Negative electrode material and preparation method thereof and battery

Through acid solution treatment and nitrogen source compound doping methods, negative electrode materials with excellent microstructure were prepared, which solved the problem of poor performance of negative electrode materials in sodium ion batteries, achieved efficient sodium ion adsorption and transmission, and improved the battery energy density.

CN118666272BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411155130.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The lack of negative electrode materials with good comprehensive performance in existing sodium ion batteries makes it difficult to improve the energy density of sodium ion batteries, especially difficult to balance capacity performance and first-time Coulomb efficiency.

Method used

The hard carbon precursor is treated by purification of the acid solution to build a porous structure, and the doping and carbon coating of nitrogen source compounds is formed to form a negative electrode material with excellent microstructure, improving its adsorption active sites and transport efficiency.

Benefits of technology

It significantly improves the capacity performance and first-time Coulomb efficiency of the negative electrode material, realizes efficient adsorption and transmission of sodium ions, and solves the problem of balance between capacity performance and first-time Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118666272B_ABST
    Figure CN118666272B_ABST
Patent Text Reader

Abstract

The embodiments of the present application relate to a negative electrode material, a preparation method thereof and a battery. The preparation method of the negative electrode material comprises the following steps: S1: a hard carbon precursor is purified by an acid solution, and a first precursor is obtained by washing, filtering and drying; the first precursor comprises an oxygen-containing functional group; S2: the first precursor is added to a mixed solution of an organic solvent and water for a hydrothermal reaction, and a porous second precursor is obtained by washing, filtering and drying; S3: the porous second precursor is added to a solvent, and then a nitrogen source compound solution and an initiator solution are added for a cross-linking reaction, and a third precursor is obtained by washing, filtering and drying; S4: the third precursor is subjected to a carbon coating treatment to obtain a negative electrode material having a coating layer, which can effectively improve the capacity performance and the first coulombic efficiency of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode material and a preparation method thereof, and a battery. Background Art

[0002] As people's awareness of fossil fuel depletion and environmental pollution increases, higher requirements are being placed on sustainable and cost-effective energy storage technologies. Due to the natural abundance of sodium resources, sodium-ion batteries have attracted more and more research and are considered to be a powerful supplement to lithium-ion batteries. Although a large number of positive electrode materials have been developed, there is a lack of negative electrode materials with good comprehensive performance, which hinders the further improvement of the energy density of sodium-ion batteries.

[0003] Hard carbon has the advantages of large interlayer spacing, stable structure, and low operating potential, and is a feasible negative electrode material for sodium ion batteries. Currently, a variety of methods are used to improve the microstructure and electron distribution of hard carbon negative electrode materials to increase their sodium storage capacity, such as increasing the pyrolysis temperature and reducing the heating rate to obtain hard carbon with a more ordered structure and fewer defects, thereby obtaining a higher capacity. However, in practical applications, hard carbon materials still have some problems, such as the difficulty in achieving a balance between capacity performance and first coulombic efficiency. Summary of the invention

[0004] In view of this, the embodiments of the present application provide a negative electrode material, a preparation method thereof, and a battery to solve at least one problem existing in the background technology.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a negative electrode material, the method comprising the following steps:

[0006] S1: Purifying a hard carbon precursor with an acid solution, washing, filtering and drying to obtain a first precursor; the first precursor includes an oxygen-containing functional group;

[0007] S2: adding the first precursor to a mixed solution of an organic solvent and water for hydrothermal reaction, washing, filtering and drying to obtain a porous second precursor;

[0008] S3: adding the porous second precursor into a solvent, then adding a nitrogen source compound solution and an initiator solution to carry out a cross-linking reaction, and washing, filtering and drying to obtain a third precursor;

[0009] S4: performing carbon coating treatment on the third precursor to obtain a negative electrode material having a coating layer.

[0010] In conjunction with the first aspect of the present application, in an optional implementation manner, step S1 satisfies at least one of the following features (1) to (3):

[0011] (1) The hard carbon precursor comprises a biomass-based hard carbon material;

[0012] (2) The acid solution includes at least one of sulfuric acid, nitric acid, hydrofluoric acid, and hydrochloric acid;

[0013] (3) The oxygen-containing functional group includes a carboxyl group and / or a hydroxyl group.

[0014] In conjunction with the first aspect of the present application, in an optional implementation manner, step S2 satisfies at least one of the following features (1) to (6):

[0015] (1) The mass ratio of the first precursor, the organic solvent and the water is (10-100): (10-50): (30-100);

[0016] (2) The organic solvent includes at least one of ethanol, propanol, butanol, ethyl ether, butyl ether, formic acid, and acetic acid;

[0017] (3) The reaction temperature of the hydrothermal reaction is 80°C to 200°C, the heating rate is 0.1°C / min to 5°C / min, and the reaction time is 0.5h to 5h;

[0018] (4) The specific surface area of ​​the porous second precursor is 100 m 2 / g~500m 2 / g;

[0019] (5) The pore size of the porous second precursor is 0.2 nm to 150 nm, wherein the volume of macropores accounts for 60% to 90%, the volume of mesopores accounts for 10% to 30%, and the volume of micropores accounts for 1% to 5%;

[0020] (6) The true density of the porous second precursor is 1.8 g / cm 3 ~2.2g / cm 3 .

[0021] In conjunction with the first aspect of the present application, in an optional implementation manner, step S3 satisfies at least one of the following features (1) to (6):

[0022] (1) The nitrogen source compound includes at least one of acrylamide, phenylalanine, glutamic acid, acrylonitrile and β-nitrostyrene;

[0023] (2) The initiator includes at least one of azobisisobutyronitrile, ammonium persulfate-sodium bisulfite, azobisisoheptylnitrile, and hydrogen peroxide;

[0024] (3) The mass fraction of the nitrogen source compound solution is 0.1%~10%;

[0025] (4) The mass fraction of the initiator solution is 0.01%~10%;

[0026] (5) The solvent includes at least one of water, ethanol, acetone, toluene, ether, N,N'-dimethylformamide, and ethylene glycol monomethyl ether;

[0027] (6) The reaction temperature of the cross-linking reaction is 40°C~250°C, and the reaction time is 1h~10h.

[0028] In conjunction with the first aspect of the present application, in an optional implementation manner, the carbon coating treatment in step S4 includes:

[0029] A carbon source gas and a first inert gas are introduced to perform gas phase coating on the third precursor; the gas phase coating has at least one of the following characteristics: a) the gas phase deposition temperature is 600°C~1000°C; b) the heating rate is 1°C / min~5°C / min; c) the deposition time is 1h~10h; d) the flow rate of the carbon source gas is 0.1L / min~10L / min; e) the flow rate of the first inert gas is 0.1L / min~10L / min; f) the carbon source gas includes alkane and / or olefin compounds; g) the first inert gas includes at least one of argon, nitrogen, and helium.

[0030] In conjunction with the first aspect of the present application, in an optional implementation manner, step S4 satisfies at least one of the following features (1) to (5):

[0031] (1) The thickness of the coating layer of the negative electrode material is 0.001 μm to 0.01 μm;

[0032] (2) The median particle size Dv50 of the negative electrode material is 4 μm to 10 μm;

[0033] (3) The specific surface area of ​​the negative electrode material is 10m 2 / g~20m 2 / g;

[0034] (4) The pore size of the negative electrode material is 0.25 nm to 75 nm, of which the volume of macropores accounts for 15% to 30%, the volume of mesopores accounts for 25% to 50%, and the volume of micropores accounts for 10% to 20%;

[0035] (5) The true density of the negative electrode material is 1.7 g / cm 3 ~2.0g / cm 3 .

[0036] In conjunction with the first aspect of the present application, in an optional implementation manner, the method further includes:

[0037] The negative electrode material is heat-treated under a second inert gas atmosphere; the heat treatment has at least one of the following characteristics: a) the heat treatment temperature is 1000°C~1600°C; b) the insulation time is 1h~10h; c) the heating rate is 0.1°C / min~10°C / min; d) the second inert gas includes at least one of argon, nitrogen, and helium.

[0038] In conjunction with the first aspect of the present application, in an optional implementation manner, the method further includes:

[0039] After the heat treatment, cooling and sieving are performed; wherein the negative electrode material after sieving has at least one of the following characteristics: a) the median particle size is 5 μm to 15 μm; b) the specific surface area is 2 m 2 / g~10m 2 / g; c) pore size is 0.35nm~55nm, of which the volume of macropores accounts for 1%~10%, the volume of mesopores accounts for 15%~20%, and the volume of micropores accounts for 40%~60%; d) true density is 1.4g / cm 3 ~1.6g / cm 3 ; e) The interlayer spacing of the carbon layers is 0.380nm~0.405nm.

[0040] In a second aspect, an embodiment of the present application provides a negative electrode material, which is prepared using the method for preparing a negative electrode material as described in any one of the first aspects.

[0041] In a third aspect, an embodiment of the present application provides a battery, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode material prepared by the preparation method as described in any one of the first aspect, or comprises the negative electrode material as described in the second aspect.

[0042] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0043] The negative electrode material, preparation method and battery provided in the embodiments of the present application are as follows: first, the hard carbon precursor is purified by an acid solution, which can remove metal and / or non-metal impurities on the one hand, and the acid solution as an oxidant can increase oxygen-containing functional groups in the carbon skeleton on the other hand; secondly, porous carbon is constructed by a hydrothermal reaction in an organic solvent aqueous solution to form a porous second precursor, which can provide sufficient space for the doping of nitrogen source compounds; furthermore, the nitrogen source compound forms positively charged free radicals under the action of an initiator, and enters the internal carbon interlayer through the surface defects of the porous second precursor and the pores in the material to chemically cross-link with the oxygen-containing functional groups, thereby stably and accurately doping nitrogen atoms into the internal structure of the material, which can provide a large number of adsorption active sites for active ions and expand the graphite layer spacing, thereby effectively improving the adsorption efficiency and transmission efficiency of active ions; then, the third precursor is carbon-coated to modify the surface defects of the third precursor; this can effectively improve the capacity performance and first coulomb efficiency of the negative electrode material.

[0044] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0046] Figure 1 A schematic diagram of a process for preparing a negative electrode material provided in an embodiment of the present application;

[0047] Figure 2 This is a pore size distribution diagram of the negative electrode material prepared in Example 1;

[0048] Figure 3 This is a scanning electron microscope image of the negative electrode material prepared in Example 1;

[0049] Figure 4 This is a transmission electron microscope image of the negative electrode material prepared in Example 1;

[0050] Figure 5 The charge and discharge curve of the battery made of the negative electrode material prepared in Example 1;

[0051] Figure 6 The charge and discharge curve of the battery made of the negative electrode material prepared in Comparative Example 1;

[0052] Figure 7 The charge and discharge curve of the battery made of the negative electrode material prepared in Comparative Example 2;

[0053] Figure 8 This is the charge and discharge curve of the battery made of the negative electrode material prepared in Comparative Example 3. DETAILED DESCRIPTION

[0054] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is described in detail by combining the accompanying drawings and listing specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional experimental conditions. The reagents and raw materials used in the present invention are commercially available unless otherwise specified.

[0055] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.

[0056] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0057] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.

[0058] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.

[0059] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values.

[0060] In the related art, heteroatom doping is a feasible method to adjust the electron density of materials. Heteroatom doping enhances the affinity for active ions (such as sodium ions) by destroying the π-π conjugated system and forming electronegative functional groups. Heteroatom doping of hard carbon materials can not only improve the conductivity of hard carbon, but also introduce more active sites for adsorbing active ions and improve the capacity performance of the material. However, the strong adsorption caused by heteroatom doping may increase the so-called "trap effect", resulting in an uncontrollable proportion of defective parts in the material, thereby reducing the first coulombic efficiency. Therefore, a balance needs to be struck between capacity performance and first coulombic efficiency.

[0061] Based on this, the present application embodiment provides a method for preparing a negative electrode material. Figure 1 The method for preparing the modified positive electrode material provided in the embodiment of the present application comprises the following steps:

[0062] S1: purifying the hard carbon precursor with an acid solution, washing, filtering and drying to obtain a first precursor; the first precursor includes an oxygen-containing functional group;

[0063] S2: adding the first precursor to a mixed solution of an organic solvent and water for hydrothermal reaction, and obtaining a porous second precursor through washing, filtering and drying;

[0064] S3: adding the porous second precursor into a solvent, then adding a nitrogen source compound solution and an initiator solution, performing a cross-linking reaction, and obtaining a third precursor through washing, filtering and drying;

[0065] S4: performing carbon coating treatment on the third precursor to obtain a negative electrode material having a coating layer.

[0066] In the embodiment of the present application, the hard carbon precursor is first purified by an acid solution. On the one hand, metal and / or non-metal impurities can be removed. On the other hand, the acid solution can act as an oxidant to add oxygen-containing functional groups to the carbon skeleton. The oxygen-containing functional groups are used to chemically crosslink with the nitrogen source compound to achieve precise nitrogen doping. Secondly, a hydrothermal reaction is carried out in an organic solvent aqueous solution. The organic solvent is heated and volatilized to generate steam, thereby destroying the surface and internal structure of the material to construct a porous structure, increase the specific surface area, expose more oxygen-containing functional groups, and form a porous second precursor, which can provide sufficient doping for the nitrogen source compound. Space, and further, the nitrogen source compound loses an electron under the action of the initiator to form a positively charged free radical, and enters the internal carbon layer through the surface defects of the porous second precursor and the pores in the material to undergo sufficient chemical cross-linking with the oxygen-containing functional groups, thereby stably and accurately doping the nitrogen atoms in the internal structure of the material, which can provide a large number of adsorption active sites for active ions and expand the distance between graphite layers, thereby effectively improving the adsorption efficiency and transmission efficiency of active ions. Then, the third precursor is carbon-coated to modify the surface defects of the third precursor, thereby effectively improving the capacity performance and first coulombic efficiency of the negative electrode material.

[0067] In some embodiments, the hard carbon precursor may include a biomass-based hard carbon material, because the biomass-based hard carbon material has a unique microstructure, has advantages such as self-doping effect, multiple active sites, low cost, and a wide range of sources. Specifically, the hard carbon precursor may include at least one of coconut shell, bamboo, almond shell, lotus stem, hazelnut shell, cellulose, and lignin. The above-mentioned biomass-based hard carbon materials have a wide range of sources and low costs. In practical applications, the biomass-based hard carbon precursor can be first ball-milled and then sieved through a 50-mesh to 500-mesh sieve to obtain a hard carbon precursor.

[0068] In some embodiments, the acid solution may include at least one of sulfuric acid, nitric acid, hydrofluoric acid, and hydrochloric acid. In practical applications, the acid solution can be obtained by diluting the concentrated acid solution according to the required mass fraction. When the concentration of the acid solution is low, the oxidizability is relatively low, and more oxygen-containing functional groups cannot be introduced into the hard carbon precursor. When the concentration of the acid solution is high, it is easy to damage the structure of the hard carbon precursor itself. Therefore, in some specific embodiments, the mass fraction of the acid solution can be 1% to 18%, for example, 1%, 3%, 5%, 8%, 10%, 12%, 15%, 18% or any value between any two of the above numerical ranges. Controlling the mass fraction of the acid solution within the above range can introduce sufficient oxygen-containing functional groups into the hard carbon precursor, thereby facilitating a better cross-linking reaction with the nitrogen source compound in the subsequent step S3.

[0069] In some embodiments, the oxygen-containing functional group includes a carboxyl group and / or a hydroxyl group. The carboxyl group and / or the hydroxyl group can undergo a good cross-linking reaction with the amino functional group of the nitrogen source compound, so that nitrogen can be accurately doped into the first precursor in the subsequent step S3.

[0070] In some embodiments, performing the above step S2 may specifically include: adding the first precursor to a hydrothermal reactor containing an organic solvent for hydrothermal reaction, washing, filtering and drying to obtain a porous second precursor. The mass ratio of the first precursor, the organic solvent and water may be (10-100): (10-50): (30-100), for example, (10:50:100), (20:50:100), (30:50:100), (40:50:100), (50:50:100) or any other mass ratio within the above range. Controlling the mass ratio of the first precursor, the organic solvent and water within the above range can make the hydrothermal reaction more sufficient, facilitate the control of the formation of pores, and thus make the pores in the obtained porous second precursor uniform and the number and pore size of the pores appropriate.

[0071] In some embodiments, the organic solvent includes a volatile solvent, and the specific organic solvent may include at least one of ethanol, propanol, butanol, ether, butyl ether, formic acid, and acetic acid. The above organic solvents have good volatility. In the hydrothermal reaction, it is easier to generate steam by heating and volatilizing the organic solvent to destroy the surface and internal structure of the material to construct a porous structure, so that the specific surface area of ​​the porous second precursor formed is further increased, thereby exposing more oxygen-containing functional groups, which is conducive to the sufficient doping of the nitrogen source compound in the subsequent step S3, thereby better improving the capacity performance of the final negative electrode material.

[0072] When the reaction temperature of the hydrothermal reaction in step S2 is low, the organic solvent cannot be fully volatilized well, so that the porous structure cannot be well constructed to form a porous second precursor suitable for pores. When the reaction temperature of the hydrothermal reaction is high, the organic solvent evaporates faster, which is not conducive to forming a porous second precursor with uniform pores and suitable pore size, and the controllability of the hydrothermal reaction is also poor. Therefore, in some embodiments, the reaction temperature of the hydrothermal reaction can be 80°C~200°C, for example, 80°C, 90°C, 100°C, 120°C, 130°C, 150°C, 170°C, 190°C, 200°C or any value between any two of the above numerical ranges. In this way, the controllability of the hydrothermal reaction is good, and it is easy to form a porous second precursor suitable for pores, thereby exposing more oxygen-containing functional groups, which is conducive to sufficient cross-linking reaction with the nitrogen source compound.

[0073] It can be understood that the heating rate and reaction time of the hydrothermal reaction are closely related to the treatment effect of the hydrothermal reaction. In some specific embodiments, the heating rate of the hydrothermal reaction can be 0.1°C / min~5°C / min, for example, 0.1°C / min, 0.2°C / min, 0.3°C / min, 0.4°C / min, 5°C / min or any value between any two numerical ranges, and the reaction time of the hydrothermal reaction can be 0.5h~5h, for example, 0.5h, 1h, 2h, 3h, 4h, 5h or any value between any two numerical ranges. Controlling the heating rate and reaction time of the hydrothermal reaction in the above ranges can make the uniformity of solution heating in the hydrothermal reaction better, the hydrothermal reaction is more fully carried out, and then it is easy to control the formation of a porous second precursor with more suitable pores and specific surface area to prepare a high-quality negative electrode material.

[0074] It can be understood that by controlling the conditions of the hydrothermal reaction, a porous second precursor having performance parameters that meet expected conditions can be formed, and the performance of the porous second precursor is related to the performance of the negative electrode material that is ultimately formed.

[0075] In some embodiments, the pore size of the porous second precursor can be 0.2nm~150nm, of which the volume of macropores accounts for 60%~90%, the volume of mesopores accounts for 10%~30%, and the volume of micropores accounts for 1%~5%. In this embodiment, the pores in the porous second precursor are mainly mesopores and macropores, and the volume of macropores accounts for more than 60%, so that more oxygen-containing functional groups can be exposed, providing sufficient space and conditions for the doping of nitrogen source compounds, thereby enabling the final negative electrode material to have better capacity performance.

[0076] It should be noted that in the pore size test of the present application, the pore size of micropores is less than 2 nm, the pore size of mesopores (also called mesopores) is between 2 nm and 50 nm, and the pore size of macropores is greater than 50 nm.

[0077] By controlling the conditions of the hydrothermal reaction, the pore size and the number of pores in the porous second precursor can be controlled, so that a porous second precursor with a suitable specific surface area can be obtained. In some embodiments, the specific surface area of ​​the porous second precursor can be 100 m 2 / g~500m 2 / g. By controlling the specific surface area of ​​the porous second precursor within the above range, more oxygen-containing functional groups can be exposed, providing more sufficient space and conditions for the doping of the nitrogen source compound, thereby enabling the final negative electrode material to have better capacity performance.

[0078] In some embodiments, the true density of the porous second precursor is 1.8 g / cm 3 ~2.2g / cm 3The porous second precursor with a true density within the above range can be used to prepare a negative electrode material with higher quality.

[0079] In some embodiments, executing step S3 may specifically include the following steps: first, adding the porous second precursor to a hydrothermal reactor filled with an organic solvent, then sequentially adding the prepared nitrogen source compound solution and initiator solution and starting to stir to make the solution system evenly dispersed, while introducing an inert gas, then heating to a set temperature, and then cooling to room temperature after the reaction is complete, and obtaining a third precursor after washing, filtering and drying.

[0080] In this embodiment, the introduction of inert gas can avoid the introduction of impurities such as air, and the cross-linking reaction can be carried out in an environment isolated from the outside world, which can make the cross-linking reaction more complete and the cross-linking effect better, thereby making it possible to improve the performance of the negative electrode material by nitrogen doping.

[0081] There is no particular limitation on the types of the nitrogen source compound, initiator and solvent in step S3, and they can be selected according to actual needs.

[0082] The "nitrogen source compound" refers to a compound for providing nitrogen. Exemplarily, the nitrogen source compound may include at least one of acrylamide, phenylalanine, glutamic acid, acrylonitrile, and β-nitrostyrene.

[0083] In some specific embodiments, the mass fraction of the nitrogen source compound solution may be 0.1% to 10%, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any value between any two of the above ranges. This can promote sufficient cross-linking reaction between the nitrogen source compound and the oxygen-containing functional groups in the porous second precursor, thereby improving the performance of the final negative electrode material.

[0084] The initiator is known to those skilled in the art as long as it can achieve the initiation reaction. For example, the initiator may include at least one of azobisisobutyronitrile, ammonium persulfate-sodium bisulfite, azobisisoheptylnitrile, and hydrogen peroxide.

[0085] In some specific embodiments, the mass fraction of the initiator solution may be 0.01% to 10%, for example, 0.01%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any value between any two of the above ranges. In this way, the nitrogen source compound and the oxygen-containing functional group may be better induced to react with each other, thereby improving the performance of the final negative electrode material.

[0086] Illustratively, the solvent may include at least one of water, ethanol, acetone, toluene, diethyl ether, N,N'-dimethylformamide, and ethylene glycol monomethyl ether.

[0087] In some embodiments, the reaction temperature of the cross-linking reaction in step S3 can be 40°C to 250°C, for example, 40°C, 50°C, 80°C, 100°C, 120°C, 150°C, 200°C, 230°C, 250°C or any value between any two of the above numerical ranges. The reaction time can be 1h to 10h, for example, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or any value between any two of the above numerical ranges. By controlling the reaction temperature and reaction time of the cross-linking reaction within the above ranges, the oxygen-containing functional groups and nitrogen source compounds in the porous second precursor can be quickly, evenly and fully cross-linked under the action of the initiator, thereby achieving a better cross-linking effect, and further improving the performance of the obtained negative electrode material.

[0088] The washing, filtration and drying in the above steps S2 and S3 can be carried out by methods well known to those skilled in the art, which will not be described in detail here.

[0089] In some embodiments, the carbon coating treatment in step S4 may include: introducing a carbon source gas and a first inert gas to perform gas phase coating on the third precursor. Through gas phase coating, carbon can be deposited on the interface of the third precursor, thereby modifying the surface defects of the third precursor, obtaining a negative electrode material with a carbon coating layer, and thereby improving the first coulombic efficiency.

[0090] Exemplarily, the carbon source gas may include alkane and / or olefin compounds, and specifically, the carbon source gas may include at least one of methane, ethane, ethylene, and acetylene. By chemical vapor deposition, gas-phase small molecule alkane or olefin compounds are cracked so that they can be uniformly deposited on the third precursor interface, modifying the defects on the surface of the hard carbon material and reducing the specific surface area, thereby better improving the first coulombic efficiency.

[0091] For example, the first inert gas may include at least one of argon, nitrogen, and helium, which is used to mix with the carbon source gas to control the reaction pressure within a suitable range and protect the third precursor during the vapor deposition process. In some specific embodiments, the flow rate of the first inert gas may be 0.1 L / min to 10 L / min, which can better assist in adjusting the reaction pressure and protecting the third precursor.

[0092] Specifically, the third precursor can be added to the vapor deposition furnace for vapor coating, for example, the temperature is increased from room temperature to a set vapor deposition temperature at a heating rate of 1°C / min to 5°C / min. After reaching the set temperature, the carbon source gas and the first inert gas are introduced for vapor coating.

[0093] In some specific embodiments, the vapor deposition temperature in the vapor coating may be 600°C to 1000°C, for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C or any value between any two of the above ranges. In this way, the carbon source gas can be fully cracked to better modify the surface defects of the third precursor, thereby further improving the first coulombic efficiency and obtaining a higher quality negative electrode material.

[0094] At the above vapor deposition temperature, in some specific embodiments, the vapor deposition time may be 1 h to 10 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h or any value between any two of the above ranges. In this way, carbon can be more evenly and fully deposited on the interface of the third precursor, thereby further enhancing the modification effect of the vapor coating on the surface defects of the third precursor.

[0095] At the above vapor deposition temperature and / or vapor deposition time, in some specific embodiments, the flow rate of the carbon source gas is 0.1L / min to 10L / min, for example, 0.1L / min, 1L / min, 2L / min, 3L / min, 4L / min, 5L / min, 6L / min, 7L / min, 8L / min, 9L / min, 10L / min or any value between any two of the above numerical ranges. In this way, sufficient carbon source supply can be guaranteed, so that the carbon coating layer formed in the negative electrode material is more uniform, and the performance of the obtained negative electrode material is better.

[0096] By controlling the conditions of gas phase coating, parameters such as the thickness of the coating layer, the median particle size of the negative electrode material, the specific surface area of ​​the negative electrode material after coating, and the pore size distribution of the negative electrode material can be controlled.

[0097] In some embodiments, the thickness of the coating layer of the negative electrode material is 0.001 μm to 0.01 μm. By controlling the coating layer within the above range, the surface defects of the material can be better modified by the coating layer while avoiding the coating layer affecting the transmission of active ions, thereby better improving the first coulombic efficiency.

[0098] In some embodiments, the median particle size Dv50 of the negative electrode material is 4 μm to 10 μm. Controlling the median particle size Dv50 of the negative electrode material within the above range can improve the performance of the negative electrode sheet prepared using the negative electrode material.

[0099] In some embodiments, the specific surface area of ​​the negative electrode material having the coating layer is 10 m 2 / g~20m 2 / g, the surface defects of the third precursor can be modified by gas phase coating to reduce the specific surface area. Controlling the specific surface area within the above range can make the performance of the negative electrode sheet prepared by the negative electrode material better.

[0100] In some embodiments, the pore size of the negative electrode material with the coating layer is 0.25nm~75nm, of which the volume of macropores accounts for 15%~30%, the volume of mesopores accounts for 25%~50%, and the volume of micropores accounts for 10%~20%. After the gas phase coating treatment, the particle size of the negative electrode material is significantly reduced, the pores in the negative electrode material shrink, the volume of macropores in the negative electrode material is significantly reduced relative to the porous second precursor, and the volume of mesopores and micropores is significantly increased, thereby providing better storage space for active ions, thereby improving the capacity performance of the negative electrode material.

[0101] In some embodiments, the true density of the negative electrode material is 1.7 g / cm 3 ~2.0g / cm 3 The true density within the above range can make the performance of the negative electrode sheet prepared by using the negative electrode material better.

[0102] In some embodiments, the method for preparing the negative electrode material may further include: heat treating the negative electrode material under a second inert gas atmosphere.

[0103] In the embodiment of the present application, the negative electrode material is carbonized by heat treatment, which can induce the growth and winding of graphite-like crystallites to form more microporous structures, provide more storage space for sodium ions, improve the capacity performance of the negative electrode material, and further reduce surface defects, thereby further improving the first coulombic efficiency.

[0104] Specifically, the negative electrode material can be placed in a high-temperature carbonization furnace, and heated from room temperature to a set temperature under the protection of a second inert gas atmosphere, and then heat treated. The second inert gas can include, for example, at least one of argon, nitrogen, and helium, which is used to better protect the negative electrode material from oxidation during the heat treatment process.

[0105] It can be understood that when the temperature of the heat treatment is low, it is not possible to effectively form more microporous structures in the negative electrode material and reduce the surface defects of the negative electrode material, and thus the performance of the negative electrode material cannot be effectively improved. When the temperature of the heat treatment is high, the excessive growth of graphite-like crystallites easily leads to complete closure of the pores, which is not conducive to improving the capacity performance of the negative electrode material. Therefore, in some embodiments, the temperature of the heat treatment can be 1000°C to 1600°C, for example, it can be 1000°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C or any value between any two of the above numerical ranges. In this way, the capacity performance and the first coulombic efficiency of the negative electrode material can be better improved, and high-quality negative electrode materials can be prepared.

[0106] The holding time of the heat treatment is closely related to the effect of the heat treatment. Therefore, in some embodiments, the holding time of the heat treatment can be 1 h to 10 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h or any value between any two of the above ranges. Controlling the holding time within the above range can further improve the quality of the prepared negative electrode material.

[0107] The heating rate of the heat treatment is closely related to the effect of the heat treatment. Therefore, in some embodiments, the heating rate of the heat treatment can be 0.1°C / min to 10°C / min, for example, 0.1°C / min, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or any value between any two of the above ranges. Controlling the heating rate within the above range can further improve the quality of the prepared negative electrode material.

[0108] In some embodiments, the method for preparing the negative electrode material may further include: cooling and sieving after the heat treatment, so as to obtain a negative electrode material with suitable particle size and excellent performance.

[0109] In some specific embodiments, the median particle size of the negative electrode material after sieving is 5 μm to 15 μm, so that the negative electrode sheet prepared by using the negative electrode material can have better performance.

[0110] In some specific embodiments, the specific surface area of ​​the negative electrode material after sieving is 2 m 2 / g~10m 2 / g. In this way, the negative electrode sheet prepared by using the negative electrode material can have better performance.

[0111] In some specific embodiments, the pore size of the negative electrode material after sieving is 0.35nm~55nm, of which the volume of macropores accounts for 1%~10%, the volume of mesopores accounts for 15%~20%, and the volume of micropores accounts for 40%~60%. After sieving, the particle size of the negative electrode material is further reduced, the volume of micropores in the negative electrode material accounts for the largest proportion, the volume of mesopores accounts for a moderate proportion, and the volume of macropores accounts for a small proportion, which can make the capacity performance of the negative electrode material better and the first coulomb efficiency higher, so that the negative electrode sheet prepared using the negative electrode material has better performance.

[0112] In some specific embodiments, the true density of the negative electrode material after sieving is 1.4 g / cm 3 ~1.6g / cm 3When the true density is within the above range, the negative electrode sheet prepared by using the negative electrode material can have better performance.

[0113] In some specific embodiments, the interlayer spacing of the carbon layer of the negative electrode material after the screening process is 0.380nm~0.405nm. The interlayer spacing of the carbon layer within the above range can better improve the transmission of active ions, thereby further improving the performance of the negative electrode material.

[0114] Based on this, an embodiment of the present application further provides a negative electrode material, which is prepared using the preparation method of the negative electrode material described in any of the above embodiments.

[0115] It should be understood that all the features and advantages of the method for preparing the negative electrode material described in the above embodiments are also applicable to the negative electrode material in the embodiments of the present application, and will not be described one by one here.

[0116] Based on this, an embodiment of the present application also provides a battery, including a negative electrode plate, the negative electrode plate includes a negative electrode material prepared by the preparation method of the negative electrode material described in any of the above embodiments or includes the negative electrode material described in the above embodiments.

[0117] It should be understood that since the negative electrode plate of the battery in the embodiment of the present application includes the negative electrode material prepared by the preparation method of the negative electrode material described in any of the above embodiments or includes the negative electrode material described in the above embodiments, the beneficial effects of the negative electrode material described in any of the above embodiments are applicable to the battery.

[0118] In some embodiments, the negative electrode plate may include a negative electrode current collector and a negative electrode active material layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer may include a negative electrode material prepared by the preparation method of the negative electrode material described in any of the above embodiments or include the negative electrode material described in the above embodiments.

[0119] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active material layer is disposed on either or both of the two facing surfaces of the negative electrode current collector.

[0120] In some embodiments, the battery may be a secondary battery, and the secondary battery may be a lithium-ion secondary battery or a sodium-ion secondary battery. Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0121] The technical solution of the present application is further described below in combination with a plurality of embodiments and comparative examples. Example 1

[0122] The preparation of the negative electrode material in this embodiment includes the following steps:

[0123] S101: ball-milling and sieving the coconut shell carbon precursor, taking the sieve material for purification in a 10% by mass sulfuric acid solution, washing, filtering and drying to obtain a first precursor;

[0124] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol and water for hydrothermal reaction, and heating the temperature to 80°C at a heating rate of 0.1°C / min for 0.5h, wherein the mass ratio of the first precursor, ethanol and water is 10:10:30. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0125] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor containing an ethanol solution, and add a 5% by mass acrylamide solution and a 0.3% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 100°C at a rate of 1°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 1 hour. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0126] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 800°C at a rate of 2°C / min and then N is introduced. 2 Gas and methane for vapor deposition, where N 2 The flow rate is 3 L / min, the methane flow rate is 6 L / min, the deposition time is 4 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0127] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1300°C at a rate of 2°C / min under atmosphere protection and the insulation time was 3h. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening. Example 2

[0128] The preparation of the negative electrode material in this embodiment includes the following steps:

[0129] S101: ball-milling and sieving the bamboo carbon precursor, taking the sieve material for purification in a nitric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0130] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with butanol and water for hydrothermal reaction, and heating the temperature to 200°C at a heating rate of 5°C / min for 5 hours, wherein the mass ratio of the first precursor, butanol and water is 50:10:30. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0131] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor containing an ethanol solution, and add a 6% by mass acrylonitrile solution and a 0.5% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 100°C at a rate of 1°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 2 hours. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0132] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 1000°C at a rate of 3°C / min and then N is introduced. 2 Gas and acetylene for vapor deposition, where N 2 The flow rate was 8 L / min, the methane flow rate was 10 L / min, the deposition time was 4 h, and the negative electrode material with a coating layer was obtained after cooling to room temperature;

[0133] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1400°C at a rate of 2.5°C / min under atmosphere protection and the insulation time was 3h. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening. Example 3

[0134] The preparation of the negative electrode material in this embodiment includes the following steps:

[0135] S101: ball-milling and sieving the hazelnut shell carbon precursor, taking the sieve material for purification in a 10% by mass sulfuric acid solution, washing, filtering and drying to obtain a first precursor;

[0136] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol and water for hydrothermal reaction, and heating the temperature to 90°C at a heating rate of 0.2°C / min for 1 hour, wherein the mass ratio of the first precursor, ethanol and water is 100:10:30. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0137] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor containing an ethanol solution, and add a 5% by mass fraction phenylalanine solution and a 0.3% by mass fraction hydrogen peroxide solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 80°C at a rate of 1°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 0.5h. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0138] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 900°C at a rate of 3°C / min and then N is introduced. 2 Gas and ethylene are vapor deposited, where N 2 The flow rate is 3 L / min, the ethylene flow rate is 6 L / min, the deposition time is 3 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0139] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1400°C at a rate of 3°C / min under atmosphere protection and kept at this temperature for 6 hours. After the temperature was kept at this temperature, the material was cooled to room temperature and the treated negative electrode material was obtained through screening. Example 4

[0140] The preparation of the negative electrode material in this embodiment includes the following steps:

[0141] S101: ball-milling and sieving the cellulose carbon precursor, taking the sieve material for purification in a nitric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0142] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol and water for hydrothermal reaction, and heating the temperature to 120°C at a heating rate of 1°C / min for 2 hours, wherein the mass ratio of the first precursor, ethanol and water is 100:50:30. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0143] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor filled with ethanol solution, and add 7% by mass phenylalanine solution and 1% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 120°C at a rate of 2°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 0.5h. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0144] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 1000°C at a rate of 2°C / min and then N is introduced. 2 Gas and ethylene are vapor deposited, where N 2 The flow rate is 6 L / min, the ethylene flow rate is 8 L / min, the deposition time is 3 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0145] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1400°C at a rate of 2°C / min under atmosphere protection and the insulation time was 6 hours. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening. Example 5

[0146] The preparation of the negative electrode material in this embodiment includes the following steps:

[0147] S101: ball-milling and sieving the almond shell carbon precursor, taking the sieve material for purification in a nitric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0148] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with butanol and water for hydrothermal reaction, and heating the temperature to 150°C at a heating rate of 0.5°C / min for 3 hours, wherein the mass ratio of the first precursor, butanol and water is 100:50:40. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0149] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor containing an ethanol solution, and add a 10% by mass acrylonitrile solution and a 0.1% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2Air impurities were removed, and then the temperature was raised to 120°C at a rate of 2°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 0.5h. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0150] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 900°C at a rate of 2°C / min and then N is introduced. 2 Gas and ethane for vapor deposition, where N 2 The flow rate is 6 L / min, the ethane flow rate is 8 L / min, the deposition time is 3 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0151] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1500°C at a rate of 2°C / min under atmosphere protection and the insulation time was 6 hours. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening.

[0152] Comparative Example 1

[0153] The preparation of the negative electrode material in this comparative example includes the following steps:

[0154] S101: ball-milling and sieving the coconut shell carbon precursor, taking the sieve material for purification in a nitric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0155] S103: Add the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol solution, and add 7% by mass phenylalanine solution and 1% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 120°C at a rate of 2°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 0.5h. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0156] S104: Add the third precursor obtained in step S103 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 1000°C at a rate of 2°C / min and then N is introduced. 2 Gas and ethylene are vapor deposited, where N 2 The flow rate is 6 L / min, the ethylene flow rate is 8 L / min, the deposition time is 3 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0157] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1400°C at a rate of 2°C / min under atmosphere protection and the insulation time was 6 hours. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening.

[0158] Comparative Example 2

[0159] The preparation of the negative electrode material in this comparative example includes the following steps:

[0160] S101: ball-milling and sieving the hazelnut shell carbon precursor, taking the sieve material for purification in a sulfuric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0161] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol and water for hydrothermal reaction, and heating the temperature to 80°C at a heating rate of 0.1°C / min for 0.5h, wherein the mass ratio of the first precursor, ethanol and water is 100:50:50. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0162] S104: Add the porous second precursor obtained in step S102 into a vapor deposition furnace for vapor coating. The vapor deposition furnace is heated to 1000°C at a rate of 2°C / min and then N is introduced. 2 Gas and ethylene are vapor deposited, where N 2 The flow rate is 6 L / min, the ethylene flow rate is 8 L / min, the deposition time is 3 h, and the negative electrode material with a coating layer is obtained after cooling to room temperature;

[0163] S105: Place the negative electrode material obtained in step S104 into a high temperature carbonization furnace for heat treatment. 2 The temperature was raised to 1400°C at a rate of 2°C / min under atmosphere protection and the insulation time was 6 hours. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening.

[0164] Comparative Example 3

[0165] The preparation of the negative electrode material in this comparative example includes the following steps:

[0166] S101: ball-milling and sieving the cellulose carbon precursor, taking the sieve material for purification in a nitric acid solution with a mass fraction of 18%, washing, filtering and drying to obtain a first precursor;

[0167] S102: adding the first precursor obtained in step S101 into a hydrothermal reactor filled with ethanol and water for hydrothermal reaction, and heating the temperature to 80°C at a heating rate of 0.1°C / min for 0.5h, wherein the mass ratio of the first precursor, ethanol and water is 100:50:100. After the reaction is completed, washing, filtering and drying are performed to obtain a porous second precursor;

[0168] S103: Add the porous second precursor obtained in step S102 into a hydrothermal reactor filled with ethanol solution, and add 7% by mass phenylalanine solution and 1% by mass azobisisobutyronitrile solution in sequence, start stirring to make the solution system evenly dispersed, and introduce N 2 Air impurities were removed, and then the temperature was raised to 120°C at a rate of 2°C / min. After reaching the reaction temperature, the cross-linking reaction was carried out for 0.5h. After the reaction was complete, the mixture was cooled to room temperature, and the third precursor was obtained after washing, filtering and drying.

[0169] S105: The third precursor obtained in step S103 is placed in a high temperature carbonization furnace for heat treatment at N 2 The temperature was raised to 1400°C at a rate of 2°C / min under atmosphere protection and the insulation time was 6 hours. After the insulation was completed, it was cooled to room temperature and the treated negative electrode material was obtained through screening.

[0170] The performance of the negative electrode materials obtained in the above embodiments and comparative examples was tested:

[0171] (1) Pore size and specific surface area test of negative electrode materials

[0172] The pore size and specific surface area of ​​the negative electrode material were tested using a rapid specific surface and pore size analyzer. The specific test steps were as follows: 100 mg of pretreated adsorbent sample was placed in a sample tube, and the whole system was vacuumed and degassed first, and then the sample tube was immersed in a liquid nitrogen bath and filled with an appropriate amount of gas. By measuring the amount of nitrogen adsorbed by the sample under a series of nitrogen partial pressures P / P0, the nitrogen isothermal adsorption or desorption curve can be drawn, and then the specific surface area can be calculated. The specific surface area and pore size distribution were calculated by the Brunauer-Emmett-Teller (BET) method and the density functional theory (DFT) method, respectively. The test results are shown in Table 1.

[0173] (2) Battery electrochemical performance test

[0174] The negative electrode materials obtained in the above examples and comparative examples were assembled into half-cells to test the electrochemical performance of the battery. The specific operation steps are as follows: weigh 19g of negative electrode material, 5.0g of conductive carbon black (super-P) and 5.0g of binder (2.5% sodium carboxymethyl cellulose), stir magnetically at a speed of 500rpm to mix the slurry, apply it on the current collector and place it in a vacuum oven at 80℃ to dry for 8h to remove moisture to obtain a pole piece, with a sodium sheet as the counter electrode, a polypropylene microporous membrane as the separator, and an electrolyte of 1M NaClO 4 A battery to be tested was obtained by preparing a solution in a three-component mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC) and propylene carbonate (PC) in a volume ratio of 1:1:1.

[0175] The battery is tested to obtain the battery's first discharge specific capacity, first charge specific capacity and first coulombic efficiency.

[0176] 0.1C discharge capacity test: 0.1C constant current discharge to 0V, let stand for 5 minutes. The capacity measured in this step is the 0.1C discharge capacity (denoted as C0), which is the first discharge specific capacity.

[0177] 0.1C charging capacity: 0.1C constant current and constant voltage charging to 2.0V, the cut-off current is 0.05C, and it is left to stand for 5 minutes. The capacity measured in this step is the 0.1C charging capacity (denoted as C1), which is the first charging specific capacity.

[0178] The first coulombic efficiency is: C1 / C0.

[0179] The test results are shown in Table 1.

[0180] It can be seen from the test results of Examples 1 to 5 and Comparative Examples 1 to 3 in Table 1 that in the present application, the hard carbon precursor is first purified by an acid solution, which can remove metal and / or non-metal impurities on the one hand, and on the other hand, the acid solution can increase oxygen-containing functional groups in the carbon skeleton as an oxidant. Secondly, porous carbon is constructed by a hydrothermal reaction in an organic solvent solution to form a porous second precursor with a significantly increased specific surface area to expose more oxygen-containing functional groups, which can provide sufficient space for the doping of nitrogen source compounds. Furthermore, under the action of the initiator, the nitrogen source compound loses an electron to form a positively charged free radical, and enters the internal carbon layer through the surface defects of the porous second precursor and the pores in the material to chemically cross-link with the oxygen-containing functional groups, thereby stably and accurately doping nitrogen atoms in the internal structure of the material, which can be active ions (such as Na + or Li +) provides a large number of adsorption active sites, expands the graphite layer spacing, and thus effectively improves the adsorption efficiency and transmission efficiency of active ions. Then, the third precursor is subjected to carbon coating treatment, which can modify the surface defects of the third precursor, thereby effectively improving the capacity performance and the first coulomb efficiency of the negative electrode material. It can be seen from the data in Table 1 that the first charge and discharge specific capacity and the first coulomb efficiency of the embodiment are better than those of the comparative example as a whole. The first charge specific capacity in this application can reach 350mAh·g -1 As mentioned above, while ensuring a high first charge and discharge specific capacity, the first coulombic efficiency can reach between 85% and 89%, and the first coulombic efficiency is also at a relatively high level.

[0181] Table 1

[0182]

[0183] It can be seen from the data in Table 1 that the median particle size Dv50 and specific surface area of ​​the negative electrode material in the embodiment are generally smaller than the median particle size Dv50 and specific surface area of ​​the negative electrode material in the comparative example. Figure 2 It can be seen from the pore size distribution diagram of the negative electrode material prepared in Example 1 that in the internal structure of the negative electrode material prepared in the present application, the pores are mainly composed of micropores less than 2nm, and the overall pore size distribution is uniform, which achieves better regulation of the internal structure of the negative electrode material, thereby making the performance of the negative electrode material better.

[0184] Since the negative electrode material in the present application has a suitable particle size and specific surface area, the first charge and discharge specific capacity and the first coulombic efficiency of the battery made using the negative electrode material are at a relatively high level.

[0185] It can be seen from the data in Table 1 that the interlayer spacing of the graphite carbon layers of the negative electrode materials in the embodiments is greater than the interlayer spacing of the graphite carbon layers of the negative electrode materials in the comparative examples. In the present application, since more oxygen-containing functional groups are added to the hard carbon precursor by acid solution treatment, and then a porous second precursor with suitable pores and large specific surface area is obtained by hydrothermal reaction, the oxygen-containing functional groups are fully exposed, providing sufficient space and conditions for the doping of nitrogen source compounds, so that nitrogen atoms are stably, accurately and fully doped in the internal structure of the material, effectively expanding the graphite interlayer spacing, and then the active ions (such as Na + or Li + ) provide a large number of adsorption active sites. Therefore, the first charge and discharge specific capacity and the first coulombic efficiency of the battery are at a relatively high level.

[0186] In Comparative Example 1, since the first precursor is not subjected to a hydrothermal reaction in an organic solvent solution, it is not possible to construct a porous material in the first precursor to obtain a porous material with a large specific surface area, so that the oxygen-containing functional groups in the first precursor cannot be well exposed, and the amino functional groups in the nitrogen source compound cannot undergo a good cross-linking reaction with the oxygen-containing functional groups, and the interlayer spacing d of the graphite carbon layer is 002 It is difficult to expand effectively, resulting in low sodium ion adsorption efficiency and transmission efficiency, relatively poor performance of the negative electrode material, and low first charge and discharge specific capacity and first coulomb efficiency.

[0187] In Comparative Example 2, since the porous second precursor is not subjected to a crosslinking polymerization reaction with the nitrogen source compound, that is, the porous second precursor is not doped with nitrogen atoms, the interlayer spacing of the graphite carbon layer is d 002 It is too small to store sodium ions in the micropores inside the material from the intercalation layer. At the same time, the lack of cross-linking between nitrogen atoms and oxygen-containing functional groups in the carbon layer makes it impossible to effectively absorb and store sodium ions. Therefore, the initial charge-discharge capacity and initial coulombic efficiency are low. It can be seen that in the preparation of the negative electrode material of the present application, the hard carbon precursor is subjected to a first heat treatment, the first precursor, the nitrogen source compound, the cross-linking agent and the initiator are added to the solvent for a cross-linking polymerization reaction, and the second precursor is subjected to a carbon coating treatment. The lack of any step cannot maintain a high initial charge-discharge capacity and effectively improve the initial coulombic efficiency.

[0188] In Comparative Example 3, the step of preparing the negative electrode material includes constructing a porous structure through a hydrothermal reaction to increase the specific surface area of ​​the porous second precursor, so that the nitrogen source compound can fully enter the pores for chemical cross-linking reaction. Since the third precursor obtained after the cross-linking reaction is not carbon-coated in Comparative Example 3, the surface defects of the material cannot be effectively modified to reduce the specific surface area of ​​the material, resulting in significantly lower first charge specific capacity and first coulombic efficiency.

[0189] From the above, it can be seen that in the preparation of the negative electrode material of the present application, the first precursor is subjected to a hydrothermal reaction in an organic solvent solution, the porous second precursor is subjected to a cross-linking polymerization reaction with a nitrogen source compound, and the third precursor is subjected to a carbon coating treatment. If any of the steps is missing, a high first charge and discharge specific capacity and first coulombic efficiency cannot be maintained.

[0190] The microscopic morphology of the negative electrode material prepared in Example 1 is as follows: Figure 3 shown. Figure 4 TEM image of the negative electrode material prepared in Example 1. Figure 4It can be seen that the graphite interlayer spacing in the negative electrode material is above 3.95Å, and the average graphite interlayer spacing of the negative electrode material prepared in Example 1 is 0.399nm, i.e. 3.99Å. The graphite interlayer spacing of conventional hard carbon materials is about 3.7Å. In the negative electrode material prepared in this application, the graphite interlayer spacing is significantly increased, which can effectively improve the active ion diffusion rate and the ability to embed active ions in the intercalation layer, thereby improving the capacity of the negative electrode material. In addition, by Figure 4 It can be seen that the negative electrode material contains a large number of short-range ordered graphite-like microcrystals entangled and stacked microporous structures. This structure can provide a large amount of storage space for sodium ions, thereby increasing the capacity of the battery, which is consistent with the above-mentioned electrochemical performance test results.

[0191] Figure 5 The charge and discharge curve of the battery made of the negative electrode material obtained in Example 1, Figures 6 to 8 The charge and discharge curves of the batteries made of the negative electrode materials obtained in Comparative Examples 1 to 3 are shown respectively.

[0192] In the charge-discharge curve, the gram capacity in the slope area (>0.1V) of the charge curve is mainly related to the adsorption of active ions on the surface of the negative electrode material, and the gram capacity in the platform area (0.1V-0V) of the charge curve is mainly related to the filling of active ions in the micropores inside the negative electrode material and the embedding between carbon layers. Therefore, the gram capacity ratio in the platform area of ​​the charge curve can reflect the ratio of micropore volume in the negative electrode material, that is, the size of the storage space that can be provided for active ions in the negative electrode material. Figures 5 to 8 The test charge and discharge curves show that the platform area gram capacity of the negative electrode material charging curve prepared in Example 1 accounts for more than 78%, and the platform area gram capacity of the negative electrode material charging curve prepared in Comparative Examples 1 to 3 accounts for 42%, 36%, and 47%, respectively, which are significantly lower than that in Example 1. This shows that the present application first constructs a better porous structure in the hard carbon material through hydrothermal reaction, and secondly effectively increases the graphite layer spacing through sufficient doping of nitrogen source compounds, and further better modifies the surface defects of the material through gas phase coating, so that the prepared negative electrode material can provide a larger storage space for active ions, which is convenient for the embedding and transmission of active ions, thereby effectively improving the capacity performance of the negative electrode material.

[0193] It should be noted that the negative electrode material embodiments, negative electrode material preparation method embodiments, negative electrode plate embodiments and battery embodiments provided in the present application belong to the same concept; the technical features in the technical solutions recorded in each embodiment can be arbitrarily combined without conflict.

[0194] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.

Claims

1. A method for preparing a negative electrode material, It is characterized in that The method comprises the following steps: S1: Purifying a hard carbon precursor with an acid solution, washing, filtering and drying to obtain a first precursor; the hard carbon precursor includes a biomass-based hard carbon material, and the first precursor includes an oxygen-containing functional group; S2: adding the first precursor to a mixed solution of an organic solvent and water for hydrothermal reaction, and obtaining a porous second precursor through washing, suction filtration and drying; S3: adding the porous second precursor into a solvent, then adding a nitrogen source compound solution and an initiator solution, performing a cross-linking reaction, washing, filtering and drying to obtain a third precursor, wherein the reaction temperature of the cross-linking reaction is 40° C. to 250° C.; S4: performing carbon coating treatment on the third precursor to obtain a negative electrode material having a coating layer.

2. The method for preparing the negative electrode material according to claim 1, It is characterized in that Step S1 satisfies at least one of the following characteristics (1) and (2): (1) The acid solution includes at least one of sulfuric acid, nitric acid, hydrofluoric acid, and hydrochloric acid; (2) The oxygen-containing functional group includes a carboxyl group and / or a hydroxyl group.

3. The method for preparing the negative electrode material according to claim 1, It is characterized in that Step S2 satisfies at least one of the following characteristics (1) to (6): (1) The mass ratio of the first precursor, the organic solvent and the water is (10-100): (10-50): (30-100); (2) The organic solvent includes at least one of ethanol, propanol, butanol, ethyl ether, butyl ether, formic acid, and acetic acid; (3) The reaction temperature of the hydrothermal reaction is 80°C to 200°C, the heating rate is 0.1°C / min to 5°C / min, and the reaction time is 0.5h to 5h; (4) The specific surface area of ​​the porous second precursor is 100 m 2 / g~500m 2 / g; (5) The pore size of the porous second precursor is 0.2 nm to 150 nm, wherein the volume of macropores accounts for 60% to 90%, the volume of mesopores accounts for 10% to 30%, and the volume of micropores accounts for 1% to 5%; (6) The true density of the porous second precursor is 1.8 g / cm 3 ~2.2g / cm 3 .

4. The method for preparing the negative electrode material according to claim 1, It is characterized in that Step S3 satisfies at least one of the following characteristics (1) to (6): (1) The nitrogen source compound includes at least one of acrylamide, phenylalanine, glutamic acid, acrylonitrile and β-nitrostyrene; (2) The initiator includes at least one of azobisisobutyronitrile, ammonium persulfate-sodium bisulfite, azobisisoheptylnitrile, and hydrogen peroxide; (3) The mass fraction of the nitrogen source compound solution is 0.1%~10%; (4) The mass fraction of the initiator solution is 0.01%~10%; (5) The solvent includes at least one of water, ethanol, acetone, toluene, ether, N,N'-dimethylformamide, and ethylene glycol monomethyl ether; (6) The reaction time of the cross-linking reaction is 1h~10h.

5. The method for preparing the negative electrode material according to claim 1, It is characterized in that The carbon coating process in step S4 includes: A carbon source gas and a first inert gas are introduced to perform gas phase coating on the third precursor; the gas phase coating has at least one of the following characteristics: a) the gas phase deposition temperature is 600°C~1000°C; b) the heating rate is 1°C / min~5°C / min; c) the deposition time is 1h~10h; d) the flow rate of the carbon source gas is 0.1L / min~10L / min; e) the flow rate of the first inert gas is 0.1L / min~10L / min; f) the carbon source gas includes alkane and / or olefin compounds; g) the first inert gas includes at least one of argon, nitrogen, and helium.

6. The method for preparing the negative electrode material according to claim 1, It is characterized in that Step S4 satisfies at least one of the following characteristics (1) to (5): (1) The thickness of the coating layer of the negative electrode material is 0.001 μm to 0.01 μm; (2) The median particle size Dv50 of the negative electrode material is 4 μm to 10 μm; (3) The specific surface area of ​​the negative electrode material is 10m 2 / g~20m 2 / g; (4) The pore size of the negative electrode material is 0.25 nm to 75 nm, of which the volume of macropores accounts for 15% to 30%, the volume of mesopores accounts for 25% to 50%, and the volume of micropores accounts for 10% to 20%; (5) The true density of the negative electrode material is 1.7 g / cm 3 ~2.0g / cm 3 .

7. The method for preparing the negative electrode material according to any one of claims 1 to 6, It is characterized in that The method further comprises: The negative electrode material is heat-treated under a second inert gas atmosphere; the heat treatment has at least one of the following characteristics: a) the heat treatment temperature is 1000°C~1600°C; b) the insulation time is 1h~10h; c) the heating rate is 0.1°C / min~10°C / min; d) the second inert gas includes at least one of argon, nitrogen, and helium.

8. The method for preparing the negative electrode material according to claim 7, It is characterized in that The method further comprises: After the heat treatment, cooling and sieving are performed; wherein the negative electrode material after sieving has at least one of the following characteristics: a) the median particle size is 5 μm to 15 μm; b) the specific surface area is 2 m 2 / g~10m 2 / g; c) pore size is 0.35nm~55nm, of which the volume of macropores accounts for 1%~10%, the volume of mesopores accounts for 15%~20%, and the volume of micropores accounts for 40%~60%; d) true density is 1.4g / cm 3 ~1.6g / cm 3 ; e) The interlayer spacing of the carbon layers is 0.380nm~0.405nm.

9. A negative electrode material, It is characterized in that The negative electrode material is prepared by the method for preparing the negative electrode material according to any one of claims 1 to 8.

10. A battery comprising a negative electrode plate, It is characterized in that The negative electrode plate includes the negative electrode material prepared by the preparation method according to any one of claims 1 to 8 or includes the negative electrode material according to claim 9.

Citation Information

Patent Citations

  • Hard carbon-nitrogen phosphorus double-doped nanocarbon composite carbon material and preparation method thereof

    CN115663152A

  • Nitrogen-doped multi-carbon coated graphite composite material, composite material and secondary battery

    CN115744895A

  • Hard carbon material and preparation method and application thereof

    CN118016847A