A composite porous material for recovering tin element in etching liquid and preparation method thereof
By modifying 1,2-divinylbenzene and compositeing magnetic nanomaterials, the adsorption amount is increased and the regeneration cost is reduced, and the problems of low adsorption amount and high regeneration cost of existing tin ion adsorption materials are solved, thus achieving high efficiency Tin element recycling.
Patent Information
- Application Number
- CN202411159100.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing tin ion adsorption materials have low adsorption amount and high regeneration costs, making it difficult to effectively recover tin elements in waste etching liquid.
By modifying 1,2-divinylbenzene and the composite of magnetic nanomaterials with porous materials, the adsorption amount of adsorbed materials is increased, and the regeneration cost is reduced through magnetic separation technology.
The adsorption amount of tin ions and the regeneration rate of materials are significantly improved, the regeneration cost is reduced, and efficient tin element recovery is achieved.
Smart Images

Figure CN118663234B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorbents, and specifically refers to a composite porous material for recovering tin elements in etching liquid and a preparation method thereof. Background Art
[0002] Tin is a low-melting-point metallic element with a slightly bluish white luster, usually present in a divalent or tetravalent form in solution. With the continued rapid development of emerging industries such as the electronics industry, the demand for metallic tin is growing. In the process of etching printed circuit boards with nitric acid, waste liquid containing a large amount of tin and other metallic elements will be generated. At the same time, tin ore is a non-renewable resource, so it is very important to recover tin from waste etching liquid and regenerate etching liquid. For the recovery of metal elements in waste liquid, currently commonly used methods include precipitation, ion exchange, adsorption, solvent extraction, membrane separation and other methods, but due to the need to recover nitric acid in waste etching liquid and the limitation of recovery cost, most methods are not suitable for use. Adsorption is a green and environmentally friendly waste etching liquid treatment method because of its simple operation, stable performance, and the ability to recycle heavy metals. However, the commonly used tin ion adsorption materials have low adsorption capacity and high regeneration cost.
[0003] The existing technologies currently have the following main problems: low adsorption capacity of adsorption materials and high regeneration costs. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a composite porous material for recovering tin element in etching liquid and a preparation method thereof. In order to solve the problems of low adsorption capacity and high regeneration cost of the adsorption material, the present invention proposes to improve the adsorption capacity of the adsorption material by modifying 1,2-divinylbenzene, and at the same time, composite the magnetic nanomaterial with the porous material to further improve the adsorption capacity of the adsorption material, while achieving the technical effect of reducing the regeneration cost.
[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: the present invention proposes a composite porous material for recovering tin element in etching liquid, and the composite porous material for recovering tin element in etching liquid is prepared by comprising the following components in parts by weight: 20-30 parts of 1,2-divinylbenzene, 6-10 parts of double-terminated thiol polyethylene glycol, 1.2-1.5 parts of azobisisobutyronitrile, 12-16 parts of nanomagnetic material, 6-10 parts of N-phenylmaleimide, 30-40 parts of styrene, 25-30 parts of bis(2,4,4-trimethylpentyl)phosphonic acid and 1-1.5 parts of calcium carbonate.
[0006] Preferably, the double-terminated mercapto polyethylene glycol has a Mw of 1000.
[0007] Preferably, the nanomagnetic material is prepared from the following components in parts by weight: 25-30 parts of ferric chloride hexahydrate, 50-60 parts of sodium acetate, 120-150 parts of hexamethylenediamine and 10-15 parts of 3-methacryloxypropyltrimethoxysilane.
[0008] Preferably, the method for preparing the nanomagnetic material comprises the following steps:
[0009] (1) Add ferric chloride hexahydrate to ethylene glycol at an addition amount of 25-30 mg / mL, then add sodium acetate and hexamethylenediamine, mix evenly, and stir in an oil bath to obtain a mixed solution;
[0010] (2) transferring the mixed solution obtained in step (1) into a reaction kettle, heating for reaction, cooling to room temperature to obtain a black powder, washing and drying to obtain nano-iron tetroxide;
[0011] (3) The nano-iron tetroxide obtained in step (2) is added to deionized water in an amount of 15-25 mg / mL, ultrasonically dispersed for 20 minutes, the pH is adjusted to 4, nitrogen is introduced to expel the air, 3-methacryloxypropyltrimethoxysilane is added, the mixture is stirred in a water bath, cooled, washed, dried, and magnetically separated to remove non-magnetic and weakly magnetic substances, thereby obtaining a magnetic nanomaterial.
[0012] Preferably, in step (1), the oil bath stirring temperature is 150-200°C, the speed is 200-300 rpm, and the time is 20-30 min.
[0013] Preferably, in step (2), the heating reaction time is 180-200° C. for 6-10 hours.
[0014] Preferably, in step (3), the water bath heating temperature is 50-60°C, the speed is 60-100 rpm, and the time is 3-4 hours.
[0015] The present invention also provides a method for preparing a composite porous material for recovering tin element in etching solution, which specifically comprises the following steps:
[0016] S1 and 1,2-divinylbenzene are added to anhydrous ethanol, followed by adding double-terminated thiol polyethylene glycol and azobisisobutyronitrile, and the mixture is evenly mixed, nitrogen is introduced to exclude air, and the mixture is heated in a water bath at 50-60° C. for 6-8 hours to obtain a reaction solution;
[0017] S2, adding the nanomagnetic material to the reaction solution obtained in S1, adding N-phenylmaleimide and styrene, stirring evenly, adding bis(2,4,4-trimethylpentyl)phosphonic acid, stirring evenly to obtain a mixed solution;
[0018] S3, adding the mixed solution obtained in S2 to 10-15 times the volume of deionized water, adding sodium dodecyl sulfate in an amount of 0.2-0.3 mg / mL, and then adding calcium carbonate, stirring in a water bath, then heating and stirring, cooling, filtering, washing, and drying to obtain a recycled etching liquid tin element composite porous material.
[0019] Preferably, in S3, the water bath stirring temperature is 40-50°C, the speed is 80-120 rpm, and the time is 15-25 min.
[0020] Preferably, in S3, the heating temperature is continued to be 70-80°C and the heating time is 5-6h.
[0021] The beneficial effects achieved by the present invention are as follows:
[0022] Nano-ferroferric oxide was prepared with ferric chloride hexahydrate and modified with 3-methacryloxypropyltrimethoxysilane to enhance its dispersibility and make it have double bonds. Non-magnetic and weakly magnetic substances were removed by magnetic separation technology to obtain magnetic nanomaterials. After use, they can be recycled and reused by magnetic separation technology, reducing the loss of small particles and improving the regeneration rate. At the same time, they are evenly dispersed inside the material and tightly combined with the adsorption material, enhancing the ability of the porous material to adsorb tin ions, improving the material strength and reducing the loss during use, and further improving the regeneration rate. Double-terminated thiol polyethylene glycol was used to modify 1,2-divinylbenzene as a functional monomer through Markov addition, integrating double bonds, benzene ring structure, polyethylene glycol soft segment, -CSC- and -SH. With magnetic nanomaterials as the core, N-phenylmaleimide and styrene were selected as polymerization monomers for polymerization reaction to form a porous material with a large specific surface area, high strength, multiple adsorption sites and a fast adsorption rate, which is beneficial to the adsorption of tin ions in the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The results of adsorption experiments of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0024] Figure 2 The results of the adsorption time test of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0025] Figure 3 The results of the specific surface area analysis of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0026] Figure 4 The results of desorption experiments of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0027] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0030] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0031] Example 1
[0032] A composite porous material for recycling tin elements in etching liquid is prepared by comprising the following components in parts by weight: 20 parts of 1,2-divinylbenzene, 6 parts of double-terminated mercapto polyethylene glycol, 1.2 parts of azobisisobutyronitrile, 12 parts of nanomagnetic material, 6 parts of N-phenylmaleimide, 30 parts of styrene, 25 parts of bis(2,4,4-trimethylpentyl)phosphonic acid and 1 part of calcium carbonate.
[0033] The nano magnetic material is prepared from the following components in parts by weight: 25 parts of ferric chloride hexahydrate, 50 parts of sodium acetate, 120 parts of hexamethylenediamine and 10 parts of 3-methacryloxypropyltrimethoxysilane.
[0034] The preparation method of nano magnetic material comprises the following steps:
[0035] (1) Add ferric chloride hexahydrate to ethylene glycol at an addition amount of 25 mg / mL, then add sodium acetate and hexamethylenediamine and mix evenly, stir in an oil bath at 150°C and 200 rpm for 20 min to obtain a mixed solution;
[0036] (2) transferring the mixed solution obtained in step (1) into a reaction kettle, heating at 180° C. for 6 h, cooling to room temperature to obtain a black powder, and washing and drying to obtain nano-iron tetroxide;
[0037] (3) The nano-iron tetroxide obtained in step (2) was added to deionized water in an amount of 15 mg / mL, ultrasonically dispersed for 20 min, the pH was adjusted to 4, nitrogen was introduced to expel the air, 3-methacryloxypropyltrimethoxysilane was added, and the mixture was stirred at 60 rpm in a 50°C water bath for 3 h. The mixture was cooled, washed, dried, and magnetically separated to remove non-magnetic and weakly magnetic substances to obtain a magnetic nanomaterial.
[0038] The present invention also provides a method for preparing a composite porous material for recovering tin element in etching solution, which specifically comprises the following steps:
[0039] S1 and 1,2-divinylbenzene were added to anhydrous ethanol, followed by adding double-terminated thiol polyethylene glycol and azobisisobutyronitrile, mixed evenly, nitrogen was introduced to exclude air, and heated in a water bath at 50°C for 6h to obtain a reaction solution;
[0040] S2, adding the nanomagnetic material to the reaction solution obtained in S1, adding N-phenylmaleimide and styrene, stirring evenly, adding bis(2,4,4-trimethylpentyl)phosphonic acid, stirring evenly to obtain a mixed solution;
[0041] S3. Add the mixed solution obtained in S2 to 10 times the volume of deionized water, add sodium dodecyl sulfate at an addition amount of 0.2 mg / mL, and then add calcium carbonate. Stir at 80 rpm in a 40°C water bath for 15 min, then raise the temperature to 70°C and continue heating and stirring for 5 h, cool, filter, wash, and dry to obtain a recycled etching liquid tin element composite porous material.
[0042] Example 2
[0043] A composite porous material for recycling tin elements in etching liquid is prepared by comprising the following components in parts by weight: 30 parts of 1,2-divinylbenzene, 10 parts of double-terminated mercapto polyethylene glycol, 1.5 parts of azobisisobutyronitrile, 16 parts of nanomagnetic material, 10 parts of N-phenylmaleimide, 40 parts of styrene, 30 parts of bis(2,4,4-trimethylpentyl)phosphonic acid and 1.5 parts of calcium carbonate.
[0044] The nano magnetic material is prepared from the following components in parts by weight: 30 parts of ferric chloride hexahydrate, 60 parts of sodium acetate, 150 parts of hexamethylenediamine and 15 parts of 3-methacryloxypropyltrimethoxysilane.
[0045] The preparation method of nano magnetic material comprises the following steps:
[0046] (1) Add ferric chloride hexahydrate at an addition amount of 30 mg / mL to ethylene glycol, then add sodium acetate and hexamethylenediamine and mix evenly, stir at 300 rpm in an oil bath at 200°C for 30 min to obtain a mixed solution;
[0047] (2) The mixed solution obtained in step (1) was transferred to a reaction kettle, heated at 200° C. for 10 h, cooled to room temperature to obtain a black powder, and washed and dried to obtain nano-iron tetroxide;
[0048] (3) The nano-iron tetroxide obtained in step (2) was added to deionized water in an amount of 25 mg / mL, ultrasonically dispersed for 20 min, the pH was adjusted to 4, nitrogen was introduced to expel the air, 3-methacryloxypropyltrimethoxysilane was added, and the mixture was stirred at 100 rpm in a 60°C water bath for 4 h, cooled, washed, dried, and magnetically separated to remove non-magnetic and weakly magnetic substances to obtain a magnetic nanomaterial.
[0049] The present invention also provides a method for preparing a composite porous material for recovering tin element in etching solution, which specifically comprises the following steps:
[0050] S1 and 1,2-divinylbenzene were added to anhydrous ethanol, followed by adding double-terminated thiol polyethylene glycol and azobisisobutyronitrile, mixed evenly, nitrogen was introduced to exclude air, and heated in a water bath at 60°C for 8h to obtain a reaction solution;
[0051] S2, adding the nanomagnetic material to the reaction solution obtained in S1, adding N-phenylmaleimide and styrene, stirring evenly, adding bis(2,4,4-trimethylpentyl)phosphonic acid, stirring evenly to obtain a mixed solution;
[0052] S3. Add the mixed solution obtained in S2 to 15 times the volume of deionized water, add sodium dodecyl sulfate at an addition amount of 0.3 mg / mL, and then add calcium carbonate. Stir at 120 rpm in a 50°C water bath for 25 min, then raise the temperature to 80°C and continue heating and stirring for 6 h, cool, filter, wash, and dry to obtain a recycled etching liquid tin element composite porous material.
[0053] Example 3
[0054] A composite porous material for recycling tin elements in etching liquid is prepared by comprising the following components in parts by weight: 25 parts of 1,2-divinylbenzene, 8 parts of double-terminated mercapto polyethylene glycol, 1.3 parts of azobisisobutyronitrile, 14 parts of nanomagnetic material, 8 parts of N-phenylmaleimide, 35 parts of styrene, 26 parts of bis(2,4,4-trimethylpentyl)phosphonic acid and 1.3 parts of calcium carbonate.
[0055] The nano magnetic material is prepared from the following components in parts by weight: 28 parts of ferric chloride hexahydrate, 55 parts of sodium acetate, 130 parts of hexamethylenediamine and 12 parts of 3-methacryloxypropyltrimethoxysilane.
[0056] The preparation method of nano magnetic material comprises the following steps:
[0057] (1) Add ferric chloride hexahydrate to ethylene glycol at an addition amount of 28 mg / mL, then add sodium acetate and hexamethylenediamine and mix evenly, stir in an oil bath at 170°C and 250 rpm for 25 min to obtain a mixed solution;
[0058] (2) The mixed solution obtained in step (1) was transferred to a reaction kettle, heated at 190° C. for 8 h, cooled to room temperature to obtain a black powder, and washed and dried to obtain nano-iron tetroxide;
[0059] (3) The nano-iron tetroxide obtained in step (2) was added to deionized water in an amount of 20 mg / mL, ultrasonically dispersed for 20 min, the pH was adjusted to 4, nitrogen was introduced to expel the air, 3-methacryloxypropyltrimethoxysilane was added, and the mixture was stirred at 80 rpm in a 55°C water bath for 3.5 h. The mixture was cooled, washed, dried, and magnetically separated to remove non-magnetic and weakly magnetic substances to obtain a magnetic nanomaterial.
[0060] The present invention also provides a method for preparing a composite porous material for recovering tin element in etching solution, which specifically comprises the following steps:
[0061] S1 and 1,2-divinylbenzene were added to anhydrous ethanol, followed by addition of double-terminated thiol polyethylene glycol and azobisisobutyronitrile, mixed evenly, nitrogen was introduced to exclude air, and heated in a water bath at 55°C for 7h to obtain a reaction solution;
[0062] S2, adding the nanomagnetic material to the reaction solution obtained in S1, adding N-phenylmaleimide and styrene, stirring evenly, adding bis(2,4,4-trimethylpentyl)phosphonic acid, stirring evenly to obtain a mixed solution;
[0063] S3. Add the mixed solution obtained in S2 to 12 times the volume of deionized water, add sodium dodecyl sulfate at an addition amount of 0.25 mg / mL, then add calcium carbonate, stir at 100 rpm in a 45°C water bath for 20 min, then raise the temperature to 75°C and continue heating and stirring for 5.5 h, cool, filter, wash, and dry to obtain a recycled etching liquid tin element composite porous material.
[0064] Comparative Example 1
[0065] This comparative example provides a composite porous material for recovering tin element in etching solution, which differs from Example 1 only in that 3-methacryloxypropyltrimethoxysilane is replaced by γ-aminopropyltriethoxysilane in the components, and the remaining components and component contents are the same as those in Example 1.
[0066] Comparative Example 2
[0067] This comparative example provides a composite porous material for recovering tin element in etching solution, which differs from Example 1 only in that the double-terminated mercapto polyethylene glycol in the component is replaced by polyethylene glycol, and the other components and component contents are the same as those in Example 1.
[0068] Experimental example
[0069] 1. Adsorption experiment
[0070] 5 g of the porous material obtained in Example 1-3 and Comparative Example 1-2 was dried at 50° C., and then added into 5 L of etching solution waste liquid with a tin ion concentration of 60 mg / L, respectively, stirred at 300 rpm for 100 min, and allowed to stand for 6 h. The tin ion concentration in the waste liquid was detected and recorded as the final concentration. The adsorption amount was calculated using the following formula:
[0071] Adsorption amount = (initial concentration - final concentration) × solution volume / adsorbent mass.
[0072] Figure 1 It is a result graph of the adsorption experiment of Examples 1-3 and Comparative Examples 1-2 of the present invention. As shown in the figure, the tin ion adsorption amounts of Examples 1-3 and Comparative Examples 1-2 are 52.36 mg / g, 53.16 mg / g, 51.23 mg / g, 30.68 mg / g, and 36.45 mg / g, respectively; the tin ion adsorption amount of Example 1-3 is significantly higher than that of Comparative Examples 1-2, indicating that the use of 3-methacryloxypropyltrimethoxysilane and double-terminated mercapto polyethylene glycol effectively increases the tin ion adsorption amount of the porous material.
[0073] 2. Adsorption time test
[0074] 5 g of the porous material obtained in Example 1-3 and Comparative Example 1-2 was dried at 50° C., and then added into 5 L of etching solution waste liquid with a tin ion concentration of 60 mg / L, respectively, stirred at 300 rpm for 100 min, and allowed to stand for 1 h, 2 h, 3 h, and 4 h. The tin ion concentration in the waste liquid was detected and recorded as the final concentration. The adsorption amount was calculated using the following formula:
[0075] Adsorption amount = (initial concentration - final concentration) × solution volume / adsorbent mass.
[0076] Figure 2 This is a result graph of the adsorption time test of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, it can be seen that the adsorption rate of Examples 1-3 is significantly faster than that of Comparative Examples 1-2, indicating that the use of 3-methacryloxypropyltrimethoxysilane and double-terminated mercapto polyethylene glycol effectively improves the rate at which the porous material adsorbs tin ions.
[0077] 3. Specific surface area analysis
[0078] Using N 2 The adsorption-desorption method was used to analyze Examples 1-3 and Comparative Examples 1-2. After vacuum degassing at 180°C for 6 h, the N 2The adsorption-desorption curves were analyzed and the specific surface area of the samples was calculated using the BET method.
[0079] Figure 3 The results of the specific surface area analysis of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in the figure. The specific surface areas of Examples 1-3 and Comparative Examples 1-2 are 832.4 m 2 / g, 856.3m 2 / g, 812.9m 2 / g, 659.9m 2 / g, 629.7m 2 / g; The specific surface area of Examples 1-3 is significantly higher than that of Comparative Examples 1-2, indicating that the use of 3-methacryloxypropyltrimethoxysilane and double-terminated mercapto polyethylene glycol effectively increases the surface area of the porous material.
[0080] 4. Desorption Experiment
[0081] The adsorbed Example 1-3 was added to a 0.2 mol / L sodium phosphate solution for desorption for 1 h, and then repeatedly washed with deionized water until the leaching solution was neutral. After drying, the tin ion adsorption experiment was performed again to calculate the adsorption amount. This was performed 5 times in total, and the regeneration rate was calculated using the following formula:
[0082] Regeneration rate = nth adsorption amount / 1st adsorption amount × 100%
[0083] Figure 4 It is a result graph of the desorption experiment of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, as the number of experiments increases, the adsorption capacity of the adsorbent shows a downward trend. After 5 cycles of desorption, the regeneration rates of Examples 1-3 and Comparative Examples 1-2 are 86.3%, 82.6%, 85.4%, 53.7% and 68.6%, respectively; the regeneration rate of Example 1-3 is higher than that of Comparative Example 1-2, indicating that the use of 3-methacryloxypropyltrimethoxysilane and double-terminated mercapto polyethylene glycol effectively improves the regeneration rate of the porous material.
[0084] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0085] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A composite porous material for recovering tin element in etching solution, characterized in that: The method comprises the following components in parts by weight: 20-30 parts of 1,2-divinylbenzene, 6-10 parts of double-terminated mercapto polyethylene glycol, 1.2-1.5 parts of azobisisobutyronitrile, 12-16 parts of nanomagnetic material, 6-10 parts of N-phenylmaleimide, 30-40 parts of styrene, 25-30 parts of bis(2,4,4-trimethylpentyl)phosphonic acid and 1-1.5 parts of calcium carbonate; The nano magnetic material is prepared from the following components in parts by weight: 25-30 parts of ferric chloride hexahydrate, 50-60 parts of sodium acetate, 120-150 parts of hexamethylenediamine and 10-15 parts of 3-methacryloxypropyltrimethoxysilane; The method for preparing the composite porous material of tin element recovered from etching liquid specifically comprises the following steps: S1 and 1,2-divinylbenzene are added to anhydrous ethanol, followed by adding double-terminated thiol polyethylene glycol and azobisisobutyronitrile, and the mixture is evenly mixed, nitrogen is introduced to exclude air, and the mixture is heated in a water bath at 50-60° C. for 6-8 hours to obtain a reaction solution; S2, adding the nanomagnetic material to the reaction solution obtained in S1, adding N-phenylmaleimide and styrene, stirring evenly, adding bis(2,4,4-trimethylpentyl)phosphonic acid, stirring evenly to obtain a mixed solution; S3, adding the mixed solution obtained in S2 to 10-15 times the volume of deionized water, adding sodium dodecyl sulfate in an amount of 0.2-0.3 mg / mL, and then adding calcium carbonate, stirring in a water bath, then heating and continuing heating and stirring, cooling, filtering, washing, and drying to obtain a recycled etching liquid tin element composite porous material; The preparation method of the nanomagnetic material specifically comprises the following steps: (1) Add ferric chloride hexahydrate to ethylene glycol at an addition amount of 25-30 mg / mL, then add sodium acetate and hexamethylenediamine, mix evenly, and stir in an oil bath to obtain a mixed solution; (2) transferring the mixed solution obtained in step (1) into a reaction kettle, heating for reaction, cooling to room temperature to obtain a black powder, washing and drying to obtain nano-iron tetroxide; (3) The nano-iron tetroxide obtained in step (2) is added to deionized water in an amount of 15-25 mg / mL, ultrasonically dispersed for 20 minutes, the pH is adjusted to 4, nitrogen is introduced to expel the air, 3-methacryloxypropyltrimethoxysilane is added, the mixture is stirred in a water bath, cooled, washed, dried, and magnetically separated to remove non-magnetic and weakly magnetic substances, thereby obtaining a magnetic nanomaterial.
2. The tin composite porous material for recovering etching liquid according to claim 1, characterized in that: In S3, the water bath stirring temperature is 40-50°C, the speed is 80-120 rpm, and the time is 15-25 min.
3. The tin composite porous material for recovering etching liquid according to claim 2, characterized in that: In S3, the heating is continued to the temperature of 70-80°C and the heating time is 5-6h.
4. The tin composite porous material for recovering etching liquid according to claim 3, characterized in that: In step (1), the oil bath stirring temperature is 150-200°C, the speed is 200-300 rpm, and the time is 20-30 min.
5. The tin composite porous material for recovering etching liquid according to claim 4, characterized in that: In step (2), the heating reaction time is 180-200°C for 6-10 hours.
6. The tin composite porous material for recovering etching liquid according to claim 5, characterized in that: In step (3), the water bath heating temperature is 50-60°C, the speed is 60-100 rpm, and the time is 3-4 hours.