A double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor and preparation method thereof

By controlling the growth parameters of wurtzite piezoelectric films, a parallel piezoelectric sensor with bilayer reverse spontaneous polarization wurtzite films was prepared, solving the problems of low yield and insufficient sensitivity caused by pre-polarization treatment, and realizing a high-sensitivity piezoelectric film sensor.

CN118660611BActive Publication Date: 2024-11-15DALIAN CHIP MATERIALS & THIN FILM TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411154878.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing wurtzite piezoelectric thin film sensors require pre-polarization treatment, resulting in low device yield, difficulty in integration, and high cost. Single-layer piezoelectric thin film sensors have insufficient sensitivity and cannot meet the needs of complex applications.

Method used

By adjusting the growth parameters of wurtzite piezoelectric films to ensure consistent spontaneous polarization directions, a parallel piezoelectric sensor with double-layered reverse spontaneous polarization wurtzite films was fabricated. A stacked structure with three electrode layers and two piezoelectric layers sandwiched in the middle was adopted to achieve parallel setup without pre-polarization.

Benefits of technology

It improves the sensitivity of piezoelectric thin film sensors, has a simple structure, is easy to integrate, has low cost, and can generate a stronger output signal under the same external excitation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118660611B_ABST
    Figure CN118660611B_ABST
Patent Text Reader

Abstract

A double-layer reverse spontaneous polarization wurtzite film parallel piezoelectric sensor and preparation method, comprising a device substrate; an insulating layer film deposited on the device substrate; a first electrode layer film deposited on the insulating layer film; a first piezoelectric layer film deposited on the first electrode layer film; a second electrode layer film deposited on the first piezoelectric layer film; a second piezoelectric layer film deposited on the second electrode layer film; a third electrode layer film deposited on the second piezoelectric layer film; a protective layer film deposited on the third electrode layer film; and a bridge lead for connecting the first electrode layer film and the third electrode layer film. The initial polarization directions of the first and second piezoelectric layer films are opposite. The present invention has the advantages of disorderly adding an additional pre-polarization step, simple structure, easy preparation, conducive to integration, and low cost; the structure of the piezoelectric film stacking arrangement can obtain a stronger output signal under the same external excitation, significantly improving the sensitivity of the piezoelectric film sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of piezoelectric film sensors and relates to a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor and a preparation method thereof. Background Art

[0002] Piezoelectric film sensor is a sensor that can convert mechanical pressure into electrical signals. Its working principle is based on the positive piezoelectric effect of piezoelectric materials. By detecting the change of charge density or potential difference on the surface of piezoelectric materials, it can sense and measure force, acceleration, air pressure, inertia and flow rate. It is widely used in aerospace, mobile communications, high-end equipment manufacturing and other fields. In order to adapt to more and more complex application scenarios and meet more and more stringent application requirements, piezoelectric film sensors based on different piezoelectric materials such as lead zirconate titanate (PZT), lithium niobate (LN), barium titanate (BT) and different design structures such as single layer and stacked layers have emerged on the market.

[0003] For common piezoelectric materials such as lead zirconate titanate (PZT), lithium niobate (LN), and barium titanate (BT), piezoelectric films usually need to be pre-polarized after preparation. Under the action of the polarization electric field, the direction of polarization inside the piezoelectric film tends to be consistent, and it shows polarity to the outside. In this process, a strong polarization voltage needs to be applied, which is a challenge to the construction of the entire device. The high polarization voltage can easily cause the piezoelectric film to break down at the electrode interface, resulting in failure, resulting in a reduction in device yield. The additional polarization steps also make integration difficult and increase costs. However, for wurtzite-type piezoelectric materials such as aluminum nitride (AlN) and zinc oxide (ZnO), there is spontaneous polarization from the metal polar end to the N / O polar end, and the direction of the spontaneous polarization can be controlled by controlling the film growth parameters to make it parallel or anti-parallel to the film growth direction. In other words, wurtzite-type piezoelectric materials can show polarity to the outside without pre-polarization, and the direction of spontaneous polarization can be controlled by regulating the film growth parameters.

[0004] In addition, the Chinese invention patent (CN114242884A) and the literature (Nam-InKim et al., Piezoelectric Sensors Operating at Very High Temperatures and in Extreme Environments Made of Flexible Ultrawide-Bandgap Single-Crystalline AlN Thin Films, Adv. Funct. Mater. 2023, 33, 2212538) respectively disclose single-layer piezoelectric film sensors based on wurtzite piezoelectric materials ZnO and AlN, but this single-layer piezoelectric film sensor has low sensitivity and is difficult to meet the growing application needs. The present invention realizes the control of the spontaneous polarization direction of the wurtzite piezoelectric film by regulating the film growth parameters, and then proposes a design structure of a piezoelectric film stack to improve the performance of the piezoelectric film sensor. By superimposing two layers of piezoelectric film with opposite polarization directions and connecting two layers of electrode layer film with the same polarity, the parallel connection of two layers of piezoelectric film can be realized. This structure can generate a stronger output signal under a smaller external excitation, achieving twice the result with half the effort. Summary of the invention

[0005] In view of the technical problems existing in the prior art, the present invention proposes a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor and a preparation method. At present, the textured film growth technology of wurtzite piezoelectric film materials (AlN, ZnO, etc.) along the polarization axis (0001) has become mature. Based on this, the present invention modifies the film growth process and controls the polarity so that each grain of the prepared film has a uniform polarization direction, thereby realizing the concept of parallel setting of piezoelectric layers without pre-polarization.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A double-layer reverse spontaneous polarization wurtzite film parallel piezoelectric sensor, the parallel piezoelectric sensor includes: a device substrate, an insulating layer film deposited on the device substrate, a first electrode layer film deposited on the insulating layer film, a first piezoelectric layer film deposited on the first electrode layer film, a second electrode layer film deposited on the first piezoelectric layer film, a second piezoelectric layer film deposited on the second electrode layer film, a third electrode layer film deposited on the second piezoelectric layer film, a protective layer film deposited on the third electrode layer film, and a bridge lead located outside the first and third electrode layer films. Finally, a stacked structure with two piezoelectric layers sandwiched between three electrode layers is formed, wherein the polarization directions of the two piezoelectric layers are opposite, the second electrode layer serves as one of the output ends, and the first and third electrode layers serve as the other output end after being connected in parallel. Based on the positive piezoelectric effect of the piezoelectric film, under the same mechanical pressure input, the first and second piezoelectric layer films respectively generate unequal amounts of response polarization charges and output them after being superimposed by a parallel circuit. Therefore, the output signal is enhanced under the same mechanical pressure input, thereby improving the sensitivity of the piezoelectric film sensor.

[0008] Furthermore, there is no special material requirement for the device substrate. Available substrate materials include but are not limited to metal materials (Cu, Ti, stainless steel, etc.), semiconductor materials (Si, Ge, SiC, etc.) and insulator materials (Al2O3, quartz, glass, etc.), and the surface is polished to a mirror surface.

[0009] Furthermore, the insulating layer film is made of SiO2, Al2O3 or other insulating films, and the protective layer film is made of SiO2, Al2O3 or other insulating films.

[0010] Furthermore, the first electrode layer film is selected from a highly conductive elemental metal or a highly conductive transition metal nitride, wherein the highly conductive elemental metal includes Al, Cu, Ti, Mo, W, Ni, Ag, Au, and Pt, and the highly conductive transition metal nitride includes TiN, ZrN, and Mo2N.

[0011] Furthermore, the second electrode layer film is selected from a highly conductive elemental metal or a highly conductive transition metal nitride, wherein the highly conductive elemental metal includes Al, Cu, Ti, Mo, W, Ni, Ag, Au, and Pt, and the highly conductive transition metal nitride includes TiN, ZrN, and Mo2N.

[0012] Furthermore, the third electrode layer film is selected from a highly conductive single metal or a highly conductive transition metal nitride, wherein the highly conductive single metal includes Al, Cu, Ti, Mo, W, Ni, Ag, Au, Pt, and the highly conductive transition metal nitride includes TiN, ZrN, and Mo2N. The materials of the first electrode layer film, the second electrode layer film, and the third electrode layer film may be the same or different, and there is no consistency requirement.

[0013] Furthermore, the first piezoelectric layer film is a wurtzite piezoelectric material, including wurtzite-based ZnO, AlN, GaN, and multi-doped compounds thereof, preferably Al x Sc 1-x N, Zn x Mg 1-x O.Ga x Sc 1-x N.

[0014] Furthermore, the second piezoelectric layer film is a wurtzite piezoelectric material, including wurtzite-based ZnO, AlN, GaN, and multi-doped compounds thereof, preferably Al x Sc 1-x N, Zn x Mg 1-x O.Ga x Sc 1-x N. The materials of the first piezoelectric layer film and the second piezoelectric layer film may be the same or different, and there is no consistency requirement.

[0015] Furthermore, by regulating the growth parameters of the first piezoelectric layer film and the second piezoelectric layer film, the initial polarization directions of the first piezoelectric layer film and the second piezoelectric layer film are opposite.

[0016] Furthermore, the bridge lead is made of a highly conductive material such as Cu, Ag, Au, Al, etc., to connect the first electrode layer film and the third electrode layer film, so that the two piezoelectric layer films are arranged in parallel.

[0017] The present invention also provides a method for preparing the above-mentioned double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor, comprising the following steps:

[0018] S1. Device substrate cleaning: remove organic pollutants, metal particles and other impurities on the device substrate surface. The substrate materials include metal materials (Cu, Ti, stainless steel, etc.), semiconductor materials (Si, Ge, SiC, etc.) and insulator materials (Al2O3, quartz, glass, etc.), including but not limited to these materials.

[0019] S2. Preparation of insulating layer film: mounting the device substrate on a positioning fixture and placing them together in a vacuum sputtering chamber, and depositing the insulating layer film using magnetron sputtering technology;

[0020] S3, preparing the first electrode layer thin film: installing the electrode thin film mechanical mask plate on the positioning fixture, mechanically fixing it, placing it in the vacuum sputtering chamber, and depositing the first electrode layer thin film by magnetron sputtering technology;

[0021] S4. Prepare the first piezoelectric film layer: install the piezoelectric film mechanical mask plate on the positioning fixture, fix it mechanically, put it into the vacuum sputtering chamber, and deposit the first piezoelectric film layer using magnetron sputtering technology. By changing the specific film growth parameters of the first piezoelectric film layer, where the film growth parameters include sputtering mode, sputtering power, sputtering gas pressure, and gas flow rate, the initial polarization direction of the prepared wurtzite piezoelectric film material is parallel to the film growth direction. Specific preferred film growth parameters include higher sputtering power or lower sputtering gas pressure;

[0022] S5, preparing the second electrode layer thin film: installing the electrode thin film mechanical mask plate on the positioning fixture, mechanically fixing it, placing it in the vacuum sputtering chamber, and depositing the second electrode layer thin film by magnetron sputtering technology;

[0023] S6. Prepare the second piezoelectric film: install the piezoelectric film mechanical mask on the positioning fixture, fix it mechanically, put it into the vacuum sputtering chamber, and use magnetron sputtering technology to deposit the second piezoelectric film. By changing the specific film growth parameters of the second piezoelectric film, where the film growth parameters include sputtering mode, sputtering power, sputtering gas pressure, and gas flow rate, the initial polarization direction of the prepared wurtzite piezoelectric film material is antiparallel to the film growth direction. Specific preferred process parameters include lower sputtering power or higher sputtering gas pressure;

[0024] S7, preparing the third electrode layer thin film: installing the electrode thin film mechanical mask plate on the positioning fixture, mechanically fixing it, placing it in the vacuum sputtering chamber, and depositing the third electrode layer thin film by magnetron sputtering technology;

[0025] S8. Prepare a protective layer film: place the laminated film prepared above in a vacuum sputtering chamber, deposit the protective layer film using magnetron sputtering technology, and take out the sample after cooling in the furnace.

[0026] S9. Lead bridging: Use leads made of highly conductive materials such as Cu, Ag, Au, and Al to connect the first electrode layer and the third electrode layer.

[0027] Furthermore, in the steps S4 and S6, the film growth parameters for preparing the first and second piezoelectric layer films can be interchanged, and ultimately it should be ensured that the polarization directions of the first and second piezoelectric layer films are opposite.

[0028] Furthermore, in the steps S2, S3, S4, S5, S6, S7 and S8, the technology for preparing the insulating layer film, the electrode layer film, the piezoelectric layer film and the protective layer film can be replaced by other thin film growth technologies such as pulsed laser deposition, electron beam evaporation coating, atomic layer deposition, metal organic compound chemical vapor deposition, etc., and the growth parameters of various thin film growth technologies are selected to ensure that the initial polarization directions of the first piezoelectric layer film and the second piezoelectric layer film are opposite, that is, the initial polarization direction of one wurtzite piezoelectric film material is parallel to the film growth direction, and the initial polarization direction of the other wurtzite piezoelectric film material is anti-parallel to the film growth direction. It is a known technical content in the art to achieve the change of the initial polarization direction of the wurtzite film by adjusting the growth parameter range.

[0029] Furthermore, the thickness of the insulating layer film is 2~10μm; the thickness of the first electrode layer film is 50~200nm; the thickness of the first piezoelectric layer film is 300~1500nm; the thickness of the second electrode layer film is 50~200nm; the thickness of the second piezoelectric layer film is 300~1500nm; the thickness of the third electrode layer film is 50~200nm; and the thickness of the protective layer film is 2~10μm.

[0030] The principle of the present invention is:

[0031] The present invention controls the spontaneous polarization direction by changing the film growth parameters of the wurtzite piezoelectric material, thereby realizing a stacked structure in which two piezoelectric layers with opposite polarization directions are sandwiched between three electrode layers, wherein the second electrode layer serves as one of the output ends, and the first and third electrode layers are connected in parallel to form another output end. Under the input of mechanical pressure, the magnitude of the input mechanical pressure is extracted by detecting the change in the charge density of the polarization surface or the potential difference between the two output ends, thereby realizing pressure sensing.

[0032] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0033] (1) Based on the spontaneous polarization characteristics of wurtzite piezoelectric materials, by simply changing the growth parameters of wurtzite piezoelectric thin film materials, the internal polarization direction of the deposited piezoelectric thin film can be made consistent, showing polarity to the outside. Therefore, there is no need to add an additional pre-polarization step, which has the advantages of simple structure, easy preparation, easy integration, and low cost. The structure of the piezoelectric thin film stack can obtain a stronger output signal under the same external excitation, significantly improving the sensitivity of the piezoelectric thin film sensor.

[0034] (2) Based on the above reasons, the present invention can be widely promoted in the field of piezoelectric film sensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1This is a cross-sectional view of the single-layer ZnO piezoelectric film sensor in Comparative Example 1.

[0036] Figure 2 This is a cross-sectional view of the double-layer ZnO piezoelectric film sensor in Example 1.

[0037] Figure 3 This is a cross-sectional view of the ZnO and AlN composite double-layer piezoelectric film sensor in Example 2.

[0038] Figure 4 For the double-layer Al in Example 3 x Sc 1-x Cross-sectional view of a piezoelectric film sensor.

[0039] Figure 5 This is a cross-sectional view of the double-layer AlN piezoelectric film sensor in Example 4.

[0040] Figure 6 1 and 1 are polarization surface charge density characteristic curves of two different piezoelectric film sensors in comparative example 1 and embodiment 1 under different mechanical pressure inputs.

[0041] Figure 7 Schematic diagram of the polarity of wurtzite structure. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0043] In addition, it should be noted that the use of terms such as "first", "second", and "third" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0044] Comparative Example 1

[0045] In this comparative example, a ZnO single-layer piezoelectric thin film sensor was prepared using magnetron sputtering technology. Figure 1 shown.

[0046] 1) Cleaning the substrate: Select stainless steel as the substrate, polish the substrate to a mirror surface, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow dry with nitrogen, and place it in a vacuum chamber.

[0047] 2) Preparation of insulating film: Pulsed DC magnetron sputtering technology was used, with Si as the target material, 65 mm target-substrate distance, 0.7 Pa working pressure, 250 W power, 20 SCCM argon flow, 10 SCCM oxygen flow, room temperature substrate temperature, and 60 min sputtering time to grow a 2 μm thick SiO2 insulating layer with a resistance value of up to 10 8 Ω, to play the role of insulation.

[0048] 3) Preparation of the first electrode layer film: A 200 nm thick Ni first electrode layer film was grown using pulsed DC magnetron sputtering technology with a Ni target, a target-substrate distance of 65 mm, a working pressure of 0.7 Pa, a power of 150 W, an argon gas flow rate of 20 SCCM, a substrate temperature of room temperature, and a sputtering time of 10 min.

[0049] 4) Preparation of piezoelectric layer film: Using RF magnetron sputtering technology, the target material is Zn, the target substrate distance is 65mm, the working pressure is 0.7Pa, the power is 150W, the argon flow rate is 25SCCM, the oxygen flow rate is 10SCCM, the substrate temperature is room temperature, and the sputtering time is 80min to grow a ZnO film with a thickness of 1.0μm.

[0050] 5) Preparation of second electrode layer film: A 200 nm thick Ni second electrode layer film was prepared using the same process as the first electrode layer film.

[0051] 6) Preparation of protective layer film: A 2 μm thick SiO2 protective layer film was prepared using the same process as the insulating layer film.

[0052] The polarization direction of the piezoelectric film is defined as positive when it is parallel to the film growth direction, and negative when it is anti-parallel. The piezoelectric coefficient of the prepared ZnO film is 1.36pC / N.

[0053] Example 1

[0054] In the specific implementation, as a preferred implementation method of the present invention, a ZnO double-layer piezoelectric thin film sensor is prepared by using magnetron sputtering technology and electron beam evaporation coating technology, such as Figure 2 shown.

[0055] 1) Cleaning the substrate: Select stainless steel as the substrate, polish the substrate to a mirror surface, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow dry with nitrogen, and place it in a vacuum chamber.

[0056] 2) Preparation of insulating film: Pulsed DC magnetron sputtering technology was used, with Si as the target material, 30 mm target-substrate distance, 0.5 Pa working pressure, 500 W power, 20 SCCM argon flow, 10 SCCM oxygen flow, room temperature substrate temperature, and sputtering time of 2 h to grow a 2 μm thick SiO2 insulating layer with a resistance value of up to 10 8 Ω, to play the role of insulation.

[0057] 3) Preparation of the first electrode layer film: The first electrode layer film is made of Pt and is deposited by electron beam evaporation technology with a heating current of 3A, a evaporation temperature of 1800°C, and a background vacuum of 5×10 -6 A Pt first electrode layer film with a thickness of 60 nm was grown under the conditions of a deposition time of 10 min.

[0058] 4) Preparation of the first piezoelectric layer film: Using RF magnetron sputtering technology, the target material is Zn, the ratio of argon flow rate to oxygen flow rate is 1:1, the substrate temperature is 400°C, the working gas pressure is 0.5Pa, the RF sputtering power is 100W, and the sputtering time is 5h to grow a ZnO first piezoelectric layer film with a thickness of 400nm.

[0059] 5) Preparation of the second electrode layer film: A Mo second electrode layer film with a thickness of 100 nm was grown using DC magnetron sputtering technology with a target material of Mo, a target-substrate distance of 90 mm, a working gas pressure of 0.4 Pa, a power of 100 W, an argon gas flow rate of 30 SCCM, a substrate temperature of 300 °C, and a sputtering time of 10 min.

[0060] 6) Preparation of the second piezoelectric layer film: A 400nm thick ZnO second piezoelectric layer film was grown using RF magnetron sputtering technology, with Zn as the target material, a 1:1 ratio of argon flow to oxygen flow, a substrate temperature of 400°C, a working gas pressure of 0.5Pa, an RF sputtering power of 500W, and a sputtering time of 1h.

[0061] 7) Preparation of the third electrode layer thin film: A 60 nm thick Pt third electrode layer thin film was prepared using the same process as the first electrode layer thin film.

[0062] 8) Preparation of protective layer film: A 3 μm thick SiO2 protective layer film was prepared using the same process as the insulating layer film.

[0063] 9) The first and third electrode layer films are connected by Cu wires so that the two piezoelectric layer films are arranged in parallel.

[0064] Under the above film growth parameter conditions, the piezoelectric coefficient of the prepared first piezoelectric film is -1.32pC / N, and the piezoelectric coefficient of the second piezoelectric film is 1.27pC / N. The polarization direction of the prepared ZnO piezoelectric film can be changed by changing the power of the RF power supply of the RF sputtering, thereby achieving the concept of the present invention of realizing the parallel arrangement of piezoelectric film stacks without pre-polarization.

[0065] Example 2

[0066] In the specific implementation, as a preferred implementation method of the present invention, a magnetron sputtering technology is used to prepare an AlN and ZnO composite double-layer piezoelectric thin film sensor, such as Figure 3 shown.

[0067] 1) Cleaning the substrate: Select single crystal Si as the substrate, polish the substrate to a mirror surface, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow dry with nitrogen, and place it in a vacuum chamber.

[0068] 2) Preparation of insulating film: Pulsed DC magnetron sputtering technology was used, with Al as the target material, 50 mm target-substrate distance, 0.8 Pa working pressure, 300 W power, 30 SCCM argon flow, 5 SCCM oxygen flow, room temperature substrate temperature, and sputtering time of 2 h to grow an Al2O3 insulating layer with a thickness of 10 μm and a resistance value of up to 10 8 Ω, to play the role of insulation.

[0069] 3) Preparation of the first electrode layer film: A 200 nm thick TiN first electrode layer film was grown using DC magnetron sputtering technology with a Ti target, a target-substrate distance of 90 mm, a working gas pressure of 0.4 Pa, a power of 200 W, an argon flow rate and a nitrogen flow rate ratio of 10:1, a substrate temperature of 300 °C, and a sputtering time of 30 min.

[0070] 4) Preparation of the first piezoelectric layer film: Using RF magnetron sputtering technology, the target material is Al, the ratio of argon flow rate to nitrogen flow rate is 1:1, the substrate temperature is room temperature, the working gas pressure is 0.36Pa, the RF sputtering power is 400W, and the sputtering time is 5h to grow an AlN first piezoelectric layer film with a thickness of 1500nm.

[0071] 5) Preparation of the second electrode layer film: A Mo2N second electrode layer film with a thickness of 200 nm was grown by using DC magnetron sputtering technology, with a Mo target as the target material, a target-substrate distance of 70 mm, a working gas pressure of 0.3 Pa, a power of 150 W, an argon flow rate to nitrogen flow rate ratio of 10:2, a substrate temperature of 300 °C, and a sputtering time of 30 min.

[0072] 6) Preparation of the second piezoelectric layer film: Using RF magnetron sputtering technology, the target material was Zn, the ratio of argon flow rate to oxygen flow rate was 1:1, the substrate temperature was 300°C, the working gas pressure was 4.0Pa, the RF sputtering power was 400W, and the sputtering time was 8h to grow a ZnO second piezoelectric layer film with a thickness of 1500nm.

[0073] 7) Preparation of the third electrode layer thin film: A 200 nm thick Ti third electrode layer thin film was grown using DC magnetron sputtering technology with a target material of Ti, a target-substrate distance of 90 mm, a working gas pressure of 0.3 Pa, a power of 145 W, an argon gas flow rate of 30 SCCM, a substrate temperature of 300 °C, and a sputtering time of 15 min.

[0074] 8) Preparation of protective layer film: Pulse DC magnetron sputtering technology was used, the target material was Si, the target-substrate distance was 30 mm, the working pressure was 0.5 Pa, the power was 500 W, the argon flow rate was 20 SCCM, the oxygen flow rate was 10 SCCM, the substrate temperature was room temperature, and the sputtering time was 6 h to grow a SiO2 protective layer with a thickness of 10 μm.

[0075] 9) Use Ag wire to connect the first and third electrode layer films so that the two piezoelectric layer films are arranged in parallel.

[0076] Under the above film growth parameter conditions, the piezoelectric coefficient of the prepared first piezoelectric layer film is 3.7pC / N, and the piezoelectric coefficient of the second piezoelectric layer film is -1.57pC / N. By changing the film growth parameters, the polarization direction of the prepared wurtzite piezoelectric film can be changed, thereby achieving the concept of the present invention of realizing the parallel arrangement of piezoelectric film stacks without pre-polarization.

[0077] Example 3

[0078] In the specific implementation, as a preferred implementation method of the present invention, the Al x Sc 1-x N double-layer piezoelectric film sensor, such as Figure 4 shown.

[0079] 1) Cleaning the substrate: Use glass as the substrate, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow it dry with nitrogen, and place it in a vacuum chamber.

[0080] 2) Preparation of insulating film: Pulsed DC magnetron sputtering technology was used, with Al as the target material, 50 mm target-substrate distance, 0.8 Pa working pressure, 300 W power, 30 SCCM argon flow, 5 SCCM oxygen flow, room temperature substrate temperature, and sputtering time of 1 h to grow an Al2O3 insulating layer with a thickness of 5 μm and a resistance value of up to 10 8Ω, to play the role of insulation.

[0081] 3) Preparation of the first electrode layer film: Using DC magnetron sputtering technology, the target material is Zr, the target-substrate distance is 90 mm, the working gas pressure is 0.3 Pa, the power is 145 W, the ratio of argon flow rate to nitrogen flow rate is 10:1, the substrate temperature is 350 ° C, and the sputtering time is 10 min. Under these conditions, a ZrN first electrode layer film with a thickness of 50 nm was grown.

[0082] 4) Preparation of the first piezoelectric layer film: RF magnetron sputtering technology was used, with Al and Sc as the target materials, and sputtering was carried out in a pure nitrogen atmosphere. The substrate temperature was 300°C, the working pressure was 0.4 Pa, the RF sputtering power of the Al target was 400 W, the RF sputtering power of the Sc target was 320 W, and the sputtering time was 1 h. A 300 nm thick Al film was grown. x Sc 1-x N: First piezoelectric thin film layer.

[0083] 5) Preparation of the second electrode layer film: Using DC magnetron sputtering technology, the target material is Al, the target-substrate distance is 90 mm, the working gas pressure is 0.4 Pa, the power is 100 W, the argon gas flow rate is 30 SCCM, the substrate temperature is room temperature, and the sputtering time is 10 min. Under the conditions, a 100 nm thick Al second electrode layer film was grown.

[0084] 6) Preparation of the second piezoelectric layer film: Using RF magnetron sputtering technology, the target materials are Al and Sc, sputtering is carried out in a pure nitrogen atmosphere, the substrate temperature is 300°C, the working pressure is 0.4 Pa, the RF sputtering power of the Al target is 100W, the RF sputtering power of the Sc target is 80W, and the sputtering time is 3h. A 300nm thick Al film is grown. x Sc 1-x N: The second piezoelectric layer film.

[0085] 7) Preparation of the third electrode layer film: A Ni third electrode layer film with a thickness of 100 nm was grown using DC magnetron sputtering technology with Ni as the target material, a target-substrate distance of 45 mm, a working gas pressure of 0.4 Pa, a power of 150 W, an argon gas flow rate of 30 SCCM, a substrate temperature of 200 °C, and a sputtering time of 10 min.

[0086] 8) Preparation of protective layer film: A 2 μm thick Al2O3 protective layer film was prepared using the same process as the insulating layer film.

[0087] 9) Use Al wire to connect the first and third electrode layer films so that the two piezoelectric layer films are arranged in parallel.

[0088] Under the above film growth parameter conditions, the piezoelectric coefficient of the prepared first piezoelectric layer film is 13.6pC / N, and the piezoelectric coefficient of the second piezoelectric layer film is -12.8pC / N. By changing the RF power of the RF sputtering, the prepared Al x Sc 1-x N piezoelectric film polarization direction, thereby achieving the concept of the present invention can realize the piezoelectric film stack parallel arrangement without pre-polarization.

[0089] Example 4

[0090] In the specific implementation, as a preferred embodiment of the present invention, the AlN double-layer piezoelectric thin film sensor is prepared by using magnetron sputtering technology, electron beam evaporation coating technology, and metal organic compound chemical vapor deposition technology, such as Figure 5 shown.

[0091] 1) Cleaning the substrate: Select Ti as the substrate, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow dry it with nitrogen, and place it in a vacuum chamber.

[0092] 2) Preparation of insulating layer film: Pulsed DC magnetron sputtering technology was used, with Si as the target material, 30 mm target-substrate distance, 0.5 Pa working pressure, 500 W power, 20 SCCM argon flow, 10 SCCM oxygen flow, room temperature substrate temperature, and sputtering time of 80 min to grow a 2 μm thick SiO2 insulating layer with a resistance value of up to 10 8 Ω, to play the role of insulation.

[0093] 3) Preparation of the first electrode layer film: Using DC magnetron sputtering technology, the target material is Mo, the target-substrate distance is 90 mm, the working gas pressure is 0.4 Pa, the power is 100 W, the argon gas flow rate is 30 SCCM, the substrate temperature is 300 ° C, and the sputtering time is 10 min. Under the conditions, a Mo first electrode layer film with a thickness of 100 nm was grown.

[0094] 4) Preparation of the first piezoelectric layer film: Using metal organic compound chemical vapor deposition technology, the metal organic source is trimethylaluminum, the nitrogen source is ammonia, the flow ratio of trimethylaluminum to ammonia is 6000:1, the substrate temperature is 1200°C, the reaction gas pressure is 20Torr, the bias voltage applied in the direction perpendicular to the substrate is +200V, and the deposition time is 2h. Under these conditions, a 400nm thick AlN first piezoelectric layer film was grown.

[0095] 5) Preparing a second electrode layer thin film: A 100 nm Mo second electrode layer thin film was prepared using the same process as the first electrode layer thin film.

[0096] 6) Preparation of the second piezoelectric layer film: Using metal organic compound chemical vapor deposition technology, the metal organic source is trimethylaluminum, the nitrogen source is ammonia, the flow ratio of trimethylaluminum to ammonia is 6000:1, the substrate temperature is 1200°C, the reaction gas pressure is 20Torr, the bias voltage applied in the direction perpendicular to the substrate is -200V, and the deposition time is 2h. Under these conditions, a 350nm thick AlN second piezoelectric layer film was grown.

[0097] 7) Preparation of the third electrode layer film: The third electrode layer film is made of Au and is coated by electron beam evaporation technology with a heating current of 3A, an evaporation temperature of 1100°C, and a background vacuum of 5×10 -6 A 60nm thick Au third electrode layer film was grown under the conditions of Pa and deposition time of 10min.

[0098] 8) Prepare the protective layer film by pulsed DC magnetron sputtering technology. The target material is Al, the target substrate distance is 50 mm, the working pressure is 0.8 Pa, the power is 300 W, the argon flow rate is 30 SCCM, the oxygen flow rate is 5 SCCM, the substrate temperature is room temperature, and the sputtering time is 40 min. A 2 μm thick Al2O3 protective layer film was grown.

[0099] 9) Use Al wire to connect the first and third electrode layer films so that the two piezoelectric layer films are arranged in parallel.

[0100] Under the above film growth parameter conditions, the piezoelectric coefficient of the prepared first piezoelectric layer film is 3.6pC / N, and the piezoelectric coefficient of the second piezoelectric layer film is -4.8pC / N. By changing the positive and negative bias voltage applied in the direction perpendicular to the substrate during the deposition process, the polarization direction of the prepared AlN piezoelectric film can be changed, thereby achieving the concept of the present invention of realizing the parallel arrangement of piezoelectric film stacks without pre-polarization.

[0101] Example 5

[0102] In specific implementation, as a preferred embodiment of the present invention, atomic layer deposition technology, magnetron sputtering technology, and pulsed laser deposition technology are used to prepare GaN and AlN composite double-layer piezoelectric thin film sensors.

[0103] 1) Cleaning the substrate: Use stainless steel as the substrate, clean it with acetone, anhydrous ethanol, and deionized water in sequence, blow it dry with nitrogen, and then place it in a vacuum chamber.

[0104] 2) Preparation of insulating layer film: Pulsed DC magnetron sputtering technology was used, with Al as the target material, 50 mm target-substrate distance, 0.8 Pa working pressure, 300 W power, 30 SCCM argon flow rate, 5 SCCM oxygen flow rate, room temperature substrate temperature, and sputtering time of 40 min to grow an Al2O3 insulating layer film with a thickness of 2 μm.

[0105] 3) Preparation of the first electrode layer film: A 50 nm thick TiN first electrode layer film was grown using DC magnetron sputtering technology with a target material of Ti, a target-substrate distance of 90 mm, a working gas pressure of 0.4 Pa, a power of 200 W, an argon flow rate to nitrogen flow rate ratio of 10:1, a substrate temperature of 300 °C, and a sputtering time of 10 min.

[0106] 4) Preparation of the first piezoelectric layer film: Atomic layer deposition technology was used, the gallium precursor was trimethylgallium (TMG), and the nitrogen precursor was Ar / N2 / H2. The total flow rate of the nitrogen precursor was 8SCCM, and the ratio was Ar:N2:H2=6:3:1. The nitrogen precursor was ionized by radio frequency power to form plasma, and the radio frequency power was 80W. The carrier gas was Ar, which was used to flush the remaining gas in the reactor and remove by-products. The total flow rate of the carrier gas was 10SCCM, and the carrier gas heating temperature was 80°C. The film growth temperature was 400°C, the background vacuum was 0.15Torr, the number of cycles was 1800 times, and a single cycle included: Ar / N2 / H2 plasma pulse 0.1s, Ar flushing 50s, gas phase precursor trimethylgallium pulse 0.25s, Ar flushing 50s. A 300nm thick GaN first piezoelectric layer film was grown under the above parameters.

[0107] 5) Preparation of the second electrode layer film: A 50 nm thick TiN second electrode layer film was prepared using the same process as the first electrode layer film.

[0108] 6) Preparation of the second piezoelectric layer film: pulsed laser deposition technology was used, the target material was Al, the target-substrate distance was 50 mm, the laser source was a KrF laser beam, the laser wavelength was 248 nm, the pulse duration was 25 ns, and the laser energy density was 3 J / cm 2 The reaction gas was N2, and RF power was used to assist ionization to form plasma. The RF power was 300W, the working gas pressure was 0.8Pa, the substrate temperature was 800℃, and the deposition time was 3h to grow a 500nm thick AlN second piezoelectric layer film.

[0109] 7) Preparation of the third electrode layer thin film: A 200 nm thick Cu third electrode layer thin film was grown using DC magnetron sputtering technology with a target material of Cu, a target-substrate distance of 90 mm, a working gas pressure of 0.4 Pa, a power of 200 W, an argon gas flow rate of 20 CCM, a substrate temperature of 200 °C, and a sputtering time of 25 min.

[0110] 8) Preparation of protective layer film: An Al2O3 protective layer film with a thickness of 2 μm was prepared using the same process as the insulating layer film.

[0111] 9) Use Ag wire to connect the first and third electrode layer films so that the two piezoelectric layer films are arranged in parallel.

[0112] Under the above film growth parameter conditions, the piezoelectric coefficient of the prepared first piezoelectric layer film is -2.8pC / N, and the piezoelectric coefficient of the second piezoelectric layer film is 4.1pC / N. By changing the film growth parameters, the polarization direction of the prepared wurtzite piezoelectric film can be changed, thereby achieving the concept of the present invention of realizing the parallel arrangement of piezoelectric film stacks without pre-polarization.

[0113] The structural verification and analysis of Comparative Example 1 and Example 1 are as follows:

[0114] For the single-layer piezoelectric film sensor shown in Comparative Example 1, there is a positive piezoelectric effect equation:

[0115] (1)

[0116] Where q is the polarization surface charge density, F is the mechanical pressure input by the piezoelectric film sensor, and d 33 is the piezoelectric coefficient of the piezoelectric film, and A is the area of ​​the piezoelectric film. According to the direct piezoelectric effect equation (1), when a piezoelectric material is subjected to mechanical pressure, polarization charges will be generated inside the material. The magnitude of the input mechanical pressure can be extracted by measuring the polarization surface charge density.

[0117] For the double-layer parallel piezoelectric film sensor shown in Example 1, according to the positive piezoelectric effect equation (1), the polarization surface charge density of the first piezoelectric film and the second piezoelectric film is:

[0118] (2)

[0119] (3)

[0120] In the formula, is the polarization surface charge density of the first piezoelectric film, is the polarization surface charge density of the second piezoelectric film, F is the mechanical pressure input by the piezoelectric film sensor, is the piezoelectric coefficient of the first piezoelectric film, A1 is the area of ​​the first piezoelectric film layer, and A2 is the area of ​​the second piezoelectric film layer.

[0121] Since the first piezoelectric film and the second piezoelectric film in Embodiment 1 of the present invention are connected in parallel, the total polarization surface charge density output by the piezoelectric film sensor is the sum of the two.

[0122] (4)

[0123] In the formula, It is the total output polarization surface charge density of the double-layer piezoelectric film sensor. Compared with the single-layer piezoelectric film sensor, the structure of the piezoelectric film stack can achieve a stronger output signal under the same external excitation.

[0124] The characteristic curves of the input mechanical stress magnitude and polarization surface charge density of the two different piezoelectric film sensors in Comparative Example 1 and Example 1 were tested by a piezoelectric tester under different mechanical pressure loading conditions. Figure 6 As shown, the polarization surface charge density q of the two sensors is approximately linearly related to the loading force F.

[0125] According to the definition of sensor sensitivity, the sensitivity of piezoelectric film sensor can be expressed as:

[0126] (5)

[0127] Where S is the sensitivity of the piezoelectric film sensor, is the change in polarization surface charge density, is the change in loading force.

[0128] Sensitivity is the slope of the two straight lines in the figure. The slope of the straight line of the polarization surface charge density q obtained in Example 1 changing with the loading force F is significantly higher than that of Comparative Example 1.

[0129] Through the above verification analysis and Figure 6 (Characteristic curves of polarization surface charge density of two different piezoelectric film sensors under different mechanical pressure inputs in comparative example and embodiment 1) It can be seen that the sensitivity of the two-layer piezoelectric film sensor shown in embodiment 1 is significantly higher than that of the single-layer piezoelectric film sensor in comparative example 1. The method of setting up two layers of piezoelectric films in parallel can indeed increase the performance of the piezoelectric film sensor and achieve the effect of increasing sensitivity.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents, and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor, characterized in that: The steps include: S1, cleaning device substrate; S2, depositing an insulating layer thin film on the surface of the device substrate using magnetron sputtering technology; S3, depositing a first electrode layer thin film using magnetron sputtering technology; S4, depositing the first piezoelectric layer film by magnetron sputtering technology; by changing the specific film growth parameters of the first piezoelectric layer film, the initial polarization direction of the prepared wurtzite piezoelectric film material is parallel to the film growth direction; the film growth parameters include sputtering mode, sputtering power, sputtering gas pressure, and gas flow rate; S5, depositing a second electrode layer thin film by using magnetron sputtering technology; S6. Depositing the second piezoelectric layer film by magnetron sputtering technology; by changing the specific film growth parameters of the second piezoelectric layer film, the initial polarization direction of the prepared wurtzite piezoelectric film material is antiparallel to the film growth direction; the film growth parameters include sputtering mode, sputtering power, sputtering gas pressure, and gas flow rate; S7, depositing a third electrode layer thin film by using magnetron sputtering technology; S8, placing the laminated film prepared above in a vacuum sputtering chamber, depositing a protective layer film using magnetron sputtering technology, and taking out the sample after cooling in the furnace; S9, connecting the first electrode layer and the third electrode layer by using a wire bridge.

2. The method for preparing a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 1, characterized in that: By regulating the growth parameters of the first piezoelectric layer film and the second piezoelectric layer film, the initial polarization directions of the first piezoelectric layer film and the second piezoelectric layer film are opposite.

3. The method for preparing a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 1, characterized in that: In S4 and S6, the film growth parameters for preparing the first and second piezoelectric layer films are interchanged, and ultimately it should be ensured that the polarization directions of the first and second piezoelectric layer films are opposite.

4. The method for preparing a double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 1, characterized in that: The thickness of the insulating layer film is 2~10μm; the thickness of the first electrode layer film is 50~200nm; the thickness of the first piezoelectric layer film is 300~1500nm; the thickness of the second electrode layer film is 50~200nm; the thickness of the second piezoelectric layer film is 300~1500nm; the thickness of the third electrode layer film is 50~200nm; and the thickness of the protective layer film is 2~10μm.

5. A double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor comprises: Device substrate; An insulating layer film deposited on the device substrate; A first electrode layer film deposited on the insulating layer film; a first piezoelectric layer film deposited on the first electrode layer film; a second electrode layer film deposited on the first piezoelectric layer film; a second piezoelectric layer film deposited on the second electrode layer film; a third electrode layer film deposited on the second piezoelectric layer film; A protective layer film deposited on the third electrode layer film; A bridge lead is located outside the first electrode layer film and the third electrode layer film, and is used to connect the first electrode layer film and the third electrode layer film so that the two piezoelectric layer films are arranged in parallel; The above structures ultimately form a stacked structure with two piezoelectric layers sandwiched between three electrode layers, wherein the polarization directions of the first piezoelectric layer and the second piezoelectric layer are opposite, the second electrode layer serves as an output end, and the first electrode layer and the third electrode layer are connected in parallel as another output end, with a total of two output ends; the first piezoelectric layer film is a wurtzite piezoelectric material; the second piezoelectric layer film is a wurtzite piezoelectric material.

6. The double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 5, characterized in that: The material of the device substrate includes metal material, semiconductor material or insulator material; The insulating layer film is made of SiO2 or Al2O3; The protective layer film is made of SiO2 or Al2O3; The bridge lead is made of a highly conductive material.

7. The double-layer reverse spontaneous polarization wurtzite film parallel piezoelectric sensor according to claim 6, characterized in that: In the device substrate: the metal material includes Cu, Ti or stainless steel; the semiconductor material includes Si, Ge or SiC; the insulator material includes Al2O3, quartz or glass; In the bridge lead, the highly conductive material includes Cu, Ag, Au or Al.

8. The double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 5, characterized in that: The first electrode layer film is selected from one of a highly conductive elemental metal or a highly conductive transition metal nitride; the second electrode layer film is selected from one of a highly conductive elemental metal or a highly conductive transition metal nitride; the third electrode layer film is selected from one of a highly conductive elemental metal or a highly conductive transition metal nitride; the materials of the first electrode layer film, the second electrode layer film, and the third electrode layer film are the same or different; The first piezoelectric layer film and the second piezoelectric layer film are made of the same or different materials.

9. The double-layer reverse spontaneously polarized wurtzite film parallel piezoelectric sensor according to claim 8, characterized in that: The highly conductive single metal includes Al, Cu, Ti, Mo, W, Ni, Ag, Au or Pt, and the highly conductive transition metal nitride includes TiN, ZrN or Mo2N; The wurtzite piezoelectric material includes wurtzite-based ZnO, AlN, GaN, and multi-doped compounds thereof.

Citation Information

Patent Citations

  • ZnO piezoelectric film sensor for monitoring bolt stress and preparation method thereof

    CN114242884A

  • Piezoelectric microphone and electronic device

    CN114339556A

  • Laminated piezoelectric body and ultrasonic transducer using the same, and method of manufacturing laminated piezoelectric body