Preparation method of polyisoprene latex

By using a composite emulsifier system of long-chain alkyl quaternary ammonium salts and co-emulsifiers, combined with a multi-stage evaporation concentration process, the insufficient stability and poor biocompatibility of polyisoprene latex emulsions under high shear forces are solved. problem, achieving a more stable emulsion and better biocompatibility.

CN118667186BActive Publication Date: 2024-10-29LIAONING LUHUA HONGJIN NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411149769.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

In the existing polyisoprene latex preparation methods, the emulsion has insufficient stability under high shear force and poor biocompatibility, making it difficult to meet the needs of high-standard products in the fields of medical and food.

Method used

Long-chain alkyl quaternary ammonium salts are used as the main emulsifier, combined with nonylphenol polyoxyethylene ether and other co-emulsifiers, and through shear emulsification and multi-stage evaporation concentration processes, a stable oil-in-water emulsion is formed, avoiding chemical interactions. The use of linking agents forms a dynamic adsorption balance and a composite network structure, which improves the stability and dispersion of the emulsion.

Benefits of technology

It significantly improves the mechanical stability and biocompatibility of the emulsion, extends the shelf life of the product, reduces the phenomenon of emulsion droplet aggregation, and avoids the problems of uneven chemical cross-linking and cross-linking agent residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118667186B_ABST
    Figure CN118667186B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of latex preparation, and specifically relates to a method for preparing polyisoprene latex, comprising five steps: adding a primary emulsifier, an auxiliary emulsifier, and a lipophilic and hydrophilic regulator into water to obtain an emulsifier aqueous solution, wherein the primary emulsifier is a long-chain alkyl quaternary ammonium salt; adding polyisoprene rubber into a saturated alkane and heating it to obtain a polyisoprene rubber solution; then mixing the polyisoprene rubber solution with the emulsifier aqueous solution, shearing and emulsifying it to obtain an oil-in-water emulsion; sequentially passing the oil-in-water emulsion through a first flash evaporator and a second flash evaporator to remove the solvent; after the solvent is removed, sequentially passing through an MVR evaporator and a centrifuge to evaporate and concentrate and centrifuge to obtain polyisoprene latex. The invention solves the problems that the stability of the emulsion under high shear force in the existing preparation method is still insufficient, and the latex has poor biocompatibility by rationally selecting and compounding the emulsifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of latex preparation, and in particular relates to a method for preparing polyisoprene latex. Background Art

[0002] There are two main methods for preparing polyisoprene latex: emulsion polymerization and solution emulsification. The emulsion polymerization method has a high microgel content in the final product, unstable product quality, and is difficult to meet the production requirements of high-specification products; while the solution emulsification method is currently a common method for preparing polyisoprene latex because of its advantages of controllable molecular weight and structure, high purity, and no isoprene monomer residue.

[0003] The solution emulsification method uses polyisoprene rubber as raw material, and goes through the steps of dissolution, emulsification, solvent removal and concentration in sequence to finally obtain polyisoprene latex. When preparing the water-in-oil emulsion of polyisoprene during the emulsification process, the dispersibility and stability of the emulsion will directly affect the effect of subsequent solvent removal and concentration, and ultimately affect the quality of the polyisoprene latex; at the same time, polyisoprene latex is mostly used in the fields of medical care, food, etc., and has high requirements for biocompatibility and other aspects.

[0004] At present, due to the low film stacking density of a single emulsifier at the oil-water interface, the emulsion layer strength is insufficient, which easily leads to the aggregation and demulsification of emulsion droplets under the influence of high shear force or high temperature, thereby affecting the stability and dispersibility of the emulsion. Therefore, in view of the shortcomings of a single emulsifier, how to select a variety of suitable emulsifiers for compounding to maximize the synergistic effect between different emulsifiers is one of the main research topics of those skilled in the art.

[0005] Chinese patent application CN104292473A discloses a method for preparing polyisoprene latex, wherein the emulsifier system is anionic emulsifier and nonionic emulsifier, wherein the anionic emulsifier is one or two of sodium dodecylbenzene sulfonate and isomeric alcohol ether carboxylate, and the nonionic emulsifier is one or more of Tween80, Peregal O-20 and hexadecylphenol polyoxyethylene ether, and the total amount of emulsifier is 10-20% of the dry rubber mass, wherein the proportion of auxiliary emulsifier is less than 20%. The rubber is dissolved by saturated alkane to prepare the rubber solution, the rubber concentration in the rubber solution is 9.0-12.0%, and the oil-water ratio is 1.0-1.5.

[0006] This patent application aims to improve the mechanical stability of the emulsion by compounding anionic emulsifiers and nonionic emulsifiers in a certain ratio to address the shortcomings of a single emulsifier. However, the synergistic mechanism of anionic emulsifiers and nonionic emulsifiers is to use anionic emulsifiers to form a charge barrier to prevent oil droplets from aggregating with each other. At the same time, the high permeability of nonionic emulsifiers is used to disperse large oil droplets into smaller and more uniform oil droplets, further improving the mechanical stability of the emulsion. Therefore, compared with the direct cross-linking mechanism of emulsifiers, the stability and dispersibility of this emulsion are still insufficient when facing higher shear forces.

[0007] Chinese patent application CN112022729A discloses an O / W emulsion with remibond A as an emulsifier and a preparation method thereof, which specifically includes preparing remibond A using natural protein in hair as a raw material, using the prepared remibond A as an emulsifier to prepare the O / W emulsion, and then treating the emulsion with H2O2 to perform thiol cross-linking.

[0008] This patent application uses a chemical cross-linking mechanism to form a more stable interfacial film on the surface of the oil droplets, thereby improving the stability of the emulsion. However, this patent application uses H2O2 as a cross-linking agent. If the emulsifier obtained from this patent application is used in the preparation of isoprene latex, it will be difficult to completely remove H2O2 during the subsequent solvent removal, and the cross-linking agent residues are likely to cause allergic reactions in organisms, especially in scenarios that require high biocompatibility, such as medical implants. At the same time, according to the cross-linking mechanism of the cross-linking agent, the polymer chains are cross-linked to form a complex network structure, which will increase the diffusion resistance of the reaction system, affecting the reaction rate on the one hand, and causing problems such as uneven cross-linking reactions or the appearance of uncross-linked polymer segments on the other hand, affecting the stability and dispersibility of the emulsion. Summary of the invention

[0009] The object of the present invention is to provide a method for preparing polyisoprene latex, and to solve the problems of insufficient stability of the emulsion under high shear force and poor biocompatibility of the latex in the existing preparation method by reasonably selecting and compounding the emulsifier.

[0010] To achieve the above object, the technical solution adopted by the present invention is:

[0011] The preparation method of the polyisoprene latex comprises the following steps:

[0012] (1) adding a primary emulsifier, a secondary emulsifier, and a lipophilic and hydrophilic modifier into water to obtain an emulsifier aqueous solution, wherein the primary emulsifier is a long-chain alkyl quaternary ammonium salt;

[0013] (2) adding polyisoprene rubber to saturated alkane and heating to obtain a polyisoprene rubber solution;

[0014] (3) mixing the polyisoprene rubber solution with the emulsifier aqueous solution, and then shearing and emulsifying the mixture to obtain an oil-in-water emulsion;

[0015] (4) passing the oil-in-water emulsion through a first flash evaporator and a second flash evaporator in sequence to remove the solvent;

[0016] (5) After the solvent is removed, the product is evaporated and concentrated by centrifugation in an MVR evaporator and centrifuged to obtain polyisoprene latex.

[0017] in:

[0018] In the step (1), the main emulsifier is one or more of stearyl (dihydroxyethyl) methyl ammonium chloride, dodecyl bis(hydroxyethyl) methyl ammonium chloride or hexadecyl methyl dihydroxyethyl ammonium bromide; the auxiliary emulsifier is one or more of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether or dodecylphenol polyoxyethylene ether.

[0019] In the step (1), the lipophilic and hydrophilic modifier is prepared by mixing propylene glycol and ethyl sorbate in a mass ratio of (0.1-1):1.

[0020] In the step (1), a primary emulsifier, an auxiliary emulsifier, a lipophilic and hydrophilic regulator, a stabilizer and a thickener are added into water to obtain an emulsifier aqueous solution; the stabilizer is one or more of methyl cellulose, carboxymethyl cellulose or hydroxypropyl cellulose, and the thickener is one or more of gum arabic, sodium alginate or sodium tripolyphosphate.

[0021] The mass fraction of the main emulsifier in the emulsifier aqueous solution is 3-5%, the mass fraction of the auxiliary emulsifier is 0.35-1.5%, the mass fraction of the lipophilic and hydrophilic regulator is 1-2%, the mass fraction of the stabilizer is 0.05-0.1%, and the mass fraction of the thickener is 0.1-0.5%.

[0022] In the step (2), the heating temperature is 45-55° C., the heating time is 30-50 min, the mass fraction of polyisoprene rubber in the polyisoprene rubber solution is 8-15%, and the saturated alkane is n-hexane or cyclohexane.

[0023] The mass ratio of the main emulsifier to the polyisoprene rubber is 1:(6-12).

[0024] In the step (3), the mixing time is 15-45 min, the shear emulsification temperature is 40-65° C., the shear emulsification rate is 8-14 m / s, and the shear emulsification time is 25-40 min.

[0025] In the step (4), the flash evaporation temperature of the first flash evaporator is 75-85°C, the flash evaporation pressure of the first flash evaporator is 0.3-0.5MPa, the flash evaporation temperature of the second flash evaporator is 80-90°C, and the flash evaporation pressure of the second flash evaporator is 0.01-0.05MPa.

[0026] In the step (5), the evaporation concentration temperature is 85-100°C, the evaporation concentration time is 70-90 min, the centrifugal concentration rate is 2500-3500 rad / min, and the centrifugal concentration time is 20-30 min.

[0027] The beneficial effects of the present invention are as follows:

[0028] (1) The positive charge of the primary emulsifier forms a strong adsorption effect with the negative charge on the surface of the oil droplet. At the same time, the ether bond in the co-emulsifier and the hydroxyethyl group of the primary emulsifier form a hydrogen bond, which allows it to be free between the molecules of the primary emulsifier, forming a dynamic adsorption equilibrium. When subjected to high shear force, the co-emulsifier tends to adsorb on the primary emulsifier, forming a more uniform and more stable interfacial film, reducing demulsification and stratification, and promoting emulsion stability.

[0029] (2) The long-chain alkyl group of the primary emulsifier and the alkylphenol group of the auxiliary emulsifier are both large groups and electrically neutral, resulting in a greater hydrophobic effect. The two attract each other, promoting the aggregation of the primary emulsifier and the auxiliary emulsifier, thereby reducing the critical micelle concentration and promoting the dispersibility of the emulsion.

[0030] (3) Since the steric hindrance of the cationic quaternary ammonium salt part of the main emulsifier and the polyoxyethylene chain part of the auxiliary emulsifier are both small, the two will interweave on the surface of the oil droplet to form a composite network structure. Compared with a single emulsifier or existing compounding methods, it provides greater steric hindrance, thereby further preventing the aggregation of emulsion droplets, so that the emulsion can maintain good stability when subjected to external shear force.

[0031] (4) The long-chain alkyl groups of the primary emulsifier are intertwined to form a stable network structure, which further isolates the droplets and reduces the aggregation of the droplets. During long-term storage, the stability and uniformity of the emulsion are better.

[0032] (5) Since the cross-linking effect between the main emulsifier and the auxiliary emulsifier is a reversible physical effect, there is a dynamic equilibrium and no emulsifier flocs will be produced. Therefore, the shortcomings of uneven cross-linking and low cross-linking efficiency of the emulsifier in the chemical cross-linking system are effectively avoided. At the same time, no peroxide cross-linking agent is used, and the biocompatibility is better.

[0033] (6) By adding a lipophilic-hydrophilic regulator, the hydrophilic-lipophilic balance value range of the synergistic system of the primary emulsifier and the auxiliary emulsifier can be flexibly adjusted, so that the polyisoprene latex can meet different application scenarios; at the same time, the lipophilic-hydrophilic regulator is prepared from propylene glycol and ethyl sorbate. Propylene glycol is hydrophilic and can also form hydrogen bonds with the hydroxyethyl group of the primary emulsifier and the ether bond in the auxiliary emulsifier. Ethyl sorbate is a long chain and adsorbed on the surface of the emulsion droplets. It can also be intertwined with the long-chain alkyl group of the primary emulsifier, thereby making the emulsifier molecular interface film more stable, the droplet size more uniform, and the uniformity and stability of the emulsion better. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0035] The present invention is specifically described and illustrated below in conjunction with embodiments.

[0036] Example 1

[0037] like Figure 1 The process flow comprises the following steps: weighing 300 g of dodecyl bis(hydroxyethyl)methylammonium chloride, 35 g of nonylphenol polyoxyethylene ether, 9 g of propylene glycol, and 90 g of ethyl sorbate, adding the mixture into a mixing kettle, and then adding deionized water to prepare 10 kg of an emulsifier aqueous solution; starting the mixing kettle and stirring the mixture at room temperature until the mixture is completely dissolved, thereby obtaining an emulsifier aqueous solution.

[0038] 1800 g of polyisoprene rubber was weighed and added into a mixing kettle, and then n-hexane was added to prepare a polyisoprene rubber solution with a polyisoprene mass fraction of 8%. The mixing kettle was heated to 45° C. and stirred for 30 minutes until the polyisoprene rubber was completely dissolved, thereby obtaining a polyisoprene rubber solution.

[0039] The polyisoprene rubber solution and the emulsifier aqueous solution were added to a mixer, stirred and mixed for 15 minutes, and then added to an emulsification pump, heated to 40°C, the shear rate of the pump was set to 8 m / s, and shear emulsification was performed for 25 minutes to obtain an oil-in-water emulsion.

[0040] The prepared oil-in-water emulsion is added to the first flash evaporator, the flash temperature is set to 75°C, the flash pressure is set to 0.3 MPa, and after the first flash evaporation, it enters the second flash evaporator, and the flash temperature of the second flash evaporator is set to 80°C, and the flash pressure is set to 0.01 MPa for the second flash evaporation.

[0041] The flash-evaporated emulsion was sent to an MVR evaporator for evaporation concentration at 85° C. for 90 min. Finally, the evaporated and concentrated emulsion was sent to a horizontal centrifuge for centrifugal concentration. The speed of the horizontal centrifuge was set to 2500 rad / min. The centrifugal concentration was performed for 30 min to obtain polyisoprene latex.

[0042] Example 2

[0043] like Figure 1 The process flow comprises the following steps: weighing 400 g of stearyl (dihydroxyethyl) methyl ammonium chloride, 95 g of octylphenol polyoxyethylene ether, 50 g of propylene glycol, and 100 g of ethyl sorbate and adding them into a mixing kettle; then adding deionized water to prepare 10 kg of an emulsifier aqueous solution; starting the mixing kettle and stirring, stirring at room temperature until the mixture is completely dissolved, to obtain an emulsifier aqueous solution.

[0044] 3600 g of polyisoprene rubber was weighed and added into a mixing kettle, and then cyclohexane was added to prepare a polyisoprene rubber solution with a mass fraction of 12%. The mixing kettle was heated to 50° C. and stirred for 40 minutes until the polyisoprene rubber was completely dissolved, thereby obtaining a polyisoprene rubber solution.

[0045] The polyisoprene rubber solution and the emulsifier aqueous solution were added to a mixer, stirred and mixed for 30 minutes, and then added to an emulsification pump, heated to 50°C, the shear rate of the pump was set to 14 m / s, and shear emulsification was performed for 40 minutes to obtain an oil-in-water emulsion.

[0046] The prepared oil-in-water emulsion was added to the first flash evaporator, the flash temperature was set to 80°C, and the flash pressure was set to 0.4 MPa. After the first flash evaporation, it entered the second flash evaporator, and the flash temperature of the second flash evaporator was set to 85°C, and the flash pressure was set to 0.03 MPa for the second flash evaporation.

[0047] The flash-evaporated emulsion was sent to an MVR evaporator for evaporation concentration at 90° C. for 80 min. Finally, the evaporated and concentrated emulsion was sent to a horizontal centrifuge for centrifugal concentration. The speed of the horizontal centrifuge was set to 3000 rad / min. After centrifugal concentration for 25 min, polyisoprene latex was obtained.

[0048] Example 3

[0049] like Figure 1 The process flow comprises the following steps: weighing 500 g of hexadecyl methyl dihydroxyethyl ammonium bromide, 150 g of dodecylphenol polyoxyethylene ether, 100 g of propylene glycol, and 100 g of ethyl sorbate, adding the mixture into a mixing kettle, and then adding deionized water to prepare 10 kg of an emulsifier aqueous solution; starting the mixing kettle and stirring the mixture at room temperature until the mixture is completely dissolved, thereby obtaining an emulsifier aqueous solution.

[0050] 6000 g of polyisoprene rubber was weighed and added into a mixing kettle, and cyclohexane was then added to prepare a polyisoprene rubber solution with a polyisoprene mass fraction of 15%. The mixing kettle was heated to 55° C. and stirred for 50 min until the polyisoprene rubber was completely dissolved, thereby obtaining a polyisoprene rubber solution.

[0051] The polyisoprene rubber solution and the emulsifier aqueous solution were added to a mixer, stirred and mixed for 45 minutes, and then added to an emulsification pump, heated to 65° C., the shear rate of the pump was set to 12 m / s, and shear emulsification was performed for 35 minutes to obtain an oil-in-water emulsion.

[0052] The prepared oil-in-water emulsion is added to the first flash evaporator, and the flash temperature and flash pressure are set to 85°C and 0.5 MPa, and after the first flash evaporation, it enters the second flash evaporator, and the flash temperature and flash pressure of the second flash evaporator are set to 90°C and 0.05 MPa for the second flash evaporation.

[0053] The flash-evaporated emulsion was sent to an MVR evaporator for evaporation concentration at 100° C. for 70 minutes. Finally, the evaporated and concentrated emulsion was sent to a horizontal centrifuge for centrifugal concentration. The speed of the horizontal centrifuge was set to 3500 rad / min. After centrifugal concentration for 20 minutes, polyisoprene latex was obtained.

[0054] Example 4

[0055] On the basis of dodecyl bis(hydroxyethyl)methylammonium chloride, nonylphenol polyoxyethylene ether, propylene glycol and ethyl sorbate in Example 1, 5 g of methyl cellulose and 10 g of sodium alginate were added to the mixing kettle, and then deionized water was added to prepare 10 kg of emulsifier aqueous solution. The remaining steps were the same as in Example 1.

[0056] Example 5

[0057] On the basis of stearyl (dihydroxyethyl) methyl ammonium chloride, octylphenol polyoxyethylene ether, propylene glycol and ethyl sorbate in Example 2, 5 grams of carboxymethyl cellulose and 30 grams of sodium tripolyphosphate were added to the mixing kettle, and then deionized water was added to prepare 10 kilograms of emulsifier aqueous solution. The remaining steps were the same as in Example 2.

[0058] Example 6

[0059] On the basis of hexadecylmethyldihydroxyethylammonium bromide, dodecylphenol polyoxyethylene ether, propylene glycol and ethyl sorbate in Example 3, 10 g of hydroxypropyl cellulose and 50 g of gum arabic were added to the mixing kettle, and then deionized water was added to prepare 10 kg of emulsifier aqueous solution. The remaining steps were the same as in Example 3.

[0060] Comparative Example 1

[0061] Propylene glycol and ethyl sorbate were not added, and the remaining steps were the same as in Example 1.

[0062] Comparative Example 2

[0063] No co-emulsifier nonylphenol polyoxyethylene ether was added, and the remaining steps were the same as in Example 1.

[0064] Comparative Example 3

[0065] The primary emulsifier was replaced by sodium dodecylbenzenesulfonate instead of dodecyl bis(hydroxyethyl)methylammonium chloride, and the remaining steps were the same as those in Example 1.

[0066] Comparative Example 4

[0067] 300 g of sodium dodecylbenzene sulfonate, 35 g of nonylphenol polyoxyethylene ether and 30 g of hydrogen peroxide were added to a mixing kettle, and then deionized water was added to prepare 10 kg of an emulsifier aqueous solution, which was used to replace the emulsifier aqueous solution in Example 1. The remaining steps were the same as in Example 1.

[0068] The performance of the polyisoprene latex obtained in Examples 1-6 and Comparative Examples 1-4 was tested, and the data are shown in Table 1.

[0069] Among them, Wufeng LC-100 series high-performance liquid chromatograph was used to determine the content of organic solvents in the emulsion after flash evaporation. Beijing Pinzhi Chuangsi XR-14 series high-speed mechanical stability tester was used to test the shear stability of polyisoprene latex. Yishite LAP-W600 series laser particle size analyzer was used to test the particle size of polyisoprene latex. Based on the SH / T 1154-2011 standard, normal pressure drying at 70°C was selected to determine the solid content of polyisoprene latex. A windowless, light-proof environment was selected indoors, and the humidity range was set to 35-65%RH and the temperature range was set to 0-28°C. Ten groups of specific values ​​were selected from the above ranges to store polyisoprene latex. The ten groups of polyisoprene latex were observed by naked eye to see if there were any discoloration, stratification, precipitation or granulation, and the average value was taken to determine the shelf life of polyisoprene latex.

[0070] Thirty-five mice were selected, with 5 mice in each group. 2 cm of the mouse skin was 2 Partial hair removal treatment: 5 ml of the polyisoprene latex prepared in Examples 1, 2, 3, 4, 5, 6 and Comparative Example 4 was evenly applied to the hair removal area, covered with a patch and bandaged with a bandage, and the above-mentioned application steps were repeated once every 24 hours. After 48 hours, the patch and bandage were removed, the residue was removed, and the skin condition of the mice was observed.

[0071]

[0072] It can be seen from Table 1 that: Comparative Example 1 is the one in which no lipophilic and hydrophilic regulator is added, that is, the hydrophilic-lipophilic balance value of the emulsifier synergistic system is not adjusted; Comparative Examples 2 and 3 are the ones in which no auxiliary emulsifier is added and other main emulsifiers are replaced, respectively, that is, no emulsifier synergistic system is formed.

[0073] Compared with comparative examples 1-3, the polyisoprene latex in Examples 1-3 has a longer shear stability time, a longer shelf life, and a smaller average particle size, that is, better stability and dispersibility; at the same time, after adding stabilizers and thickeners, the stability and dispersibility of Examples 4-6 are also improved to a certain extent compared with Examples 1-3. In comparative example 4, a crosslinking agent, hydrogen peroxide, is added, and compared with Examples 1-6 without adding a peroxide crosslinking agent, mice have an allergic reaction, that is, the biocompatibility is poor.

[0074] Although the present invention is described in detail in conjunction with the embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, those skilled in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions should all be within the scope of the present invention.

Claims

1. A method for preparing polyisoprene latex, characterized in that: The steps include: (1) adding a primary emulsifier, a secondary emulsifier, and a lipophilic and hydrophilic modifier into water to obtain an emulsifier aqueous solution, wherein the primary emulsifier is a long-chain alkyl quaternary ammonium salt; (2) adding polyisoprene rubber to saturated alkane and heating to obtain a polyisoprene rubber solution; (3) mixing the polyisoprene rubber solution with the emulsifier aqueous solution, and then shearing and emulsifying the mixture to obtain an oil-in-water emulsion; (4) passing the oil-in-water emulsion through a first flash evaporator and a second flash evaporator in sequence to remove the solvent; (5) After the solvent is removed, the product is sequentially evaporated and concentrated by centrifugation in an MVR evaporator and centrifuged to obtain polyisoprene latex; In step (1), the main emulsifier is one or more of stearyl (dihydroxyethyl) methyl ammonium chloride, dodecyl bis(hydroxyethyl) methyl ammonium chloride or hexadecyl methyl dihydroxyethyl ammonium bromide; the auxiliary emulsifier is one or more of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether or dodecylphenol polyoxyethylene ether; The lipophilic and hydrophilic regulator is prepared by mixing propylene glycol and ethyl sorbate in a mass ratio of (0.1-1):1; The mass fraction of the main emulsifier in the emulsifier aqueous solution is 3-5%, the mass fraction of the auxiliary emulsifier is 0.35-1.5%, and the mass fraction of the lipophilic and hydrophilic regulator is 1-2%.

2. The method for preparing polyisoprene latex according to claim 1, characterized in that: In step (1), a primary emulsifier, an auxiliary emulsifier, a lipophilic and hydrophilic regulator, a stabilizer and a thickener are added into water to obtain an emulsifier aqueous solution; the stabilizer is one or more of methyl cellulose, carboxymethyl cellulose or hydroxypropyl cellulose, and the thickener is one or more of gum arabic, sodium alginate or sodium tripolyphosphate.

3. The method for preparing polyisoprene latex according to claim 2, characterized in that: The mass fraction of the stabilizer is 0.05-0.1%, and the mass fraction of the thickener is 0.1-0.5%.

4. The method for preparing polyisoprene latex according to claim 1, characterized in that: In step (2), the heating temperature is 45-55° C., the heating time is 30-50 min, the mass fraction of polyisoprene rubber in the polyisoprene rubber solution is 8-15%, and the saturated alkane is n-hexane or cyclohexane.

5. The method for preparing polyisoprene latex according to claim 1, characterized in that: The mass ratio of the primary emulsifier to the polyisoprene rubber is 1:(6-12).

6. The method for preparing polyisoprene latex according to claim 1, characterized in that: In step (3), the mixing time is 15-45 min, the shear emulsification temperature is 40-65° C., the shear emulsification rate is 8-14 m / s, and the shear emulsification time is 25-40 min.

7. The method for preparing polyisoprene latex according to claim 1, characterized in that: In step (4), the flash temperature of the first flash evaporator is 75-85°C, and the flash pressure of the first flash evaporator is 0.3-0.5 MPa; the flash temperature of the second flash evaporator is 80-90°C, and the flash pressure of the second flash evaporator is 0.01-0.05 MPa.

8. The method for preparing polyisoprene latex according to claim 1, characterized in that: In step (5), the evaporation concentration temperature is 85-100°C, the evaporation concentration time is 70-90 min, the centrifugal concentration rate is 2500-3500 rad / min, and the centrifugal concentration time is 20-30 min.

Citation Information

Patent Citations

  • Preparation method of polyisoprene rubber latex

    CN104292473A

  • O / W type emulsion taking Lamepon A as emulsifier and preparation method of O / W type emulsion

    CN112022729A

  • Method for directly preparing polyisoprene latex by using polyisoprene glue liquid

    CN102936346A

  • Method for preparing latex directly from rare-earth polyisoprene glue solution

    CN103772772A