Water-based adhesive and preparation method thereof and carbon-coated aluminum foil

By performing acid-induced polymerization at the set pH value, an aqueous binder with narrow molecular weight distribution and high end group fidelity was prepared, which solved the corrosion problems of aluminum substrates in extreme pH environments and exogenous initiators. Safety hazards improve the performance and production safety of lithium-ion batteries.

CN118658995BActive Publication Date: 2024-11-26GUANGZHOU LUSHAN NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111112.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In the prior art, aluminum substrates are prone to corrosion under extreme pH environments, resulting in unstable performance of lithium-ion batteries, and exogenous thermal radical initiators have safety hazards and heterogeneity problems in industrial production, making it difficult to control molecular weight distribution. and terminal group fidelity.

Method used

Using the preparation method of water-based binder, acid-induced polymerization is carried out by a certain proportion of monomers at a set pH value to obtain a water-based binder with narrow molecular weight distribution and high end group fidelity, which is used to prepare carbon coating. Aluminum foil avoids the use of light or thermal radical initiators.

Benefits of technology

It realizes high chemical stability and excellent dispersion performance of water-based binders, improves the bonding strength and dispersion of lithium-ion battery active materials, is suitable for the preparation of carbon-coated aluminum foil, and solves the safety hazards of aluminum corrosion and industrial production. question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of secondary batteries, and in particular to a water-based binder, a preparation method thereof, and a carbon-coated aluminum foil. The water-based binder is mainly prepared from the following components by weight: 60 to 80 parts of acrylamide monomers, 10 to 20 parts of unsaturated acid monomers, 10 to 20 parts of acrylate monomers, 0.1 to 3 parts of chain transfer agents, 100 to 400 parts of water, and a pH regulator; the amount of the pH regulator is adjusted so that the pH value of the mixed system of each component is 1 to 6. The present invention can obtain a water-based binder with a narrow molecular weight distribution and high terminal group fidelity by acid-initiated polymerization at a set pH value, and has both excellent dispersibility and bonding properties, and can be used for the preparation of slurry of active materials for lithium-ion batteries, and is particularly suitable for the preparation of carbon-coated aluminum foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of secondary batteries, in particular to a water-based binder and a preparation method thereof, and a carbon-coated aluminum foil. Background Art

[0002] As a traditional cathode current collector, aluminum substrate has a very high reduction potential value. Aluminum will oxidize rapidly in the presence of oxygen to form a very thin aluminum oxide layer (2nm). This oxide layer forms a chemical bond with the surface and acts as a protective layer to prevent further oxidation, making it corrosion-resistant and stable. However, when exposed to extreme pH environments, the protective layer will break, and direct contact between aluminum and cathode slurry will form soluble aluminum species, which will corrode the cathode active material, especially at high temperatures. The corrosion process is exacerbated. In addition, the solid products produced by the corrosion process may increase the contact resistance between the active material and the current collector, and the soluble products produced may contaminate the electrolyte. To date, solving the problem of aluminum corrosion that occurs during the operation of lithium-ion batteries at high potentials has become the key to ensuring efficient and stable operation of the battery.

[0003] In the prior art, a layer of active material is usually coated on the surface of the current collector to improve the electrode performance. The commonly used carbon-coated aluminum foil can effectively solve the corrosion problem of aluminum foil contacting the electrode slurry and occurring under high potential. In the carbon-coated current collector, the polymer binder provides functional groups to connect the electrode coating, the carbon coating layer and the bottom aluminum foil. The polymer binder plays a key role in improving the adhesion between the electrode and the current collector and maintaining its capacity.

[0004] In the industrial controlled synthesis of existing binders, exogenous thermal free radical initiators are usually used to initiate polymerization, but exogenous initiators also bring certain limitations. First, the use of free radical initiators will lead to heterogeneity of terminal groups and chain termination, resulting in higher dispersion and impure copolymers. In addition, the storage and use of exogenous initiators have certain safety risks in industrial production.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] An object of the present invention is to provide a water-based adhesive that does not require an exogenous initiator, has a narrow molecular weight distribution and high terminal group fidelity, and has excellent dispersibility and bonding properties.

[0007] Another object of the present invention is to provide a method for preparing the aqueous binder.

[0008] Another object of the present invention is to provide a carbon-coated aluminum foil.

[0009] In order to achieve the above-mentioned object of the present invention, the present invention provides a water-based binder, which is mainly prepared by the following components in parts by weight:

[0010] 60-80 parts of acrylamide monomers, 10-20 parts of unsaturated acid monomers, 10-20 parts of acrylate monomers, 0.1-3 parts of chain transfer agent, 100-400 parts of water and a pH regulator; the amount of the pH regulator is adjusted so that the pH value of the mixed system of each component is 1-6.

[0011] In a specific embodiment of the present invention, the amount of the pH adjuster is adjusted so that the pH value of the mixed system of each component is 2-5.

[0012] In a specific embodiment of the present invention, the acrylamide monomer includes at least one of acrylamide, methacrylamide, N-hydroxymethyl methacrylamide, diacetone acrylamide, N,N-dimethyl acrylamide, tert-butyl acrylamide, N-methoxymethyl acrylamide, N-hydroxyethyl acrylamide and acryloyl morpholine.

[0013] In a specific embodiment of the present invention, the acrylamide monomers include N,N-dimethylacrylamide and acrylamide. Further, in the acrylamide monomers, the mass ratio of the N,N-dimethylacrylamide to the acrylamide is (1-2):1.

[0014] In a specific embodiment of the present invention, the mass percentage of the acrylamide monomers in all monomers is ≥ 70%.

[0015] In a specific embodiment of the present invention, the unsaturated acid monomer includes at least one of an unsaturated carboxylic acid monomer or an inorganic salt thereof, and an unsaturated sulfonic acid monomer or an inorganic salt thereof. Further, the unsaturated carboxylic acid monomer includes at least one of (meth)acrylic acid, maleic anhydride, itaconic acid and fumaric acid; the unsaturated sulfonic acid monomer includes at least one of styrene sulfonic acid, allyl sulfonic acid and methacrylic sulfonic acid.

[0016] In a specific embodiment of the present invention, the acrylic acid ester monomer includes at least one of alkyl (meth)acrylate, alkylhydroxy (meth)acrylate, polyethylene glycol methyl ether acrylate, di(hydroxyethyl) phosphate, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and di[2-(methacryloyloxy)ethyl]phosphate.

[0017] In a specific embodiment of the present invention, the pH adjuster includes at least one of sulfuric acid, sulfonic acid, phosphoric acid, hydrochloric acid, acetic acid, citric acid, lactic acid, oxalic acid and malic acid.

[0018] In a specific embodiment of the present invention, the chain transfer agent includes a mercaptan chain transfer agent.

[0019] Another aspect of the present invention provides a method for preparing any of the above-mentioned water-based adhesives, comprising the following steps: in a protective atmosphere, the components are uniformly mixed in proportion, reacted at 25-90° C., discharged, and subjected to neutralization treatment.

[0020] Another aspect of the present invention provides a carbon-coated aluminum foil, comprising an aluminum foil substrate and a carbon coating disposed on the surface of the aluminum foil substrate, wherein the carbon coating is made of a slurry containing any one of the above-mentioned aqueous binders.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention adopts monomers of a certain ratio, does not require light or thermal free radical initiators, and can obtain a water-based adhesive with a narrow molecular weight distribution and high terminal group fidelity through acid-initiated polymerization at a set pH value; the improvement of the terminal group fidelity can improve the interaction between the adhesive and the surface of a specific material, thereby improving the bonding strength, and at the same time helps the adhesive maintain high chemical stability;

[0023] (2) The aqueous binder of the present invention has excellent dispersibility and bonding properties, and can be used for preparing slurry of active materials for lithium-ion batteries, and is particularly suitable for preparing carbon-coated aluminum foil. DETAILED DESCRIPTION

[0024] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0025] In one aspect, the present invention provides an aqueous binder, which is mainly prepared from the following components by weight:

[0026] 60-80 parts of acrylamide monomers, 10-20 parts of unsaturated acid monomers, 10-20 parts of acrylate monomers, 0.1-3 parts of chain transfer agent, 100-400 parts of water and pH regulator; the amount of pH regulator is adjusted so that the pH value of the mixed system of each component is 1-6.

[0027] The present invention adopts monomers of a certain ratio, does not need light or heat free radical initiators, and can obtain a water-based adhesive with narrow molecular weight and high terminal group fidelity by acid-initiated polymerization at a set pH value. The improvement of terminal group fidelity can improve the interaction between the adhesive and the surface of a specific material, thereby improving the bonding strength and helping the adhesive to maintain high chemical stability. The raw material components of the water-based adhesive of the present invention do not include light or heat free radical initiators.

[0028] The aqueous binder of the present invention starts the polymerization reaction under the action of acid, and the acid can accelerate the reaction rate, so as to obtain a high molecular weight homopolymer or a high molecular weight block copolymer with less termination. The aqueous binder of the present invention has a long chain length. When mixed with other components to prepare a slurry, it is adsorbed on the surface of particles in the slurry, so that the repulsive force between the particles is increased, thereby reducing the accumulation of particles in the slurry, which is beneficial to improving the dispersibility and reducing the viscosity of the slurry; at the same time, in conjunction with the selection of the monomer type of the present invention, while obtaining a relatively high molecular weight polymer, the solubility and bonding performance can also be guaranteed.

[0029] In the aqueous binder of the present invention, the amounts of the components in parts by weight can be as follows:

[0030] The amount of acrylamide monomers can be 60 parts, 65 parts, 70 parts, 75 parts, 80 parts or any two of them;

[0031] The amount of the unsaturated acid monomer can be 10 parts, 12 parts, 15 parts, 18 parts, 20 parts or a range consisting of any two of them;

[0032] The amount of the acrylic acid ester monomer can be 10 parts, 12 parts, 15 parts, 18 parts, 20 parts or any two of them;

[0033] The amount of the chain transfer agent can be 0.1 part, 0.2 part, 0.5 part, 0.8 part, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts or any two of them;

[0034] The amount of water can be 100 parts, 150 parts, 200 parts, 250 parts, 300 parts, 350 parts, 400 parts or a range consisting of any two of them;

[0035] The amount of pH adjuster used needs to meet the requirement of adjusting the pH value of the mixed system after mixing the components for preparing the aqueous binder to 1-6. For example, the pH value can be 1, 2, 3, 4, 5, 6 or a range consisting of any two of them.

[0036] In a specific embodiment of the present invention, the amount of the pH adjuster is adjusted so that the pH value of the mixed system of each component is 1 to 5 or 2 to 5 or 1 to 3. The present invention further adjusts the pH value of the mixed system within the above range, which helps to improve the conversion rate of the polymerization reaction and obtain a water-based adhesive with excellent dispersibility and bonding properties.

[0037] In a specific embodiment of the present invention, the acrylamide monomer includes at least one of acrylamide, methacrylamide, N-hydroxymethyl methacrylamide, diacetone acrylamide, N,N-dimethyl acrylamide, tert-butyl acrylamide, N-methoxymethyl acrylamide, N-hydroxyethyl acrylamide and acrylamide morpholine. Further, the acrylamide monomer includes at least one of acrylamide, methacrylamide, N,N-dimethyl acrylamide and acrylamide morpholine.

[0038] In a specific embodiment of the present invention, the acrylamide monomers include N,N-dimethylacrylamide and acrylamide. Further, in the acrylamide monomers, the mass ratio of N,N-dimethylacrylamide to acrylamide is (1-2):1.

[0039] For example, in different embodiments, the mass ratio of N,N-dimethylacrylamide to acrylamide in the acrylamide monomers can be 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1 or any two of them. The composition of the acrylamide monomers is as above, which can further improve the initiation conversion rate under acidic conditions.

[0040] In a specific embodiment of the present invention, the mass percentage of acrylamide monomers in all monomers is ≥ 70%. Among them, all monomers refer to acrylamide monomers, unsaturated acid monomers and acrylate monomers. For example, in different embodiments, the mass percentage of acrylamide monomers in all monomers can be 70%, 72%, 75%, 78%, 80% or a range consisting of any two thereof. On the one hand, the amount of acrylamide monomers used within the above range is conducive to achieving acid-initiated polymerization at a set pH value and improving the conversion rate; on the other hand, the appropriate amount of acrylamide monomers is more conducive to improving the dispersibility of the water-based adhesive while taking into account the bonding performance.

[0041] In a specific embodiment of the present invention, the unsaturated acid monomers include unsaturated carboxylic acid monomers or inorganic salts thereof, unsaturated sulfonic acid monomers or inorganic salts thereof. Further, the unsaturated carboxylic acid monomers include at least one of (meth) acrylic acid, maleic anhydride, itaconic acid and fumaric acid; the unsaturated sulfonic acid monomers include at least one of styrene sulfonic acid, allyl sulfonic acid and methacrylic acid sulfonic acid. The corresponding inorganic salt may be a sodium salt, etc.

[0042] By introducing a certain amount of unsaturated carboxylic acid monomers or their inorganic salts and / or unsaturated sulfonic acid monomers or their inorganic salts, the water-based adhesive can be given a certain charge, and the charge force can be used to prevent the molecular chains of the water-based adhesive from being excessively entangled. On the one hand, this improves the dispersibility, and on the other hand, it provides additional action sites to improve the bonding performance.

[0043] In a specific embodiment of the present invention, the acrylic acid ester monomer includes at least one of alkyl (meth)acrylate, alkylhydroxy (meth)acrylate, polyethylene glycol methyl ether acrylate phosphate di(hydroxyethyl acrylate), 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and di[2-(methacryloyloxy)ethyl]phosphate.

[0044] The alkyl (meth)acrylate may include but is not limited to lauryl methacrylate; the alkyl hydroxy (meth)acrylate may include but is not limited to 3-hydroxy-1-adamantyl methacrylate.

[0045] The water-based adhesive prepared by the present invention by combining various monomers can form an effective three-dimensional cross-linked structure during the preparation of slurry blending and the coating process, thereby improving the bonding performance while taking into account the high dispersion performance.

[0046] In a specific embodiment of the present invention, the pH regulator includes at least one of sulfuric acid, sulfonic acid, phosphoric acid, hydrochloric acid, acetic acid, citric acid, lactic acid, oxalic acid and malic acid. Further, the pH regulator includes at least one of sulfuric acid, sulfonic acid, phosphoric acid, hydrochloric acid, acetic acid and oxalic acid.

[0047] In actual operation, the pH adjuster can be added in the form of an aqueous solution to avoid excessive acidity leading to poor stability of the mixed system. For example, taking sulfuric acid as an example, its mass fraction can be 0.1% to 5%, but it is not limited to this and can be adjusted according to actual conditions.

[0048] In a specific embodiment of the present invention, the chain transfer agent includes a thiol chain transfer agent. The thiol chain transfer agent includes aliphatic thiols, such as n-dodecyl mercaptan, etc. The type of chain transfer agent is not limited thereto, and may also include at least one of 2-(((butylthio)carboxythio)thio)propionic acid, 3-((((1-carboxyethyl)thio)carboxythio)thio)propionic acid, methyl 2-[methyl (4-pyridyl)aminomethylthioylthio]propionic acid, 2-cyanopropane-2-yl N-methyl-N-(4-pyridyl)aminodithiocarboxylate, 2-cyano-2-propylbenzodisulfate, isopropanol, inorganic phosphate, octanol, 3-chloro-2-hydroxypropyltriethylammonium chloride (CTA), 2,4-diphenyl-4-methyl-1-pentene (TPMS), and α-methylstyrene linear dimer (AMSD).

[0049] In a specific embodiment of the present invention, the amount of the chain transfer agent is 0.5 wt% to 3 wt% of all monomers, preferably 1.5 wt% to 2.5 wt%.

[0050] In a specific embodiment of the present invention, the number average molecular weight of the water-based binder is 40,000 to 70,000; and the molecular weight distribution width index of the water-based binder is 1.1 to 2.1.

[0051] For example, in different embodiments, the number average molecular weight of the aqueous binder can be 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000 or a range consisting of any two of them; the molecular weight distribution width index Mw / Mn of the aqueous binder can be 1.1, 1.2, 1.5, 1.6, 1.8, 2, 2.1 or a range consisting of any two of them.

[0052] In some embodiments of the present invention, the number average molecular weight of the aqueous binder is 60,000 to 65,000; and the molecular weight distribution width index of the aqueous binder is 1.1 to 1.35.

[0053] Another aspect of the present invention provides a method for preparing any of the above-mentioned water-based binders, comprising the following steps: in a protective atmosphere, the components are uniformly mixed in proportion, reacted at 25-90° C., discharged, and subjected to neutralization treatment.

[0054] In actual operation, nitrogen can be introduced into the reaction system for deoxygenation treatment so that the reaction is carried out under a protective atmosphere. During the reaction process, stirring operation is performed and the reaction temperature is regulated within a limited range.

[0055] The neutralization treatment may include: adding alkali solution to the material to adjust the pH to 7-8, such as 7. The alkali solution may include ammonia water, sodium hydroxide aqueous solution, calcium hydroxide aqueous solution, magnesium hydroxide aqueous solution, etc. For example, the mass fraction of ammonia water may be 1%-15%, the mass fraction of sodium hydroxide aqueous solution may be 0.1%-10%, and the calcium hydroxide aqueous solution may be a saturated calcium hydroxide aqueous solution.

[0056] In a specific embodiment of the present invention, after the reaction, the product is vacuumed to remove residual monomers, and then the temperature is lowered and the product is discharged.

[0057] In a specific embodiment of the present invention, the uniform mixing includes: adding acrylamide monomers, unsaturated acid monomers, acrylate monomers and chain transfer agents into water, and then adding a pH adjuster to adjust the pH value of the mixed system to 1-6.

[0058] In a specific embodiment of the present invention, the reaction time is 1 to 96 hours, such as 12 to 72 hours. For example, in different embodiments, the reaction time can be 1 hour, 5 hours, 12 hours, 18 hours, 24 hours, 48 ​​hours, 60 hours, 72 hours, etc.

[0059] The present invention provides use of any one of the above aqueous binders in preparing carbon-coated aluminum foil.

[0060] Another aspect of the present invention provides a carbon-coated aluminum foil, comprising an aluminum foil substrate and a carbon coating disposed on the surface of the aluminum foil substrate, wherein the carbon coating is made of a slurry containing any one of the above-mentioned aqueous binders.

[0061] In actual operation, the slurry can be adjusted according to the actual carbon coating composition. For example, the slurry may include the following components by mass percentage: 6% aqueous binder (in terms of solid content), 6% conductive carbon black and 88% water. When the aqueous binder of the present invention is used, water is used to adjust the solid content of the aqueous binder to 15% to 25%.

[0062] Example 1

[0063] This embodiment provides a method for preparing a water-based binder, comprising the following steps:

[0064] (1) According to weight, 75 parts of acrylamide monomer, 10 parts of unsaturated acid monomer, 15 parts of acrylate monomer, 2 parts of chain transfer agent, 300 parts of deionized water and an appropriate amount of pH adjuster are weighed respectively; wherein the acrylamide monomer is N,N-dimethylacrylamide and acrylamide in a mass ratio of 1.5:1, the unsaturated acid monomer is acrylic acid, the acrylate monomer is polyethylene glycol (480) methyl ether acrylate (CAS: 32171-39-4), the chain transfer agent is dodecyl mercaptan, and the pH adjuster is a sulfuric acid aqueous solution with a mass fraction of 1wt%.

[0065] (2) Under a nitrogen atmosphere, deionized water is added to a reactor and stirred to fully remove oxygen; then acrylamide monomers, unsaturated acid monomers, acrylate monomers, and a chain transfer agent are added to the reactor, followed by a pH adjuster to adjust the pH of the mixture in the reactor to 3.0; under a nitrogen atmosphere, the temperature is raised to 70°C, and the reaction is stirred at 350 rpm for 30 hours, the temperature is lowered, and some residual monomers are removed by vacuum, and a calcium hydroxide solution is added to adjust the pH to 7 to obtain a water-based binder.

[0066] Example 2

[0067] This example is based on the preparation method of Example 1, with the only difference being that in step (2), the amount of pH adjuster used is different.

[0068] In step (2) of this embodiment, a pH adjuster is added to adjust the pH of the mixture in the reaction kettle to 1.0.

[0069] Example 3

[0070] This example is based on the preparation method of Example 1, with the only difference being that in step (2), the amount of pH adjuster used is different.

[0071] In step (2) of this embodiment, a pH adjuster is added to adjust the pH of the mixture in the reaction kettle to 2.0.

[0072] Example 4

[0073] This example is based on the preparation method of Example 1, with the only difference being that in step (2), the amount of pH adjuster used is different.

[0074] In step (2) of this embodiment, a pH adjuster is added to adjust the pH of the mixture in the reaction kettle to 5.0.

[0075] Example 5

[0076] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the composition of the acrylamide monomer is different.

[0077] In step (1) of this embodiment, the acrylamide monomers are N,N-dimethylacrylamide and acrylamide in a mass ratio of 1:1.

[0078] Example 6

[0079] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the composition of the acrylamide monomer is different.

[0080] In step (1) of this embodiment, the acrylamide monomers are N,N-dimethylacrylamide and acrylamide in a mass ratio of 2:1.

[0081] Example 7

[0082] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the composition of the acrylamide monomer is different.

[0083] In step (1) of this embodiment, the acrylamide monomer is N,N-dimethylacrylamide.

[0084] Example 8

[0085] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the composition of the acrylamide monomer is different.

[0086] In step (1) of this embodiment, the acrylamide monomer is acrylamide.

[0087] Example 9

[0088] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the amounts of the monomers used are different.

[0089] In step (1) of this embodiment, the monomers include 65 parts of acrylamide monomers, 14 parts of unsaturated acid monomers, and 21 parts of acrylate monomers.

[0090] Example 10

[0091] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the amount of chain transfer agent used is different.

[0092] In step (1) of this embodiment, the amount of chain transfer agent used is 0.5 parts.

[0093] Embodiment 11

[0094] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the amount of chain transfer agent used is different.

[0095] In step (1) of this embodiment, the amount of chain transfer agent used is 3 parts.

[0096] Example 12

[0097] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the type of acrylate monomer is different.

[0098] In step (1) of this embodiment, the acrylic acid ester monomer is 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate.

[0099] Comparative Example 1

[0100] Comparative Example 1 refers to the preparation method of Example 1, except that in step (2), the type of unsaturated acid monomer is different and the amount of pH adjuster is different.

[0101] In Comparative Example 1, an equal weight of sodium acrylate is used to replace the acrylic acid in Example 1. In step (2) of Comparative Example 1, a pH adjuster is added to adjust the pH of the mixture in the reaction kettle to 6.5.

[0102] Comparative Example 2

[0103] Comparative Example 2 refers to the preparation method of Example 1, except that in step (2), the type and amount of the pH adjuster are different.

[0104] In step (2) of comparative example 2, a pH adjuster is added to adjust the pH of the mixture in the reaction kettle to 7.0; the pH adjuster is a sodium hydroxide aqueous solution with a mass fraction of 0.1%.

[0105] Comparative Example 3

[0106] Comparative Example 3 refers to the preparation method of Example 1, except that in step (2), the type and amount of the pH adjuster are different.

[0107] In step (2) of Comparative Example 3, a pH adjuster was added to adjust the pH of the mixture in the reaction kettle to 9.0; the pH adjuster was a sodium hydroxide aqueous solution with a mass fraction of 0.1%.

[0108] Comparative Example 4

[0109] Comparative Example 4 refers to the preparation method of Example 1, except that in step (1), the amounts of each monomer used are different.

[0110] In step (1) of Comparative Example 4, the monomers include 40 parts of acrylamide monomers, 30 parts of unsaturated acid monomers, and 30 parts of acrylate monomers.

[0111] Comparative Example 5

[0112] Comparative Example 5 provides a method for preparing a water-based binder, comprising the following steps:

[0113] (1) According to weight, 75 parts of acrylamide monomer, 10 parts of unsaturated acid monomer, 15 parts of acrylate monomer, 2 parts of chain transfer agent, 300 parts of deionized water and 1 part of ammonium persulfate are weighed respectively; wherein the acrylamide monomer is N,N-dimethylacrylamide and acrylamide in a mass ratio of 1.5:1, the unsaturated acid monomer is acrylic acid, the acrylate monomer is polyethylene glycol (480) acrylate, and the chain transfer agent is dodecyl mercaptan.

[0114] (2) Under a nitrogen atmosphere, deionized water was added to a reactor and stirred to fully remove oxygen. Then, acrylamide monomers, unsaturated acid monomers, acrylate monomers, and a chain transfer agent were added to the reactor. An appropriate amount of sodium hydroxide (mass fraction: 0.1%) was added to adjust the pH to neutral. Subsequently, ammonium persulfate was added, the temperature was raised to 80°C, and the reaction was stirred at 350 rpm for 30 hours. The temperature was then lowered to obtain a water-based binder.

[0115] Experimental Example 1

[0116] The monomer conversion rate, molecular weight and molecular weight distribution of the aqueous binders prepared in different embodiments and comparative examples were tested. The test results are shown in Table 1.

[0117] Table 1 Molecular weight and molecular weight distribution of different water-based binders

[0118]

[0119] Experimental Example 2

[0120] The aqueous binders prepared in different embodiments and comparative examples were used to prepare carbon-coated aluminum foils. The prepared carbon-coated aluminum foils were tested. The test results are shown in Table 2.

[0121] The preparation of carbon-coated aluminum foil includes:

[0122] (a) The aqueous binders of Examples 1 to 12 and Comparative Examples 1 to 5 were respectively blended with conductive carbon black in proportion, and ground by a grinder to a fineness of <1 μm to prepare a carbon coating slurry; wherein, by mass ratio, the aqueous binder: conductive carbon black SP: deionized water = 6:6:88, and the amount of the aqueous binder was calculated by its solid content; before preparing the slurry, the solid content of the aqueous binder was adjusted to 20% by water before use.

[0123] (b) The prepared carbon-coated aluminum foil slurry is input into the feeding system of the coating machine, and a 12 μm smooth aluminum foil is selected as the substrate. The coating speed is 70 m / min, and the drying temperature is 90-120°C to obtain a carbon-coated aluminum foil with a coating thickness of 1.5 μm.

[0124] The test items include the following:

[0125] Cohesive peel strength: Referring to GB / T 2792-2014 "Adhesive 180° Peel Strength Test Method", the prepared pole piece was cut into test samples (length and width of 200mm×25mm), the metal side was pasted on the stainless steel plate, and 3M tape (Scotch 600 / 25mm wide) was pasted on the coating surface, and the sample was rolled back and forth three times with a 1kg roller. In accordance with the national standard GB / T 2792-2014 test conditions, the cohesive force between the carbon coating layer / aluminum foil current collector was tested using a universal tensile machine.

[0126] 300 times of electrolyte wiping: Dip a cotton swab into the electrolyte (1mol / L LiPF6, the solvent is EC and DMC with a volume ratio of 1:1), and wipe back and forth on the same position of the carbon-coated aluminum foil. The wiping distance is about 6cm, and one round trip is counted as one time. Record and observe whether there is any leakage from the aluminum foil substrate after 300 wiping experiments.

[0127] Table 2 Test results of carbon-coated aluminum foil made with different water-based binders

[0128]

[0129] Note: Comparative Examples 2 and 3 did not react to obtain water-based binders, so this test was not performed.

[0130] From the above test results, it can be seen that the aqueous binder of the present invention has a narrow molecular weight distribution, excellent dispersibility and bonding properties, and can be used for the preparation of slurry of active materials for lithium-ion batteries, especially for the preparation of carbon-coated aluminum foil.

[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-based adhesive, characterized in that: It is prepared from the following components by weight: 70-80 parts of acrylamide monomer, 10-20 parts of unsaturated acid monomer, 10-20 parts of acrylate monomer, 2-3 parts of chain transfer agent, 100-400 parts of water and pH regulator; adjusting the amount of the pH regulator so that the pH value of the mixed system of each component is 1-3; The acrylamide monomers include N,N-dimethylacrylamide and acrylamide; The mass ratio of the N,N-dimethylacrylamide to the acrylamide is (1-2):1; The preparation method of the water-based adhesive comprises the following steps: in a protective atmosphere, each component is mixed uniformly according to a proportion, reacted at 25-90° C., discharged, and subjected to neutralization treatment; The unsaturated acid monomer includes at least one of an unsaturated carboxylic acid monomer or an inorganic salt thereof, and an unsaturated sulfonic acid monomer or an inorganic salt thereof; The unsaturated carboxylic acid monomer includes at least one of (meth)acrylic acid, maleic anhydride, itaconic acid and fumaric acid; The unsaturated sulfonic acid monomer includes at least one of styrene sulfonic acid, allyl sulfonic acid and methacrylic acid sulfonic acid.

2. The aqueous adhesive according to claim 1, characterized in that The mass percentage of the acrylamide monomers in all monomers is ≥70%.

3. The aqueous adhesive according to claim 1, characterized in that: The acrylic acid ester monomer includes at least one of alkyl (meth)acrylate, alkylhydroxy (meth)acrylate, polyethylene glycol methyl ether acrylate, di(hydroxyethyl) phosphate, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and di[2-(methacryloyloxy)ethyl]phosphate.

4. The aqueous adhesive according to claim 1, characterized in that: The pH adjuster includes at least one of sulfuric acid, sulfonic acid, phosphoric acid, hydrochloric acid, acetic acid, citric acid, lactic acid, oxalic acid and malic acid; The chain transfer agent includes a mercaptan chain transfer agent.

5. Carbon coated aluminum foil, characterized in that: The invention comprises an aluminum foil substrate and a carbon coating arranged on the surface of the aluminum foil substrate, wherein the carbon coating is made of a slurry containing the aqueous binder according to any one of claims 1 to 4.