flow rate of the coating source gas can adjust the supply rate of the carbon source, affect the thickness and morphology of the carbon layer, and by adjusting the flow rate, control of the carbon layer deposition rate and uniformity can be achieved, thereby optimizing the quality and performance of the carbon coating.
[0068] In some embodiments, the heat treatment temperature may be 600°C to 1000°C, the heat treatment time may be 0 to 12 hours, and the flow rate of the protective gas may be kept unchanged during the heat treatment. The heat treatment process may further stabilize and improve the structure and properties of the carbon layer, promote the crystallization and densification of the carbon layer, and enhance the bonding force and stability between the carbon layer and the negative electrode material.
[0069] There are many favorable factors for coating the negative electrode material precursor: first, it prevents the active silicon in the negative electrode material precursor from directly contacting with the electrolyte, inhibits the occurrence of side reactions, reduces the excessive growth of SEI, alleviates volume expansion, and improves the cycle performance, capacity and first effect; second, it improves the conductivity of the negative electrode material and improves the capacity of the material; silicon-based negative electrode material precursors have the problem of poor conductivity. By improving indicators such as material conductivity, the contact of the conductive network during the cycle is guaranteed, and the generation of active substances such as "dead silicon" that are separated from the conductive network is reduced, thereby improving the cycle performance; third, the coating layer can provide a stable physical interface to inhibit excessive expansion of particles. At the same time, it can serve as a SEI growth skeleton to form a stable SEI layer, stabilize the solid-liquid interface, reduce the expansion effect, improve the cycle performance, and improve safety; fourth, the coating layer can further regulate the surface interface nanostructure. By adjusting the coating process parameters, the surface pore structure of the negative electrode material can be further optimized, the specific surface area can be regulated, and the rate and high and low temperature performance can be improved.
[0070] Step S5, using alkaline solution to remove nano-silicon dioxide from the negative electrode material matrix to obtain a negative electrode material, wherein the negative electrode material has the pore structure characteristics as described above, which will not be described in detail here.
[0071] Specifically, after adding alkaline solution to the negative electrode material matrix, the temperature is increased to perform stirring treatment; after the stirring is completed, suction filtration is performed, sieving is performed, and drying is performed at about 100° C. for about 24 h to 48 h; then, the particles are broken up and sieved to reduce agglomeration, and further vacuum drying is performed, and inert gas protection packaging is performed to form a finished negative electrode material with a surface interface structure.
[0072] In some embodiments, the alkaline solution can be obtained by dissolving lithium hydroxide in water, wherein a polar solvent, such as water, is selected as a more suitable reaction medium. The hydrolysis reaction dissolves the lithium hydroxide in water to form a solution, which can increase the reaction rate of silicon dioxide and lithium ions.
[0073] In some embodiments, the mass ratio of the negative electrode material matrix, water and lithium hydroxide can be 1:(1.5~5):(0.1~0.5). Reacting at this mass ratio can increase the reaction rate and accelerate the removal of nano-silicon dioxide.
[0074] In some embodiments, the reaction conditions may include: a temperature of 60°C to 90°C, a time of 30 min to 360 min, and a stirring speed of 1000 rpm to 3000 rpm. Increasing the reaction temperature and controlling the temperature between 60°C and 90°C to fully react at the above speed is conducive to improving the reaction efficiency.
[0075] Step S5 aims to wash away the nano-silicon dioxide with pores to form a negative electrode material with a surface pore structure. At the same time, the grading treatment can break up the powder agglomeration and control the negative electrode material to be within the optimized particle size range. Further drying can control the moisture content of the negative electrode material and reduce the influence of moisture on the electrochemical performance of the negative electrode material.
[0076] Compared with the prior art, the method for preparing the negative electrode material provided in the embodiment of the present application has the following beneficial effects:
[0077] 1. Use nano-silica with a particle size of less than or equal to 80nm, and ball-mill with the inner core in the presence of a surfactant, so that the nano-silica is deposited on the surface of the inner core to form a porous surface prototype. At the same time, optimizing the ball milling process can greatly reduce the ball-to-material ratio of ball milling, and effectively form a specific pore structure on the surface of the inner core. The pore structure has a first pore structure with a pore size of 2nm~20nm and a second pore structure with a pore size of 20nm~80nm. The distribution and volume proportion of the pore structure directly adjust the specific surface area of the negative electrode material. It has a specific pore structure distribution, adjusts the infiltration rate of the electrolyte of the negative electrode material, shortens the transmission path of lithium ions to the inner core, and improves the solid-liquid reaction efficiency of the negative electrode material surface, including the diffusion efficiency of the reaction ions at the interface, the ion diffusion flux and the diffusion depth, which is beneficial to improve the capacity, rate performance, structural stability, cycle efficiency and storage performance and electrochemical performance of the negative electrode material under high and low temperature conditions.
[0078] 2. A carbon coating layer is formed on the surface of the negative electrode material precursor by using a carbon deposition process, which optimizes the pore structure and forms a conductive network, thereby increasing the transmission rate of lithium ions in the negative electrode material, constructing an expansion buffer space, and reducing the deformation of the negative electrode material.
[0079] 3. This preparation method has simple process, low cost, easy mechanization and automation, which is conducive to the large-scale production of negative electrode materials and has excellent commercial prospects.
[0080] See also Figure 2As shown, the embodiment of the present application also provides an electrochemical device (such as a lithium-ion battery), the electrochemical device 100 includes the aforementioned negative electrode material or the negative electrode material prepared by the aforementioned preparation method. The electrochemical device 100 includes a positive electrode sheet 10, a negative electrode sheet 20, a separator 30 and an electrolyte 40, wherein the separator 30 is arranged between the positive electrode sheet 10 and the negative electrode sheet 20, and the negative electrode sheet 20 includes the aforementioned negative electrode material. The electrochemical device 100 is prepared using the aforementioned negative electrode material, which can control the wetting speed and reduce the rapid diffusion of the electrolyte inside the negative electrode material, resulting in side reactions with the active components. It also has a larger transmission interface, shortens the lithium ion diffusion path, thereby achieving an improvement in the battery rate performance and high and low temperature performance.
[0081] The above-mentioned negative electrode material and its preparation method and electrochemical device are further described below through specific examples.
[0082] Example 1
[0083] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0084] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce H2 for plasma treatment at a flow rate of 1500mL / min, control the pressure to 3000Pa, and treat for 30min. After the plasma treatment is completed, heat treatment is performed again under argon protection, the heat treatment temperature is 800℃, and the heat treatment time is 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped kernel.
[0085] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0086] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0087] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:4:0.1, and after adding the material to the alkali solution, start heating to 80°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0088] Example 2
[0089] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0090] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce a hydrogen-argon mixture with a mixing ratio of 1:1 and a flow rate of 2500mL / min. Control the pressure to 4000Pa, start the plasma generator to start the temperature reaction, and wait for the plasma light sphere to stably wrap the material. Immerse the lithium belt in the plasma light sphere and adjust the appropriate distance to keep the material in a solid state. The doping reaction time is about 24h; after the doping reaction is completed, remove the lithium belt and stop the Ar gas, continue to introduce H2 for plasma treatment, the flow rate is 1000mL / min, control the pressure to 600Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 800℃, and the heat treatment time is 12.0h. After the heat treatment is completed, it is broken up and sieved to obtain the doped kernel.
[0091] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0092] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0093] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:4:0.2, and after adding the material to the alkali solution, start heating to 75°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0094] Example 3
[0095] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0096] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, when the pressure in the chamber drops to 0.1Pa, introduce a hydrogen-argon mixture, the mixing ratio is 1:1, the flow rate is 2500mL / min, the pressure is controlled to 4000Pa, start the plasma generator to start the temperature reaction, wait for the plasma light sphere to stably wrap the material, immerse the magnesium ribbon in the plasma light sphere, adjust the appropriate distance, so that the material remains in a solid state, and the doping reaction time is about 24h; after the doping reaction is completed, remove the magnesium ribbon and stop the Ar gas, continue to introduce H2 for plasma treatment, the flow rate is 1000mL / min, the pressure is controlled to 600Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 800℃, and the heat treatment time is 12.0h. After the heat treatment is completed, it is broken up and sieved to obtain the doped kernel.
[0097] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0098] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0099] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:4:0.3, and after adding the material to the alkali solution, start heating to 75°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0100] Example 4
[0101] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0102] Step 2, weigh 1000g of kernel, put it into the plasma vacuum chamber, evacuate, when the pressure in the chamber drops to 0.1Pa, pass hydrogen and argon mixed gas, the mixing ratio is 1:1, the flow rate is 2500mL / min, control the pressure to 4000Pa, start the plasma generator to start the temperature reaction, wait for the plasma light sphere to stably wrap the material, pass gaseous titanium tetrachloride, the flow rate is set to 800mL / min, and the doping reaction time is about 24h; after the doping reaction is completed, stop passing titanium tetrachloride, continue to pass H2 for plasma treatment, the flow rate is 1000mL / min, control the pressure to 6000Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 800℃, and the heat treatment time is 12.0h. After the heat treatment is completed, it is broken up and sieved to obtain the doped kernel.
[0103] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0104] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0105] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:5:0.1, and after adding the material to the alkali solution, start heating to 90°C, treat for about 45 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0106] Example 5
[0107] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0108] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce H2 for plasma treatment at a flow rate of 3000mL / min, control the pressure to 6000Pa, and treat it for 30min. After the plasma treatment is completed, heat treatment is performed under argon protection at a temperature of 950°C and a heat treatment time of 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped kernel.
[0109] Step 3, weigh 1000g of the surface treated core, mix the doped core with water and lithium hydroxide in a ratio of 1:1:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:3. The ball milling time is 360min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0110] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce acetylene carbon source gas, the mixed coating source gas flow rate is 3000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon gas, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0111] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:4:0.1, and after adding the material to the alkali solution, start heating to 80°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0112] Example 6
[0113] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0114] Step 2, weigh 1000g of kernel, put it into the plasma vacuum chamber, evacuate, when the pressure in the chamber drops to 0.1Pa, pass hydrogen and argon mixed gas, the mixing ratio is 1:1, the flow rate is 1500mL / min, the pressure is controlled to 3000Pa, start the plasma generator to start the temperature reaction, wait for the plasma light sphere to stably wrap the material, pass gaseous titanium tetrachloride, the flow rate is set to 300mL / min, and the doping reaction time is about 1.0h; after the doping reaction is completed, stop passing titanium tetrachloride, continue to pass H2 for plasma treatment, the flow rate is 300mL / min, the pressure is controlled to 4000Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 400℃, and the heat treatment time is 3.0h. After the heat treatment is completed, it is broken up and sieved to obtain the doped kernel.
[0115] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0116] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0117] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:5:0.1, and after adding the material to the alkali solution, start heating to 90°C, treat for about 45 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0118] Example 7
[0119] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0120] Step 2, weigh 1000g of kernel, put it into the plasma vacuum chamber, evacuate, when the pressure in the chamber drops to 0.1Pa, pass hydrogen and argon mixed gas, the mixing ratio is 1:1, the flow rate is 1500mL / min, control the pressure to 3000Pa, start the plasma generator to start the temperature reaction, wait for the plasma light sphere to stably wrap the material, pass gaseous titanium tetrachloride, the flow rate is set to 600mL / min, and the doping reaction time is about 0.5h; after the doping reaction is completed, stop passing titanium tetrachloride, continue to pass H2 for plasma treatment, the flow rate is 300mL / min, control the pressure to 4000Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 400℃, and the heat treatment time is 3.0h. After the heat treatment is completed, break up and sieve to obtain the doped kernel.
[0121] Step 3, weigh 1000g of the doped core, mix the doped core with water and lithium hydroxide in a ratio of 1:3:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 60min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0122] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0123] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:5:0.1, and after adding the material to the alkali solution, start heating to 90°C, treat for about 45 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0124] Example 8
[0125] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0126] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce H2 for plasma treatment at a flow rate of 3000mL / min, control the pressure to 1000Pa, and treat for 30min. After the plasma treatment is completed, heat treatment is performed under argon protection at a temperature of 950°C and a heat treatment time of 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped kernel.
[0127] Step 3, weigh 1000g of the surface treated core, mix the doped core with water and lithium hydroxide in a ratio of 1:1:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:3. The ball milling time is 180min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0128] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce acetylene carbon source gas, the mixed coating source gas flow rate is 1500mL / min, the reaction time is about 24.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon gas, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0129] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:4:0.1, and after adding the material to the alkali solution, start heating to 80°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0130] Example 9
[0131] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0132] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce H2 for plasma treatment at a flow rate of 500mL / min, control the pressure to 1000Pa, and treat it for 30min. After the plasma treatment is completed, heat treatment is performed again under argon protection, the heat treatment temperature is 950℃, and the heat treatment time is 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped kernel.
[0133] Step 3, weigh 1000g of the surface treated core, mix the doped core with water and lithium hydroxide in a ratio of 1:1:0.15, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:3. The ball milling time is 180min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0134] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce acetylene carbon source gas, the mixed coating source gas flow rate is 300mL / min, the reaction time is about 48.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon gas, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0135] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:3:0.1, and after adding the material to the alkali solution, start heating to 80°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0136] Example 10
[0137] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0138] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce H2 for plasma treatment at a flow rate of 500mL / min, control the pressure to 1000Pa, and treat it for 30min. After the plasma treatment is completed, heat treatment is performed again under argon protection, the heat treatment temperature is 950℃, and the heat treatment time is 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped kernel.
[0139] Step 3, weigh 1000g of the surface treated core, mix the doped core with water and lithium hydroxide in a ratio of 1:1:0.1, add nano-silicon dioxide, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:0.3. The ball milling time is 30min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued. The drying temperature is 100℃ and the drying time is about 48h to obtain the negative electrode material precursor.
[0140] Step 4, weigh 1000g of the negative electrode material precursor, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce acetylene carbon source gas, the mixed coating source gas flow rate is 300mL / min, the reaction time is about 48.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon gas, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0141] Step 5, weigh 1000g of the negative electrode material matrix, and treat it with lithium hydroxide solvent, wherein the mass ratio of the negative electrode material matrix, water and lithium hydroxide is 1:3:0.1, and after adding the material to the alkali solution, start heating to 80°C, treat for about 30 minutes, and stir at a high speed of 3000r / min during the treatment process. After stirring, filter and sieve, control the particle size D50 between 5.0 and 6.0, and dry at about 80°C for about 24 hours. After drying, package under inert gas protection to obtain the negative electrode material.
[0142] Comparative Example 1
[0143] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0144] Step 2, weigh 1000g of the inner core, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0145] Step 3: further sieve the above-mentioned negative electrode material matrix to control the particle size D50 between 5.0 and 6.0, and further vacuum dry it for 24 hours after grading at a drying temperature of 80°C. After drying, vacuum package and store it under inert gas protection to obtain the negative electrode material.
[0146] Comparative Example 2
[0147] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0148] Step 2, weigh 1000g of the kernel, put it into the plasma vacuum chamber, evacuate it, and when the pressure in the chamber drops to 0.1Pa, introduce a hydrogen-argon mixture with a mixing ratio of 1:1 and a flow rate of 2500mL / min. Control the pressure to 4000Pa, start the plasma generator to start the temperature reaction, and wait for the plasma light sphere to stably wrap the material. Immerse the lithium belt in the plasma light sphere and adjust the appropriate distance to keep the material in a solid state. The doping reaction time is about 24h; after the doping reaction is completed, remove the lithium belt and stop the Ar gas, continue to introduce H2 for plasma treatment, the flow rate is 1000mL / min, control the pressure to 600Pa, and the treatment time is 30min. After the plasma treatment is completed, heat treatment is carried out again under argon protection, the heat treatment temperature is 800℃, and the heat treatment time is 12.0h. After the heat treatment is completed, it is broken up and sieved to obtain the doped kernel.
[0149] Step 3, weigh 1000g of the doped core, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0150] Step 4: further sieve the above-mentioned negative electrode material matrix to control the particle size D50 between 5.0 and 6.0, and further vacuum dry it for 24 hours after grading at a drying temperature of 80°C. After drying, vacuum package and store it under inert gas protection to obtain the negative electrode material.
[0151] Comparative Example 3
[0152] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0153] Step 2: Weigh 1000g of the core, put it into the plasma vacuum chamber, and evacuate it. When the pressure in the chamber drops to 0.1Pa, introduce H2 / Ar mixed gas (1:1) for plasma treatment at a flow rate of 3000mL / min, control the pressure to 8000Pa, and treat for 300min. After the plasma treatment, heat treatment is performed under argon protection at a temperature of 950℃ and a heat treatment time of 12.0h. After the heat treatment is completed, break it up and sieve it to obtain the doped core.
[0154] Step 3, weigh 1000g of the surface treated core, mix the doped core with water and lithium hydroxide in a ratio of 1:1:2, prepare ball milling slurry, and the mass ratio of the doped core to the ball milling beads is 1:1. The ball milling time is 360min, and after the ball milling is completed, centrifugal dehydration is performed, and vacuum drying is continued at a drying temperature of 100°C and a drying time of about 48h to obtain a negative electrode material precursor.
[0155] Step 4, weigh 1000g of the inner core, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 800℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0156] Step 3: further sieve the above-mentioned negative electrode material matrix to control the particle size D50 between 5.0 and 6.0, and further vacuum dry it for 24 hours after grading at a drying temperature of 80°C. After drying, vacuum package and store it under inert gas protection to obtain the negative electrode material.
[0157] Comparative Example 4
[0158] Step 1: SiO raw materials are graded to screen raw materials with D50 in the range of 5.0 μm to 6.0 μm. The screened SiO raw materials are cleaned with deionized water and alcohol ultrasonic for 60 min respectively, centrifuged and dehydrated after cleaning, and vacuum dried at 80° C. After drying for 24 h, they are broken up and sieved to obtain the core.
[0159] Step 2, weigh 1000g of the inner core, put it into the deposition chamber, introduce argon gas to remove oxygen, the flow rate is 4000mL / min, when the oxygen content is below 1ppm, start to heat up to 600℃, introduce methane and acetylene mixed carbon source gas (1:1), the mixed coating source gas flow rate is 2000mL / min, the reaction time is about 10.0h, after the reaction is completed, stop introducing the coating source gas sample, keep introducing argon, raise the temperature to 900℃ and continue processing for 3h, after the treatment is completed, clean and sieve to obtain the negative electrode material matrix.
[0160] Step 3: further sieve the above-mentioned negative electrode material matrix to control the particle size D50 between 5.0 and 6.0, and further vacuum dry it for 24 hours after grading at a drying temperature of 80°C. After drying, vacuum package and store it under inert gas protection to obtain the negative electrode material.
[0161] The negative electrode materials obtained in Examples 1-10 and Comparative Examples 1-4 were subjected to the following tests.
[0162] 1. Material properties of Examples 1-10 and Comparative Examples 1-4 were tested. The material properties test results of Examples 1-5 are shown in Table 1, the material properties test results of Examples 6-10 are shown in Table 2, and the material properties test results of Comparative Examples 1-4 are shown in Table 3.
[0163] (1) Particle size test: The test was completed using Matersizer 3000 in accordance with GB / T 19077-2016 method.
[0164] (2) Carbon content test: According to the technical method of GB / T 20123-2006, the sample is burned in a high-temperature furnace with oxygen to generate and release CO2 gas. This method is used to separate the carbon element from the metal elements and their compounds. The carbon content in the sample is calculated by measuring the CO2 content.
[0165] (3) Moisture test: According to the test method specified in GB / T 24533-2019, the water content in the negative electrode material is determined by Karl Fischer coulometric analysis. The water in the sample is evaporated at high temperature to become water vapor, which enters the electrolytic cell and reacts with the Karl Fischer reagent. The water content is determined by the potential change.
[0166] (4) Pore volume and specific surface area test: The BET method was used for testing. The pore volume in the pore size range of 2 nm to 20 nm was V1, the pore volume in the pore size range of 20 nm to 80 nm was V2, and the specific surface area of the negative electrode material was S.
[0167] (5) Test for doping element content: In accordance with GB / T 24533-2019, the test is carried out by ICP method. The specific method is to heat and digest in an open and normal pressure environment of a graphite digester, and use ICP-OES to test the content of each element.
[0168] (6) Oil absorption value test: The test is carried out in accordance with GB / T 3780.2-2017 "Carbon black Part 2: Determination of oil absorption value"; a certain mass of powder sample is placed in the mixing chamber, and then linseed oil is dripped onto the sample at a constant speed and stirred simultaneously with two motor-driven rotating wings. As the sample absorbs more linseed oil, the mixture changes from a free-flowing state to a semi-plastic agglomerate. During this process, the viscosity of the mixture gradually increases and a peak value appears. The measurement endpoint is the amount of linseed oil dripped when the torque generated by the change in viscosity characteristics reaches the set value or reaches a constant percentage of the maximum torque obtained from the torque curve, and the oil absorption value of the sample to linseed oil (mL / 100g) is calculated. The equipment is ASAHISOUKEN, Japan, and the equipment model is ASAHI S-500.
[0169] (7) Isothermal adsorption-desorption curve: The measurement was carried out in accordance with GB / T 19587-2017 "Determination of Specific Surface Area of Solid Substances by Gas Adsorption BET Method". A certain amount of sample was weighed and placed in a bubble tube dedicated to specific surface area. Nitrogen was purged at 300°C for a certain period of time at the degassing station. After degassing, the bubble tube containing the sample was cooled to room temperature. After weighing the actual mass of the sample, the bubble tube containing the sample was installed in the specific surface area and pore size analyzer. After inputting the sample mass, the specific surface area and pore size in the sample were measured. For samples below 0.01, quantitative gas injection was performed at 20 mL / g. For samples above 0.01, fixed-point gas injection was performed at intervals of 0.01 to 0.10, at intervals of 0.01; for samples above 0.01, at intervals of 0.02; for samples above 0.20, at intervals of 0.05. For degassing, the sample was degassed from 1.00 to 0.15, at intervals of 0.05. The equipment was ASAP2460 from McMerrittick, USA. The N2 isotherm linear plot was obtained from the test report, and the hysteresis loop area was calculated by integrating the adsorption-desorption hyperbola.
[0170]
[0171]
[0172]
[0173] In Examples 1-10, the negative electrode material is tested by the BET method. There is a pore distribution in the range of 2nm~20nm and between 20nm~80nm, and the pore volume in the pore size range of 2nm~20nm is V1, and the pore volume in the pore size range of 20nm~80nm is V2. The specific surface area of the negative electrode material is S, which satisfies 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g. However, (V1+V2) / S and V1 / V2 of Comparative Examples 1-4 are not fully satisfied, indicating that the pore structure distribution in Comparative Examples 1-4 is unreasonable. In terms of the pore volume distribution of the negative electrode material, satisfying the above distribution and specific surface contribution can effectively adjust the reaction of the interface; the reasonable combination of the first pore structure and the second pore structure in the negative electrode material can effectively adjust the infiltration speed of the electrolyte and the slurry, thereby improving the stability of the negative electrode material and the lithium ion transmission efficiency.
[0174] 2. Lithium-ion batteries were prepared using the negative electrode materials of Examples 1-10 and Comparative Examples 1-4, and the electrochemical performance of the lithium-ion batteries was tested. The results of the electrochemical performance tests are shown in Table 4.
[0175] The specific capacity of the negative electrode material and the first charge and discharge coulomb efficiency are assembled into button cells according to the equipment and methods of BTRTC / ZY / 01-020 "Button Cell Method Operation Instructions" of BTR Company. Among them, the counter electrode uses a metal lithium sheet, the separator is a PP-PE-PP composite film with a diameter of 19.2mm; the electrolyte component ratio is ethylene glycol carbonate (EC): propylene glycol carbonate (EMC): dimethyl carbonate (DMC) = 1:1:1, and the lithium salt (LiPF6) concentration is 1.05mol / L.
[0176] (1) Material capacity test: Use button cell charging and discharging equipment, 0.1C constant current charging to 10mV, then 0.02C constant current charging to 5mV, and 0.1C constant current discharging to 1.5V cutoff.
[0177] (2) Half-cell 50-week cycle test: using button cell charging and discharging equipment, in the first week, 0.1C discharge to 0.01V, 0.01C discharge to 0.01V, 0.01C discharge to 0.005V, 0.1C charge to 1.5V; in the second week, 0.2C discharge to 0.01V, 0.02C discharge to 0.01V, 0.02C discharge to 0.005V, 0.2C charge to 1.5V; in the third week, 0.5C discharge to 0 .01V, 0.05C discharge in equal steps to 0.01V, 0.05C discharge to 0.005V, 0.5C charge to 1.5V; from the 4th to the 50th week, 1C discharge to 0.01V, 0.1C discharge in equal steps to 0.01V, 0.1C discharge to 0.005V, 1C charge to 1.5V; in the 51st week, 0.1C discharge to 0.01V, 0.01C discharge in equal steps to 0.01V, 0.01C discharge to 0.005V.
[0178] (3) Full battery performance test: The negative electrode material is mixed with graphite to achieve a standard capacity of 450 mAh / g. The capacity retention rate test is carried out at high temperature (60°C). Specifically, the charge and discharge test is carried out at a current density of 0.2C (2.75-4.2V); the rate performance test is carried out at three different current densities: 1C / 0.5C, 2C / 0.5C and 3C / 0.5C.
[0179]
[0180] The batteries prepared with the negative electrode materials of Examples 1-10 of the present application have greatly improved capacity and first efficiency compared with Comparative Examples 1-4 of the same type of cores, and the cycle performance and high and low temperature performance are maintained at a good level. This is because the negative electrode materials in Examples 1-10 have a suitable nanoscale pore structure and a uniform carbon coating layer, which effectively reduces the surface side reactions in the preparation of the battery, reduces the consumption of electrolyte and the loss of active silicon and active lithium, and improves the capacity and first efficiency of the battery; secondly, during the preparation of the negative electrode material, when the negative electrode material matrix is treated with alkaline solution, part of the oxide on the surface of the negative electrode material is dissolved, the active oxygen content and inactive components are reduced, the loss of first efficiency is avoided, and the improvement of the electrochemical performance of the battery is achieved.
[0181] Among them, the capacity and first effect of the battery prepared using the negative electrode materials of Example 1 (compared with non-doped negative electrode materials such as Example 5, Examples 8-10, Comparative Example 1, Comparative Example 3 and Comparative Example 4) and Example 2 (compared with Comparative Example 2 of the same type of doped negative electrode material) are significantly improved. This is because the doping elements of the negative electrode materials in Examples 1 and 2 improve the electrochemical properties of the negative electrode materials, including increasing the storage capacity of lithium ions, increasing electrical conductivity, improving structural stability and reducing electrode polarization, thereby improving the capacity and first effect of the battery.
[0182] In addition, the pore structure of the negative electrode material optimizes the ion diffusion environment of the reaction interface. During the processing, the battery prepared with the negative electrode material in Comparative Example 2 will produce gas after being placed for 24 hours. This is because the polar solvent quickly infiltrates and enters the interior of the negative electrode material during the slurry mixing process of the negative electrode material in Comparative Example 2 in the water system (polar solvent). The active material and the polar solvent quickly undergo an oxidation-reduction reaction, which destroys the stability of the slurry and causes gas production. At the same time, the oxidation-reduction reaction will change the acid-base environment of the slurry, destroy the solubility of the dispersant, and cause the negative electrode material to agglomerate. Correspondingly, the battery prepared with the negative electrode material of Example 2 has good slurry stability, indicating that the optimization of the pore structure can effectively improve the degree of reaction at the interface, inhibit the occurrence of side reactions, and thus improve the stability of the negative electrode material.
[0183] Finally, the high and low temperature capacity is exerted, and the test results of rate performance show that the battery prepared by the negative electrode material in Examples 1-10 is significantly improved in terms of high and low temperature performance and rate performance. For Comparative Example 2 with a small (V1+V2) / S value, that is, a low pore structure depth, because the electrolyte infiltration speed is too fast, the electrolyte quickly enters the interior of the negative electrode material, causing excessive oxidation of the active material and excessive gas production, so its rate and high and low temperature performance are weaker than the battery prepared by the negative electrode material in Examples 1-10 of the present application; and the (V1+V2) / S value is large, that is, the comparative example 1 with a large pore structure depth, because the core diffusion path is too long, the electrolyte infiltration speed decreases, resulting in low lithium ion transfer efficiency, which also causes poor battery rate and low temperature performance; in Comparative Example 3, the specific surface area S of the negative electrode material is too large, resulting in an increase in the impedance of the prepared battery, and a significant decrease in thermal stability; and in Comparative Example 4, the negative electrode material V1 / V2 is too large, that is, the first pore structure accounts for too high a proportion, resulting in a decrease in the lithium ion diffusion rate, affecting the performance of the prepared battery. The negative electrode materials in Examples 1-10 have a reasonable pore structure and specific surface area, and thus have a suitable pore structure depth value, thereby achieving improvements in battery rate and high and low temperature performance.
[0184] It can be seen from this that the pore structure of the negative electrode material in the embodiment of the present application can control the surface reaction efficiency of the negative electrode material, affect the interface reaction process and reaction details, including the diffusion efficiency of the reaction ions at the appropriate interface, the ion diffusion flux and the diffusion depth, thereby improving the rate performance and high and low temperature performance of the negative electrode material.
[0185] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A negative electrode material, characterized in that: The negative electrode material comprises a silicon-containing material and a carbon-containing material, wherein the negative electrode material has a pore structure, and the pore structure has the following distribution characteristics: The negative electrode material is tested by the BET method, and it is found that the negative electrode material has a first pore structure with a pore size of 2nm~20nm and a second pore structure with a pore size of 20nm~80nm, the pore volume of the first pore structure is V1, the pore volume of the second pore structure is V2, and the specific surface area of the negative electrode material is S, wherein 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g,0.5cm 3 / g≥V1≥0.001cm 3 / g,5.0cm 3 / g≥V2≥0.01cm 3 / g.
2. The negative electrode material according to claim 1, characterized in that The negative electrode material satisfies at least one of the following conditions: (1) The particle size D50 of the negative electrode material is in the range of 2.0 μm to 15.0 μm; (2) The oil absorption value of the negative electrode material is 25 mL / 100 g to 85 mL / 100 g; (3) The pH value of the negative electrode material is 7.5-12.0; (4) The integral area of the isothermal adsorption hysteresis loop of the negative electrode material is 1.0×10 -4 ~5.0×10 -2 ; (5) The pore size range of the negative electrode material is 0.5nm~300nm.
3. The negative electrode material according to claim 1, characterized in that The proportion of each material in the negative electrode material satisfies at least one of the following conditions: (1) The total mass of the silicon-containing material and the carbon-containing material accounts for 40% to 97.5% of the total mass of the negative electrode material; (2) The mass of the carbon-containing material accounts for 1.5% to 45.5% of the total mass of the negative electrode material.
4. The negative electrode material according to claim 1, characterized in that The negative electrode material further includes a doping element, and the doping element satisfies at least one of the following conditions: (1) The doping element includes at least one of hydrogen, oxygen, lithium, magnesium, aluminum, nitrogen, phosphorus, sulfur, boron, fluorine, molybdenum, sodium, potassium, calcium, titanium, niobium, lanthanum, tin, selenium and cerium; (2) The content of the doping element in the negative electrode material is 25 ppm to 120,000 ppm.
5. A method for preparing a negative electrode material, characterized in that: include: Screening the silicon source by particle size, cleaning and drying to obtain the core; The core is added to a deionized water solution of a surfactant, and nano-silicon dioxide and ball milling beads are added for ball milling to obtain a negative electrode material precursor, wherein the particle size of the nano-silicon dioxide is less than or equal to 80 nm, the particle size of the core is greater than the particle size of the nano-silicon dioxide, the surfactant includes an alkaline solution or an organic oxidant, and the mass ratio of the core, the surfactant, deionized water, nano-silicon dioxide and ball milling beads is 1: (0.1-0.5): (1-5): (0.01-0.05): (0.3-2); Carbon coating the negative electrode material precursor to obtain a negative electrode material matrix; and The negative electrode material matrix is subjected to alkaline solution to remove the nano-silicon dioxide to obtain the negative electrode material, wherein the negative electrode material has a pore structure, and the pore structure has the following distribution characteristics: The negative electrode material is tested by the BET method, and it is found that the negative electrode material has a first pore structure with a pore size of 2nm~20nm and a second pore structure with a pore size of 20nm~80nm, the pore volume of the first pore structure is V1, the pore volume of the second pore structure is V2, and the specific surface area of the negative electrode material is S, wherein 0.1μm≥(V1+V2) / S≥0.01μm, 0.8≥V1 / V2≥0.01, 10.0m 2 / g≥S≥0.1m 2 / g.
6. The preparation method according to claim 5, characterized in that: In the preparation method, at least one of the following conditions is met: (1) In the ball milling step, the ball milling time is 30 min to 90 min; (2) In the step of removing the nano-silicon dioxide, the alkaline solution is obtained by dissolving lithium hydroxide in water, and the mass ratio of the negative electrode material matrix, the water and the lithium hydroxide is 1: (1.5-5): (0.1-0.5); (3) In the step of removing the nano-silicon dioxide, the reaction conditions include: temperature of 60°C to 90°C, time of 30 min to 360 min, and stirring speed of 1000 rpm to 3000 rpm.
7. The preparation method according to claim 5, characterized in that: In the carbon coating step, at least one of the following conditions is met: (1) The carbon coating comprises placing the negative electrode material precursor in a reaction device and introducing a coating source gas for chemical vapor deposition, wherein the coating source gas comprises at least one of methane, ethane, acetylene, ethylene and propane, and the flow rate of the coating source gas is 300 mL / min to 3000 mL / min; (2) The coating temperature is 450℃~1000℃, and the coating time is 1.0h~48.0h.
8. The preparation method according to claim 5, characterized in that: Before the step of adding the core into a deionized water solution of a surfactant, and adding nano-silicon dioxide and ball milling beads for ball milling to obtain a negative electrode material precursor, the preparation method further comprises: The core is doped with elements by plasma, and the doped elements include at least one of hydrogen, oxygen, lithium, magnesium, aluminum, nitrogen, phosphorus, sulfur, boron, fluorine, molybdenum, sodium, potassium, calcium, titanium, niobium, lanthanum, tin, selenium and cerium.
9. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material comprises the negative electrode material as described in any one of claims 1 to 4 or the negative electrode material prepared by the preparation method as described in any one of claims 5 to 8.