Preparation method and use of a slow-release carbon source
By using c-di-GMP inhibitor and manganese ion crosslinked composite porous microspheres in the caprolactone device, the problem of expansion sludge loss in the anaerobic tower is solved, and the inhibition of sludge expansion and anaerobic bacteria are achieved. The stability of the growth environment improves the operating efficiency of the device.
Patent Information
- Application Number
- CN202410765018.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The expansion sludge phenomenon of the anaerobic tower in the caprolactone device leads to sludge loss, affecting the pelletization of anaerobic bacteria and the operation efficiency of the device.
Using sustained-release polycaprolactone-polylactic acid/sodium alginate composite porous microspheres that wrap c-di-GMP inhibitors and manganese ions to reduce bacterial extracellular polysaccharide secretion by local release of inhibitors and manganese ions, controlling Sludge swells and drains.
It effectively inhibits sludge expansion, slows down sludge loss, provides a stable anaerobic bacteria growth environment, and reduces device operation losses.
Smart Images

Figure FDA0005118010750000021 
Figure GDA0005118010760000031 
Figure HDA0005000706400000011
Abstract
Description
Technical Field
[0001] The invention belongs to the material preparation technology in the field of chemical industry, and specifically relates to a preparation method of a slow-release carbon source and application thereof. Background Art
[0002] Due to the large-scale production of caprolactone monomer, the water volume per unit time is high and the waste liquid load (COD) is large. The caprolactone device is also prone to fluctuations in the sewage load during the adjustment period. This difficult anaerobic growth environment will promote the occurrence of swelling and sludge in the anaerobic reactor. The swelling sludge floats, is easy to lose, and is difficult to recover. The loss of a certain amount of swelling sludge may make it more difficult to granulate anaerobic bacteria. However, the properties of the microorganisms in the swelling sludge are basically the same as those in the anaerobic reactor. It is obviously a pity to abandon these sludges. When the wastewater temperature is low or the sludge load is too high, the bacteria do not have time to convert organic matter into simple molecules, but accumulate a large amount of highly viscous polysaccharides and volatile acids in the extracellular metabolism, which will cause a large increase in surface attachments. The attachments are easy to form bound water and are difficult to precipitate and compress. Eventually, swelling sludge will appear, leading to sludge loss.
[0003] The composite porous microspheres of slow-release polycaprolactone-polylactic acid / sodium alginate wrapped with specific c-di-GMP inhibitors and cross-linked with manganese ions can stimulate the destruction of the polycaprolactone structure of the outer layer of the microspheres due to the load fluctuations when the acid-producing bacteria decompose organic matter and locally produce a large amount of volatile acid, thereby releasing the inhibitor and manganese ions, wherein the inhibitor can reduce the conduction of c-di-GMP signals, thereby reducing the secretion of bacterial extracellular polysaccharides, and the slow-released manganese ions can also inhibit the secretion of extracellular polysaccharides, thereby inhibiting sludge swelling. The composite porous microspheres in the present invention have the ability to control the sludge swelling phenomenon, release the c-di-GMP inhibitor under the condition of local production of volatile acids to reduce bacterial polysaccharide secretion, and the porous microspheres can also provide space for the growth of bacteria. When swelling sludge occurs, the composite porous carbon source can be added to reduce the loss of sludge to avoid causing greater losses to the operation of the device. Summary of the invention
[0004] The purpose of the present invention is to solve the swelling and sludge running phenomenon in the anaerobic tower of the caprolactone stripping tower high COD sewage treatment device, inhibit the production of extracellular polysaccharides, slow down the loss caused by sludge swelling, and propose a preparation method of a slow-release carbon source.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a slow-release carbon source comprises the following steps:
[0007] S1: dissolving a manganese salt to prepare a manganese ion solution;
[0008] S2: dissolving sodium alginate to prepare a sodium alginate solution, mixing the manganese ion solution with the sodium alginate solution, adding a c-di-GMP synthetase inhibitor, stirring at room temperature for 6h-8h for cross-linking, filtering to obtain a precipitate, crushing the precipitate into 300-500 meshes using a crusher, and drying; and then dispersing in a 5wt% sodium bicarbonate solution to obtain a dispersion;
[0009] S3: preparing polymer / ethyl acetate-dichloromethane solution: mixing ethyl acetate and dichloromethane, and then adding polycaprolactone, polylactic acid, a porogen and an emulsifier to obtain a polymer / ethyl acetate-dichloromethane solution; S4: adding the dispersion dropwise to the polymer / ethyl acetate-dichloromethane solution, stirring rapidly to form emulsion droplets at the bottom and a supernatant at the top; after removing the supernatant, pouring into n-pentane at -30°C, continuing stirring for 6-10 minutes, then pouring out the flowable liquid for recovery, freezing the ice crystal particles for 12 hours, and freeze-drying them at -30°C for 24 hours to obtain the slow-release carbon source.
[0010] In a further improvement, the manganese salt is MnCl 2 or MnSO 4 The mass volume ratio of manganese salt to deionized water in the manganese ion solution is 1-5:200g / ml.
[0011] As a further improvement, the mass volume ratio of sodium alginate to deionized water in the sodium alginate solution is 3-5:150 g / ml; and the volume ratio of the manganese ion solution to the sodium alginate solution is 200:150.
[0012] As a further improvement, in step S3, ethyl acetate and dichloromethane are mixed in a volume ratio of 5:1; in the polymer / ethyl acetate-dichloromethane solution, the final concentration of polycaprolactone is 3wt%-5wt%, the final concentration of polylactic acid is 5wt%-8wt%, the final concentration of the porogen is 1g / L, and the final concentration of the emulsifier is 2.5g / L.
[0013] As a further improvement, in step S4, the volume ratio of the dispersion to the polymer / ethyl acetate-dichloromethane solution is 50:200.
[0014] In a further improvement, the c-di-GMP synthetase inhibitor is at least one of DI-3, DI-10, Eb, and EbO.
[0015] As a further improvement, the structural formulas of DI-3, DI-10, Eb, and EbO are respectively:
[0016]
[0017] In a further improvement, the porogen is one of hexadecyltrimethylammonium bromide, hexadecyltrimethylsodium bromide, hexadecyldimethylbenzylammonium chloride and hexadecyltrimethylammonium chloride; and the emulsifier is one of Tween 20, Tween 40, Tween 60 and Tween 80.
[0018] As a further improvement, the mass volume ratio of the crushed material to the 5wt% sodium bicarbonate solution is 4-10:500g / ml.
[0019] A use of a slow-release carbon source. The preparation method of the slow-release carbon source is as described above. The slow-release carbon source is used as an agent for slowing down sludge loss in an anaerobic reactor.
[0020] The present invention has the following beneficial effects:
[0021] 1. The slow-release carbon source of the present invention, the raw materials polycaprolactone, polylactic acid, and sodium alginate can be synthesized through non-petrochemical routes, and are all completely biodegradable materials, meeting the requirements of sustainable development.
[0022] 2. The slow-release carbon source of the present invention, under the action of anaerobic bacteria, will promote the decomposition of the carbon source shell, release the c-di-GMP inhibitor in the carbon source, and can play a role in reducing sludge swelling.
[0023] 3. The slow-release carbon source of the present invention can promote the decomposition of the carbon source shell and core under the action of anaerobic bacteria, slowly release manganese ions, and reduce sludge swelling.
[0024] The present invention uses sodium alginate to be cross-linked with manganese ions, and then a c-di-GMP inhibitor is added. After crushing, an emulsion method is used in combination with freeze drying technology to prepare a composite slow-release carbon source with an outer layer of polycaprolactone-polylactic acid and an inner layer of sodium alginate. The carbon source can release the inhibitor and manganese ions in an anaerobic reactor, and has the effect of reducing sludge swelling. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a measurement diagram of extracellular polymers of Examples and Comparative Examples;
[0026] Figure 2 It is a graph showing the strength of anaerobic sludge particles in the examples and comparative examples;
[0027] Figure 3 It is the measurement diagram of c-di-GMP of the embodiment and the comparative example;
[0028] Figure 4 SV30 and SVI measurement diagrams of Examples and Comparative Examples. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0030] Example 1
[0031] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0032] S1: 5g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0033] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.03g of DI-3 was added. After stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 500 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0034] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 5 wt% polycaprolactone and 5 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium bromide and 0.5 g Tween 80.
[0035] S4: Take 50ml of the final solution of S2 and add it dropwise to 200ml of the solution of S3. Stir quickly and evenly to form emulsion droplets. After removing most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify. Continue stirring at low temperature for 10 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0036] Example 2
[0037] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0038] S1: 1g MnSO 4 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0039] S2: 5g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.03g of DI-10 was added. After stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 300 mesh using a crusher, and stored in a dry and sealed place. When used, 6g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0040] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethyl sodium bromide and 0.5 g Tween 60.
[0041] S4: Take 50ml of the final solution of S2 and add it dropwise to 200ml of the solution of S3. Stir quickly and evenly to form emulsion droplets. After removing most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify. Continue stirring at low temperature for 10 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0042] Example 3
[0043] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0044] S1: 5g MnSO 4 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0045] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.01g of EbO was added. After stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 400 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0046] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 80.
[0047] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0048] Example 4
[0049] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0050] S1: 5g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0051] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.02g of Eb was added. After stirring at room temperature for 6h, the mixture was filtered, washed with deionized water several times, and then crushed to 300 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0052] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0053] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0054] Example 5
[0055] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0056] S1: 1g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0057] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.02g of Eb was added. After stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 500 mesh using a crusher, and stored in a dry and sealed container. When used, 4g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0058] S3: Prepare 200 g of a polymer / ethyl acetate-dichloromethane solution containing 5 wt % polycaprolactone and 8 wt % polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0059] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0060] Example 6
[0061] This embodiment provides a slow-release carbon source suitable for slowing down sludge loss, and the preparation method comprises the following steps:
[0062] S1: 1g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0063] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, 0.02g of Eb and 0.01g of DI-3 were added, and after stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 500 mesh using a pulverizer, and stored in a dry and sealed container. When used, 4g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0064] S3: Prepare 200 g of a polymer / ethyl acetate-dichloromethane solution containing 5 wt % polycaprolactone and 8 wt % polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0065] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0066] Comparative Example 1
[0067] Compared with Example 4, no solute polycaprolactone and polylactic acid were added in the carbon source preparation process S3.
[0068] The details are as follows:
[0069] S1: 5g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0070] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.02g of Eb was added. After stirring at room temperature for 6h, the mixture was filtered, washed with deionized water several times, and then crushed to 300 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0071] S3: Prepare 200 ml of ethyl acetate-dichloromethane solution, a composite solvent, with a volume ratio of ethyl acetate to dichloromethane of 5:1, add 0.2 g of hexadecyltrimethylammonium chloride and 0.1 g of Tween 40.
[0072] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0073] Comparative Example 2
[0074] Compared with Example 3, no solute polycaprolactone and polylactic acid were added in the carbon source preparation process S3.
[0075] The details are as follows:
[0076] S1: 5g MnSO 4 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0077] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.01g of EbO was added. After stirring at room temperature for 8h, the mixture was filtered, washed with deionized water several times, and then crushed to 400 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0078] S3: Prepare 200 ml of ethyl acetate-dichloromethane solution, where the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g of hexadecyltrimethylammonium chloride and 0.1 g of Tween 80.
[0079] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0080] Comparative Example 3
[0081] Compared with Example 4, the carbon source preparation process does not contain step S1, no c-di-GMP inhibitor is added in S2, and no solute polycaprolactone and polylactic acid are added in S3.
[0082] The details are as follows:
[0083] S2: Dissolve 3 g of sodium alginate completely in 150 ml of deionized water at 60° C. After cooling to room temperature, add 25 g of sodium bicarbonate and 350 ml of deionized water to prepare a solution.
[0084] S3: Prepare 200 ml of ethyl acetate-dichloromethane solution, where the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g of hexadecyltrimethylammonium chloride and 0.1 g of Tween 40.
[0085] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0086] Comparative Example 4
[0087] Compared with Example 4, step S1 is not included and no c-di-GMP inhibitor is added in S3.
[0088] S2: 3 g of sodium alginate was completely dissolved in 150 ml of deionized water at 60°C. After cooling to room temperature, 25 g of sodium bicarbonate and 350 ml of deionized water were added to prepare a solution.
[0089] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0090] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0091] Comparative Example 5
[0092] Compared with Example 4, the step of manganese ion cross-linking is not performed in S2, and the c-di-GMP inhibitor is not added in S3.
[0093] The details are as follows:
[0094] S1: 5g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0095] S2: Dissolve 3g of sodium alginate completely in 150ml of deionized water at 60°C. After cooling to room temperature, add 25g of sodium bicarbonate. Then add 200ml of S1 solution and 150g of deionized water to the 150ml sodium alginate solution to prepare a 500ml mixed solution.
[0096] S3: Prepare 200 ml of ethyl acetate-dichloromethane solution, where the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g of hexadecyltrimethylammonium chloride and 0.1 g of Tween 40.
[0097] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0098] Comparative Example 6
[0099] Compared with Example 4, no c-di-GMP inhibitor was added in step S3.
[0100] The details are as follows:
[0101] S1: 5g MnCl 2 Dissolve in 200 ml of deionized water and stir vigorously at room temperature for 30 min to obtain a manganese ion solution.
[0102] S2: 3g sodium alginate was completely dissolved in 150ml deionized water at 60°C. Then 150ml of sodium alginate solution was added to 200ml of S1 solution, and 0.02g of Eb was added. After stirring at room temperature for 6h, the mixture was filtered, washed with deionized water several times, and then crushed to 300 mesh using a crusher, and stored in a dry and sealed container. When used, 8g of the prepared crushed material was dispersed in 500ml of 5wt% sodium bicarbonate solution.
[0103] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0104] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0105] Comparative Example 7
[0106] Compared with Example 4, step S1 is not included and a c-di-GMP inhibitor is added.
[0107] The details are as follows:
[0108] S2: 3 g of sodium alginate was completely dissolved in 150 ml of deionized water at 60°C. After cooling to room temperature, 25 g of sodium bicarbonate, 0.02 g of Eb and 350 ml of deionized water were added to prepare a solution.
[0109] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 40.
[0110] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0111] Comparative Example 8
[0112] Compared with Example 3, step S1 is not included and no c-di-GMP inhibitor is added in S2.
[0113] S2: 3 g of sodium alginate was completely dissolved in 150 ml of deionized water at 60°C. After cooling to room temperature, 25 g of sodium bicarbonate and 350 ml of deionized water were added to prepare a solution.
[0114] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 80.
[0115] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0116] Comparative Example 9
[0117] Compared with Example 3, steps S1 and S2 are not included, and a c-di-GMP inhibitor is added.
[0118] The details are as follows:
[0119] S2: 3 g of sodium alginate was completely dissolved in 150 ml of deionized water at 60°C. After cooling to room temperature, 25 g of sodium bicarbonate, 0.01 g of EbO and 350 ml of deionized water were added to prepare a solution.
[0120] S3: Prepare 200 ml of a polymer / ethyl acetate-dichloromethane solution containing 3 wt% polycaprolactone and 8 wt% polylactic acid, wherein the volume ratio of the composite solvent ethyl acetate to dichloromethane is 5:1, and add 0.2 g hexadecyltrimethylammonium chloride and 0.1 g Tween 80.
[0121] S4: Take 50ml of S2 solution and add it dropwise to 200ml of S3 solution, stir quickly to form emulsion droplets, remove most of the supernatant, pour it into n-pentane that has been stirred and pre-cooled in a -30℃ reactor to solidify, continue stirring at low temperature for 6 minutes, pour out the remaining flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and freeze-dry them at -30℃ for 24 hours to obtain a composite carbon source.
[0122] Pre-test work: anaerobic sludge acclimatization
[0123] Anaerobic bacteria were cultured in a 20cm×40cm round tower UASB reactor with a working volume of 10L. At the beginning of each cycle, diluted caprolactone device wastewater (about 8000mg / L COD) was intermittently introduced, and the configured wastewater pH was 6.8-7.2. Domestication was carried out in stages, with the first stage configuring the influent to be about 2000mg / L COD, the second stage configuring the influent to be about 4500mg / L COD, and the third stage configuring the influent to be about 7000mg / L COD. When domestication is stable, wastewater of about 9500mg / L COD was added, and the high-load environment was simulated for operation for 3 days. 20g of carbon source was added to the device for co-cultivation test, and the influent of about 7000mg / L COD was restored during the test. The test method is shown in Test Example 1 and Test Example 2, and three parallel samples are set for the index test.
[0124] Test Example 1 Determination of Extracellular Polymers
[0125] Add 20g of carbon source to the device with the same basic conditions after acclimation. The carbon source used is prepared according to Examples 1-6 and Comparative Examples 1-9 of the present invention. Take the bottom layer sample on the 6th day of co-cultivation. The MLSS concentration of the sample is determined according to CJ / T221-2005. The formaldehyde-sodium hydroxide method is used to extract the extracellular polymers (EPs) of anaerobic sludge. The extracted protein and polysaccharide are quantified using the Folin phenol method and the phenol-sulfuric acid method, respectively. Record the protein content and polysaccharide content per gram of MLSS in the sample on the sixth day. The test results are as follows: Figure 1In the figure, the embodiment is represented by E (such as embodiment 1 is represented by E1), and the comparative example is represented by C (such as comparative example 1 is represented by C1).
[0126] Test Example 2. Determination of the strength of anaerobic sludge particles
[0127] Add 20g of carbon source to the device with the same basic conditions after acclimation. The carbon source used is prepared according to Examples 1-6 and Comparative Examples 1-9 of the present invention. Take samples on the 6th day after the co-cultivation test, wash the anaerobic sludge with clean water 3-5 times after filtration, and freeze-dry at -50°C. Evaluate the strength of anaerobic granules by ultrasound. Put 3g of anaerobic granules into a 25ml conical flask containing 15ml deionized water, and then place it in an ultrasonic bath of 20-25kHz.65W. Collect the treated sample solution every 2min, and measure the absorbance by spectrophotometry at 600nm.
[0128] Test results such as Figure 2 In the figure, the embodiment is represented by E (such as embodiment 1 is represented by E1), and the comparative example is represented by C (such as comparative example 1 is represented by C1).
[0129] Test Example 3 Determination of c-di-GMP
[0130] Add 20g of carbon source to the device with the same basic conditions after acclimation, and the carbon source used is prepared according to Examples 1-6 and Comparative Examples 1-9 of the present invention. Take UASB reaction bottom samples on the 0th, 2nd, 4th and 6th days of co-cultivation. After sampling, first freeze-dry the anaerobic sludge at -50°C. Take 0.2g of sludge and 15ml of deionized water and put them into a 50ml tube. Add lysozyme (containing buffer) with a concentration of 1mg / ml, stir for 15min, bath in 37°C water for 1h, and centrifuge at 9000rpm for 15min at 4°C. Transfer the supernatant to a new 50ml tube, add ethanol at a ratio of 2:1 of ethanol:supernatant, and stir rapidly for 10s. Incubate at 4°C for about 1h, shake once every 5-10min, and centrifuge at 9000rpm for 15min. Store the precipitate at 37°C for 3h, add 3ml of deionized water, and stir rapidly for 10s. Transfer the mixture to a 5ml tube and centrifuge at 12,000rpm for 10 minutes. Finally, 1 ml of the supernatant was placed in a chromatography vial for high performance liquid chromatography (HPLC) analysis to measure the concentration of c-di-GMP.
[0131] HPLC used a C18 chromatographic column, the detection temperature was 40°C, the eluent used contained 95% of 0.9% NaCl solvent and 5% acetonitrile, and the flow rate was 1 ml / min.
[0132] Test results such as Figure 3In the figure, the embodiment is represented by E (such as embodiment 1 is represented by E1), and the comparative example is represented by C (such as comparative example 1 is represented by C1).
[0133] Test Example 4. Determination of manganese ion release coefficient K
[0134] The carbon source used in this test example is prepared according to Examples 1-6, Comparative Examples 1-2 and Comparative Examples 5-6 of the present invention. 1g of carbon source is added to 1L of ultrapure water, and samples are taken at 0.5, 1, 2, 4, 6, 8, 10, 12, 24, 48, 72, 96, 120, 144, 168, and 192 hours to determine the trend of manganese ion concentration using ICP. The final manganese ion release coefficient K is calculated based on the data. The calculation formula is as follows:
[0135] K=c Mn / t 1 / 2
[0136] Among them, K is the manganese ion release coefficient. The lower its value, the slower the manganese ion sustained release rate of the carbon source and the better the sustained release effect. Mn is the saturated manganese ion concentration released by unit carbon source in solution, mg / L,t 1 / 2 It is the time taken for the concentration of manganese ions released by a unit carbon source in the solution to reach half of the saturation concentration, h.
[0137] The results are shown in Table 1.
[0138] Table 1
[0139] Group Manganese ion sustained release coefficient K Example 1 0.42 Example 2 0.56 Example 3 0.53 Example 4 0.58 Example 5 0.49 Example 6 0.46 Comparative Example 1 2.45 Comparative Example 2 2.39 Comparative Example 5 1.58 Comparative Example 6 0.59
[0140] Test Example 5 Determination of SV30 and SVI
[0141] Add 20g of carbon source to the device with the same basic conditions after acclimation. The carbon source used is prepared according to Examples 1-6 and Comparative Examples 1-9 of the present invention. Take the water sample from the water outlet on the 6th day of co-cultivation of carbon source and anaerobic bacteria. Pour the stirred mixed solution into the measuring cylinder quickly to the full scale, let it stand and settle for 30 minutes, and the volume ratio of the precipitated sludge to the mixed solution is the sludge settling ratio. SVI can be calculated according to the corresponding MLSS and SV30. Data as shown in Figure 4 shown.
[0142] Comparative Example 1-2 Compared with Examples 4-5, no solute polycaprolactone and polylactic acid were added in the carbon source preparation process S3. Figure 1 It can be seen that the polysaccharide and protein contents in Comparative Examples 1-2 are lower than those in Examples 4-5. Figure 2The size of OD600 indicates the turbidity of the mixed solution. It can be seen that although the turbidity changes of Example 1-2 and Comparative Example 1-2 increase with the ultrasonic time, the turbidity change trend of Comparative Example 1-2 in the early stage is faster than that of Example 4-5, which also shows that the anaerobic granular sludge co-cultured with Comparative Example 1-2 has low strength and its structure is easily destroyed under the action of ultrasound. Figure 3 In Table 1, the c-di-GMP content of Comparative Example 1-2 changes faster with the sampling time, while the c-di-GMP content of the embodiment changes more uniformly. In Table 1, the manganese ion sustained release coefficient of Comparative Example 1-2 is the largest. Figure 4 The SVI of Comparative Example 1-2 is normal, but the SV30 in the effluent is 5%, which indicates that the sludge has a certain loss rate. The data of Comparative Examples 1-2 and Examples 4-5 show that when polycaprolactone and polylactic acid solutes are not used as carbon source shells, the manganese ion release rate is faster, which will quickly inhibit the c-di-GMP value, thereby rapidly reducing its polysaccharide and protein content. Although it has a strong ability to reduce EPs (extracellular polymers), it will reduce the strength of anaerobic granular sludge, ultimately leading to a higher sludge loss rate.
[0143] Compared with Example 4, Comparative Example 4 does not contain step S1 (manganese ion solution) and no c-di-GMP inhibitor is added in S3. Compared with Example 4, Comparative Example 5 does not perform the manganese ion cross-linking step in S2 and no c-di-GMP inhibitor is added in S3. Compared with Example 4, Comparative Example 6 does not add c-di-GMP inhibitor in step S3. Figure 1 It can be seen that the polysaccharide and protein contents of Comparative Examples 4-6 are higher than those of Example 4, among which the EPs in Comparative Example 4 is the highest, followed by Comparative Example 6, and then Comparative Example 5, which indicates that when manganese ions are not cross-linked, the degree of reduction of EPs is the largest, while after manganese ion cross-linking, the degree of reduction of EPs is slightly smaller. Figure 2 It can be seen that the speed of change over time of Comparative Examples 4-6 is from fast to slow, respectively, Comparative Example 5, Comparative Example 4, and Comparative Example 6. This indicates that the strength of the anaerobic granular sludge co-cultured with the carbon source after manganese ion cross-linking is the best, and the carbon source without cross-linking using manganese ion solution will reduce its strength. Figure 3 In the table 1, the manganese ion sustained release rate of comparative example 5 is faster, and the manganese ion sustained release rate of comparative example 6 is not much different from that of the embodiment. Figure 4Among them, the SVI of Comparative Example 4 is very high (greater than 120), and there is obviously a certain amount of sludge swelling; while the SVI of Comparative Example 5 is relatively high (less than 120 but greater than 100), and there is a tendency of sludge swelling; the SVI of Comparative Example 6 is normal, and all three have a certain amount of sludge loss, and the loss rate of Comparative Example 4 is relatively large. The data show that when manganese ions are not cross-linked, their release rate is relatively fast, which will inhibit the c-di-GMP value, thereby rapidly reducing the polysaccharide and protein content secreted by bacteria. Although it has a strong ability to reduce EPs, the rapid release rate of manganese ions will reduce the strength of anaerobic granular sludge, ultimately leading to sludge loss. After cross-linking with manganese ions, manganese ions play a role of slow release, reducing the adverse effects of reduced anaerobic granular sludge strength and insignificant loss rate reduction caused by the excessively fast release rate of carbon source manganese ions.
[0144] Compared with Example 4 and Example 3, Comparative Examples 4 and 8 do not contain step S1, and no c-di-GMP inhibitor is added to S2. Compared with Example 4 and Example 3, Comparative Examples 7 and 9 do not contain step S1, and c-di-GMP inhibitor is added to S2. Figure 1 It can be seen that the polysaccharide and protein contents in Comparative Examples 4 and Comparative Examples 7-9 are higher than those in Example 3 and Example 4, among which Comparative Examples 4 and 7 have the highest EPs. Figure 2 It can be seen that after adding the inhibitor, the strength of the co-cultured anaerobic granular sludge is enhanced to a certain extent. Figure 3 In the comparative examples 4 and 8, the c-di-GMP concentration change trend is relatively slow, but after adding the inhibitor, the concentration change trend increases significantly. Figure 4 Compared with Comparative Examples 4 and 7, the SVI values of Comparative Examples 7 and 9 in which inhibitors were added were reduced to a certain extent, and the sludge loss was also alleviated to a certain extent. The data show that when inhibitors are added, c-di-GMP can be reduced and its polysaccharide and protein content can be controlled.
[0145] The data show that when the carbon source prepared by the embodiment of the present invention is used, when the load fluctuation causes the acid-producing bacteria to decompose organic matter and locally produce volatile acids, the polycaprolactone structure of the outer layer of the microspheres can be stimulated to be destroyed, thereby releasing inhibitors and manganese ions. By synergistically releasing manganese ions and c-di-GMP inhibitors, the c-di-GMP signal transduction can be effectively reduced, and the extracellular polysaccharides and proteins of anaerobic bacteria can be inhibited to a good extent, thereby improving the swelling of anaerobic granular sludge, and enhancing the strength of anaerobic granular sludge to a certain extent, and ultimately achieving the effect of effectively reducing sludge loss. However, the inhibitory effect of using a single manganese ion slow release or c-di-GMP inhibitor on sludge loss is not obvious.
[0146] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific implementation methods described.
Claims
1. A method for preparing a slow-release carbon source, characterized in that: The steps include: S1: dissolving a manganese salt to prepare a manganese ion solution; S2: dissolving sodium alginate to prepare a sodium alginate solution, mixing the manganese ion solution with the sodium alginate solution, adding a c-di-GMP synthetase inhibitor, stirring at room temperature for 6h-8h for cross-linking, filtering to obtain a precipitate, crushing the precipitate into 300-500 meshes using a crusher, and drying to obtain a crushed material; then dispersing the crushed material in a 5wt% sodium bicarbonate solution to obtain a dispersion; the c-di-GMP synthetase inhibitor is at least one of DI-3, DI-10, Eb, and EbO; S3: preparing a polymer / ethyl acetate-dichloromethane solution: mixing ethyl acetate and dichloromethane, and then adding polycaprolactone, polylactic acid, a porogen and an emulsifier to prepare a polymer / ethyl acetate-dichloromethane solution; the porogen is one of hexadecyltrimethylammonium bromide, hexadecyltrimethylsodium bromide, hexadecyldimethylbenzylammonium chloride and hexadecyltrimethylammonium chloride; the emulsifier is one of Tween 20, Tween 40, Tween 60 and Tween 80; S4: Add the dispersion dropwise to the polymer / ethyl acetate-dichloromethane solution, and stir rapidly to form emulsion droplets at the bottom and a supernatant at the top; after removing the supernatant, pour into n-pentane at -30°C, continue stirring for 6-10 minutes, then pour out the flowable liquid for recovery, freeze the ice crystal particles for 12 hours, and then freeze-dry at -30°C for 24 hours to obtain the slow-release carbon source.
2. The method for preparing a slow-release carbon source according to claim 1, characterized in that: The manganese salt is MnCl2 or MnSO4, and the mass volume ratio of the manganese salt to deionized water in the manganese ion solution is 1-5:200g / ml.
3. The method for preparing a slow-release carbon source according to claim 1, characterized in that: The mass volume ratio of sodium alginate to deionized water in the sodium alginate solution is 3-5:150 g / ml; the volume ratio of manganese ion solution to sodium alginate solution is 200:
150.
4. The method for preparing a slow-release carbon source according to claim 1, characterized in that: In step S3, ethyl acetate and dichloromethane are mixed in a volume ratio of 5:1; in the polymer / ethyl acetate-dichloromethane solution, the final concentration of polycaprolactone is 3wt%-5wt%, the final concentration of polylactic acid is 5wt%-8wt%, the final concentration of the porogen is 1g / L, and the final concentration of the emulsifier is 0.5-2.5g / L.
5. The method for preparing a slow-release carbon source according to claim 1, characterized in that: In step S4, the volume ratio of the dispersion to the polymer / ethyl acetate-dichloromethane solution is 50:
200.
6. The method for preparing a slow-release carbon source according to claim 1, characterized in that: The structural formulas of DI-3, DI-10, Eb and EbO are:
7. The method for preparing a slow-release carbon source according to claim 1, characterized in that: The mass volume ratio of the crushed material to the 5wt% sodium bicarbonate solution is 4-10:500g / ml.
8. A use of a slow-release carbon source, characterized in that: The method for preparing the slow-release carbon source is as described in any one of claims 1 to 7, and the slow-release carbon source is used as an agent for slowing down the loss of sludge in an anaerobic reactor.