A low-cost high-damping titanium alloy and preparation method thereof

By selecting reasonable element composition and process treatment in high oxygen content titanium alloys, titanium alloys with high beta stability are formed, which solves the problems of high cost and difficult processing of high damping titanium alloys, and achieves high strength, high toughness and wide temperature range. Low-cost, high-damping titanium alloy material with domain damping performance.

CN118668097BActive Publication Date: 2024-10-22INST OF MECHANICS CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411154203.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-22
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing high-damping titanium alloy materials are costly and difficult to process, and their temperature sensitivity and fatigue problems limit their application scope. In particular, the promotion and application of Snoek-type high-damping titanium alloys in industrial production is limited.

Method used

Using low-cost, high-oxygen-content titanium alloys, by rationally selecting the composition ratios of elements such as Fe, Cr, Mo and O, and combining gradient high-temperature treatment and medium-temperature rolling processes, eutectoid and isomorphic alloys with high beta stability are formed. chemical elements, avoid active eutectoid elements, regulate the spatial distribution and morphology of α precipitation phase, introduce deformation-induced twins and heterogeneous structures, and reduce the difficulty and cost of alloy production.

Benefits of technology

The preparation of low-cost high-damping titanium alloy has been achieved. It has excellent comprehensive mechanical properties and damping properties. The tensile strength, yield strength and uniform elongation are significantly improved. The peak damping performance exceeds 0.05. The peak temperature range is wide, making it suitable for industrial production applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118668097B_ABST
    Figure CN118668097B_ABST
Patent Text Reader

Abstract

The present invention provides a low-cost high-damping titanium alloy and a preparation method thereof. The alloy is composed of the following elements in mass percentage: Fe: 2.0-2.5%, Cr: 1.5-2.2%, Mo: 1.5-3%, O: 0.7-0.9%, and the balance is Ti. The preparation method comprises the following steps: (1) ingot smelting; (2) blanking forging; (3) gradient high-temperature treatment; (4) rolling processing: (4.1) medium-temperature rolling, (4.2) room temperature rolling; (5) annealing. The present invention is rationally conceived, not only to obtain a low-cost high-damping titanium alloy material with comprehensive excellent performance, but also to greatly reduce the actual production difficulty of high-oxygen titanium alloy, while combining a short-process process to reduce the alloy cost, and is suitable for promotion and application in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment and preparation of titanium alloy materials, and in particular to a low-cost high-damping titanium alloy and a preparation method thereof. Background Art

[0002] The development of aircraft and weapons and equipment is becoming increasingly high-speed and high-power. The vibration and noise problems caused by the excitation of engines and high-speed airflow are particularly prominent, which puts forward more urgent practical needs for high-performance damping materials. Titanium alloys have received special attention in the aerospace field due to their high specific strength, corrosion resistance, and wide operating temperature. At present, the research on high-damping titanium alloy materials can be divided into two categories: NiTi-based damping titanium alloys based on thermoelastic martensitic phase transformation, and TiNbO-based damping titanium alloys based on Sneok relaxation dissipation theory.

[0003] NiTi series damping titanium alloys have excellent shape memory, superelasticity and good damping performance, and are widely used in the fields of medicine, aviation, aerospace, etc. However, the thermoelastic martensitic phase transformation in NiTi series alloys is very sensitive to temperature changes, which leads to performance instability and can only be used in low temperature and room temperature environments. In addition, NiTi series alloys have problems such as high cost, difficulty in processing, and easy fatigue, which seriously limit their application range.

[0004] The physical mechanism of TiNbO damping titanium alloy based on Sneok relaxation dissipation theory is that under the action of alternating stress, interstitial atoms in different positions in the body-centered cubic crystal consume energy to generate dynamic hysteresis internal friction, thereby producing a damping effect, breaking the problem of NiTi alloys being sensitive to temperature, and improving the use temperature range of damping titanium alloys. However, the existing Snoek-type high damping titanium alloy contains a large amount of β-stabilizing element Nb and interstitial atom O, among which high Nb alloying elements are expensive, and the addition of high O elements reduces the processing deformation ability of the material, resulting in the difficulty of preparation and processing of this type of high damping alloy, long process and high cost, which is the main reason for the limited application of Snoek-type high damping titanium alloy. Therefore, the innovative development of a new generation of low-cost, high-performance Snoek-type damping titanium alloys, as well as the development of related short-process preparation and processing technologies, are of great basic research and practical engineering significance. Summary of the invention

[0005] In response to the technical problems existing in the above-mentioned background technology, the present invention proposes a high-damping titanium alloy material with reasonable conception, which can obtain high-damping titanium alloy material with comprehensive excellent performance, can greatly reduce the actual production difficulty of high-oxygen titanium alloy, and at the same time reduce the alloy cost by combining short-process technology. It is suitable for promoting and applying low-cost high-damping titanium alloy and its preparation method to industrial production.

[0006] To solve the above technical problems, the present invention provides a low-cost high-damping titanium alloy, which is composed of the following elements in mass percentage: Fe: 2.0~2.5%, Cr: 1.5~2.2%, Mo: 1.5~3%, O: 0.7~0.9%, and the balance is Ti.

[0007] The low-cost high-damping titanium alloy, wherein: the tensile strength of the alloy is ≥800MPa, the yield strength is greater than or equal to 650MPa, the uniform elongation is greater than or equal to 25%, and the elongation at break is ≥30%.

[0008] The low-cost high-damping titanium alloy, wherein: the damping performance peak of the alloy exceeds 0.05, the peak temperature range is 220~260°C, and the half-peak width is 80~160°C.

[0009] A method for preparing a low-cost high-damping titanium alloy mainly comprises the following steps:

[0010] (1) Ingot Melting

[0011] After the raw materials are evenly mixed, a high damping titanium alloy material ingot with uniform composition is prepared by a vacuum melting method;

[0012] (2) Forging

[0013] The surface of the high damping titanium alloy material ingot prepared in the above step (1) is mechanically ground, and then the sample after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace, the sample is heated to a target temperature T0 and kept at this temperature for a time of t0, and then upsetting and drawing treatment is performed and shaping and coiling is performed, and then cooling is performed in air to obtain a plate blank with a target thickness of D0;

[0014] (3) Gradient high temperature treatment

[0015] The surface of the plate blank obtained in the above step (2) is mechanically ground, and then the plate blank after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace, the plate blank is heated to a target temperature T1 in the heat treatment furnace and kept at a temperature for a time of t1, and then cooled to a target temperature T2 and kept at a temperature for a time of t2 along with the heat treatment furnace at a target cooling rate v1, and the plate blank is taken out and cooled in air;

[0016] (4) Rolling processing

[0017] (4.1) Medium temperature rolling

[0018] The plate blank after the gradient high temperature treatment in step (3) is directly placed in a heat treatment furnace at a temperature of T3, argon is introduced into the heat treatment furnace and the heat preservation time is t3, and then a medium temperature rolling process is performed, and the reduction amount is △d , put it into the heat treatment furnace again for heat preservation, and repeat the steps of heat preservation and rolling again and again until the total rolling reduction is half of D0, that is, the cumulative rolling reduction is 50%, and the rolled plate is cooled in air;

[0019] (4.2) Room temperature rolling

[0020] The rolled plate obtained in the above step (4.1) is rolled with a reduction of △ d Performing reciprocating rolling treatment at room temperature until the total rolling reduction is 80-95%, thereby obtaining a primary rolled plate of a high damping titanium alloy;

[0021] (5) Annealing

[0022] The high damping titanium alloy primary rolled plate obtained in the above step (4.2) is placed in a heat treatment furnace at a temperature of T4 and flowing argon gas is introduced. After a holding time of t4, the plate is taken out for cooling and the flowing argon gas is turned off. The surface of the plate obtained after cooling is decontaminated, and finally a low-cost high damping titanium alloy material is obtained.

[0023] The method for preparing the low-cost high-damping titanium alloy, wherein: the temperature T0 in the step (2) is 1100°C to 1200°C, and the holding time t0 is 6h to 8h.

[0024] The method for preparing the low-cost high-damping titanium alloy, wherein: before the gradient high-temperature treatment in step (3), the plate blank must be subjected to a thermal expansion analysis to obtain the α and β allotropic transition temperatures T of the alloy. α / β , in gradient high temperature treatment, T1=(T α / β +20~80)°C, T2=(T α / β -10~60)°C, the insulation time t1 is 10min~60min, t2 is 20min~120min, and the cooling rate v1 of T1 to T2 with the furnace is 1~5min / °C.

[0025] The method for preparing a low-cost high-damping titanium alloy, wherein: the temperature T3 of the medium-temperature rolling process in the step (4.1) is 580-640°C, the holding time t3 is 3-20min; and the thickness of the plate blank before each rolling pass is d j , the amount of pressure per pass△ d = d j * (2%~5%).

[0026] The method for preparing a low-cost high-damping titanium alloy, wherein: the target temperature T4 in the annealing treatment in step (5) = (T α / β-30~200)°C, and the insulation time t4 is 5~120min.

[0027] The method for preparing the low-cost high-damping titanium alloy, wherein: the vacuum melting method in step (1) includes vacuum suspension melting, vacuum consumable melting and vacuum non-consumable melting.

[0028] The method for preparing the low-cost high-damping titanium alloy, wherein: the upsetting and drawing treatment in the step (2) is performed by using a high-speed forging machine to perform multiple forging and drawing processes, first forging and deforming the height direction, then forging and deforming the width direction, and then forging and deforming the length direction, and repeating the process multiple times to refine the grains.

[0029] By adopting the above technical solution, the present invention has the following beneficial effects:

[0030] The low-cost high-damping titanium alloy of the present invention takes into account the use of eutectoid and isomorphous alloying elements with high β-stabilizing ability, and intentionally avoids elements with low β-stabilizing ability. When selecting eutectoid β-stabilizing elements, considering the large difference in the speed of eutectoid reaction between eutectoid elements and titanium, active eutectoid elements Si, Cu, Ni, etc. are avoided because their eutectoid reaction speed is fast and the β-stabilizing effect is poor. Fe and Cr, as inactive eutectoid elements, both have strong β-stabilizing ability, among which Fe element is low in cost, but its excessive addition is prone to segregation, and its content should be controlled to be less than 3%; Cr element is one of the most widely used β-stabilizing elements, and also has strong β-stabilizing ability, but excessive addition will precipitate compounds and lead to reduced plasticity, and its content should also be controlled. By adding Fe and Cr in small amounts at the same time, their strong β-stabilizing ability can be utilized and their non-beneficial effects can be avoided. The isomorphous β-stabilizing elements such as Mo, V, and Nb have an atomic radius close to that of titanium and the same lattice structure, which can achieve infinite mutual solubility in the β phase and significantly improve the strength and hardenability of the alloy. However, the cost of alloying elements is relatively high. In order to balance the stability of the β phase with the alloying cost, it is finally decided to add a small amount of Mo element, which can take into account the advantages of isomorphous elements without greatly increasing the cost of the alloy. The addition of interstitial atomic O element is mainly based on the Snoek relaxation damping effect. At the same time, the α-stabilizing element Al is not added, mainly because O has a stronger α-stabilizing element effect. Using O instead of Al reduces the cost of the alloy and reduces the volatilization of elements during vacuum melting. Finally, based on the titanium alloy d The calculation method in electronic design theory, combined with the differences in plastic deformation modes under different alloy stability, was used to determine the addition range of alloying elements such as Fe, Cr, Mo, and O, and relevant experimental verification was carried out.

[0031] The present invention not only obtains high damping titanium alloy materials by adding high O elements, but also solves the problems of difficult processing and low deformation capacity of alloys with high O addition. Based on the Snoek relaxation dissipation theory, the key core point is the addition of the interstitial element O, while traditional alloy design considers O to be a harmful element in titanium alloys, which significantly improves the crack extension ability of the alloy and reduces the plasticity of the alloy. When designing the alloy composition, the present invention changes the plastic deformation mode of the matrix β phase by adjusting the addition amount of alloying elements, introduces stress-induced deformation twins, and utilizes its dynamic grain refinement to improve the deformation capacity of the alloy, while shortening the hot working process of traditional titanium alloys.

[0032] The preparation method of the low-cost high-damping titanium alloy of the present invention has a reasonable concept and a simple process. It is a short-process preparation and processing method for high-damping titanium alloy. By coupling the gradient high-temperature precipitation control and the medium-temperature rolling treatment process, the mechanism of dynamic grain refinement of deformation-induced twinning is utilized, and the parameters such as the spatial distribution, content, and morphology of the α precipitation phase are optimized, and the content of recrystallized grains and heterogeneous interfaces are regulated to prepare a low-cost high-damping titanium alloy material with a heterogeneous structure. During the preparation process, the appearance of deformation-induced twinning enhances the plastic deformation ability of the high-oxygen content titanium alloy and improves the cold and hot processing ability of the alloy. During the processing and deformation process, the heterogeneous structure induces an additional work hardening effect, which simultaneously improves the strength and plasticity of the alloy. In addition, by optimizing the selection of alloying elements in titanium alloys and adjusting the content of elements, such as Fe is 2.0~2.5%, Cr is 1.5~2.2%, Mo is 1.5~3% and O is 0.7~0.9%, without adding element Al, and the balance is Ti, a short-process preparation and processing method is used to solve the technical bottleneck problems of high cost and difficult processing of high-oxygen-content Snoek-type high-damping titanium alloys in the existing technology.

[0033] The preparation method of the present invention utilizes a combination of gradient high temperature treatment and rolling processing, and introduces heterogeneous deformation-induced work hardening by adjusting the spatial distribution, content and morphology of the α precipitated phase and other variables, thereby greatly improving the plastic deformation capacity of the alloy, and also shortening the processing flow of the high damping titanium alloy.

[0034] The low-cost high-damping titanium alloy material prepared by the preparation method of the present invention has excellent comprehensive mechanical properties and damping properties; the low-cost high-damping titanium alloy material has a tensile strength ≥800MPa, a yield strength ≥650MPa, a uniform elongation ≥25%, and a fracture elongation ≥30%, showing an excellent strength-plasticity matching relationship; the low-cost high-damping titanium alloy material has a damping performance (tanδ) peak value exceeding 0.05, a peak temperature range of 220~260°C, and a half-peak width of 80~160°C, and has excellent damping performance and a wide temperature range service environment.

[0035] The low-cost high-damping titanium alloy material prepared by the preparation method of the present invention changes the stability of the β-phase matrix by adjusting the content of the α precipitated phase, and the β-phase matrix can undergo deformation twinning plastic deformation under stress induction.

[0036] After the low-cost high-damping titanium alloy material prepared by the preparation method of the present invention is subjected to high-temperature gradient treatment, the matrix of the β phase undergoes stress-induced phase transformation or deformation twinning during the rolling process. This phenomenon has the effect of dynamically refining the grains during the processing, significantly reducing the deformation resistance of the alloy and improving the efficiency of the microstructure refinement of the low-cost high-damping titanium alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 It is a schematic flow chart of the method for preparing the low-cost high-damping titanium alloy of the present invention;

[0039] Figure 2 It is a schematic diagram of the gradient high temperature treatment and rolling processing process involved in the preparation method of the low-cost high-damping titanium alloy of the present invention;

[0040] Figure 3 A tensile engineering stress-strain curve diagram of a tensile performance curve of a low-cost high-damping titanium alloy material prepared by the method for preparing a low-cost high-damping titanium alloy according to Example 1 of the present invention;

[0041] Figure 4 This is a damping coefficient curve of the high-damping titanium alloy material prepared by the method for preparing a low-cost high-damping titanium alloy according to Example 2 of the present invention. DETAILED DESCRIPTION

[0042] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] The present invention is further explained below in conjunction with specific implementation modes.

[0044] The low-cost high-damping titanium alloy of the present invention is composed of the following elements in percentage by mass: Fe: 2.0-2.5%, Cr: 1.5-2.2%, Mo: 1.5-3%, O: 0.7-0.9%, and the balance is Ti.

[0045] The low-cost high-damping titanium alloy of the present invention has excellent comprehensive mechanical properties and damping properties, with a tensile strength of ≥800MPa, a yield strength of ≥650MPa, a uniform elongation of ≥25%, and a fracture elongation of ≥30%, showing an excellent strength-plasticity matching relationship; the damping performance (tanδ) peak value of the low-cost high-damping titanium alloy of the present invention exceeds 0.05, the peak temperature range is 220~260°C, and the half-peak width is 80~160°C, and it has excellent damping performance and a wide temperature range service environment.

[0046] The low-cost high-damping titanium alloy of the present invention changes the stability of the β-phase matrix by adjusting the content of the α precipitated phase, and the β-phase matrix can undergo deformation twinning plastic deformation under stress induction.

[0047] like Figure 1-2 As shown, the preparation method of the low-cost high-damping titanium alloy of the present invention mainly comprises the following steps:

[0048] (1) Ingot Melting

[0049] The raw materials (including titanium sponge, pure titanium foil, iron particles, molybdenum particles, pure chromium sheets, titanium oxide powder, etc.) are mixed evenly, and then a vacuum melting method (generally including vacuum suspension melting, vacuum consumable melting, vacuum non-consumable melting, etc.) is used to prepare a high damping titanium alloy material ingot with uniform composition;

[0050] (2) Forging

[0051] The surface of the high damping titanium alloy material ingot prepared in the above step (1) is mechanically ground (specifically, a handheld angle grinder is used to grind and remove the oxide layer on the surface of the ingot, as well as impurity particles in some pit defects, etc.), and then the sample after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace (high-density argon gas is used to protect the sample to significantly reduce the degree of oxidation on its surface), and heated to the target temperature T0 under the protection of flowing argon gas and kept at this temperature for a time of t0, and then subjected to upsetting and drawing treatment (i.e., multiple forging and drawing treatments are performed using a fast forging machine, first forging and deforming the sample in the height direction by about 30%, then forging and deforming the sample in the width direction by about 30%, and then forging and deforming the sample in the length direction, and the process is repeated multiple times to refine the grains) and subjected to shaping and coiling (i.e., the sample is adjusted in length, width and height to obtain a sample of the envisioned size), and then cooled in air to obtain a plate blank with a target thickness of D0;

[0052] (3) Gradient high temperature treatment

[0053] The surface of the plate blank obtained in the above step (2) is subjected to mechanical grinding (i.e., a hand-held angle grinder is used to remove the surface oxide scale and high-density fine cracks of the plate blank obtained in the above step (2) to obtain a plate blank with a smooth surface), and then the plate blank after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace, and heated to a target temperature T1 under the protection of the flowing argon gas, and the holding time is t1, and cooled to a target temperature T2 and the holding time is t2 along with the heat treatment furnace at a target cooling rate ν1, and the plate blank is taken out and cooled in air;

[0054] (4) Rolling processing

[0055] (4.1) Medium temperature rolling

[0056] The plate blank after the gradient high temperature treatment in step (3) is directly placed in a heat treatment furnace at a temperature of T3, and argon is introduced into the heat treatment furnace. Under the protection of flowing argon (the rate of introduction depends on the size of the furnace), the heat preservation time is t3, and then a medium temperature rolling process is performed, and the reduction amount is △ d , put it into the heat treatment furnace again for heat preservation, and repeat the steps of heat preservation-rolling again and again until the total rolling reduction is half of D0, that is, the cumulative rolling reduction is 50%, and the obtained rolled plate is air-cooled;

[0057] (4.2) Room temperature rolling

[0058] The rolled plate obtained in the above step (4.1) is rolled with a reduction of △ d Performing reciprocating rolling treatment at room temperature until the total rolling reduction is 80-95%, thereby obtaining a primary rolled plate of a high damping titanium alloy;

[0059] (5) Annealing

[0060] The high damping titanium alloy primary rolled plate obtained in the above step (4.2) is placed in a heat treatment furnace at a temperature of T4 and flowing argon gas is introduced. After a holding time of t4, the plate is taken out for cooling and the flowing argon gas is turned off. The surface of the plate obtained after cooling is decontaminated (i.e., mechanical grinding is performed to remove the oxide scale on the surface of the plate), and finally a low-cost high damping titanium alloy material is obtained.

[0061] The temperature T0 in the above step (2) is 1100°C~1200°C, and the insulation time t0 is 6h~8h.

[0062] Before the gradient high temperature treatment in step (3) above, the plate blank needs to be subjected to thermal expansion analysis to obtain the α and β allotropic transformation temperatures T of the low-cost high-damping titanium alloy. α / β , in gradient high temperature treatment, T1=(T α / β+20~80)°C, T2=(T α / β -10~60)°C, the insulation time t1 is 10min~60min, t2 is 20min~120min, and the cooling rate v1 of T1 to T2 with the furnace is 1~5min / °C.

[0063] The temperature T3 of the medium temperature rolling process in the above step (4.1) is 580-640°C, the holding time t3 is 3-20min; and the thickness of the plate before each rolling is d j , the amount of pressure per pass△ d = d j * (2%~5%).

[0064] The target temperature T4 in the annealing process in the above step (5) is (T α / β -30~200)°C, and the insulation time t4 is 5~120min.

[0065] After the low-cost high-damping titanium alloy material obtained in the above step (5) is subjected to high-temperature gradient treatment, stress-induced phase transformation or deformation twinning occurs in the β-phase matrix during rolling. This phenomenon has the effect of dynamically refining the grains during processing, significantly reducing the deformation resistance of the alloy and improving the efficiency of microstructure refinement of the low-cost high-damping titanium alloy.

[0066] Example 1

[0067] The method for preparing the low-cost high-damping titanium alloy according to Example 1 of the present invention specifically comprises the following steps:

[0068] S110, Ingot Melting

[0069] Sponge titanium, pure Cr flakes, pure Fe particles, pure Mo particles and TiO2 powder are used as raw materials for smelting alloys and are proportioned according to target mass percentages. After the raw materials are evenly mixed, vacuum melting technology is used to melt and prepare high-damping titanium alloy material ingots with uniform composition.

[0070] S120, billet forging

[0071] The high damping titanium alloy ingot obtained in the above step S110 is subjected to mechanical grinding after the head and tail parts and the surface are removed, and then heated to the target temperature T0=1150°C and the holding time is t0=6h under the protection of flowing argon gas, and then directly subjected to two-pass upsetting and drawing treatments, followed by shaping and coiling, and then cooled in air to obtain a plate blank with a target thickness of D0=120mm;

[0072] S130, gradient high temperature treatment

[0073] The surface of the plate blank obtained in step S120 is subjected to mechanical grinding, and the allotropic transformation temperature of the alloy is tested by thermal expansion analysis, i.e., T α / β =833°C; then, under the protection of flowing argon, the plate blank after grinding is heated with the furnace to the target temperature T1=870°C and the holding time is t1=30min, and is cooled with the furnace to the target temperature T2=800°C and the holding time is t2=60min at the target cooling rate v1=2min / °C, and the plate blank is taken out and cooled in the air;

[0074] S140, rolling processing

[0075] The surface of the plate blank after the gradient high temperature treatment in the above step S130 is subjected to mechanical grinding processing; specifically comprising:

[0076] S141, medium temperature rolling stage

[0077] The sheet blank is directly placed in a heating furnace at a temperature of T3 = 600 ° C, and the temperature is kept for t3 = 10 min under the protection of flowing argon gas, and then a medium temperature rolling process is performed, and the reduction is 2.4 mm (△ d = d i * 2%) (i=1,2,3…), put it into the furnace again for heat preservation, and repeat the rolling-heat preservation process until the total rolling reduction is D1=60mm, that is, the cumulative deformation ε1=50%, and cool the medium temperature rolled plate in air;

[0078] S142, room temperature rolling stage

[0079] The rolled plate obtained in step S141 is subjected to the same rolling reduction amount of △ d =d j * 3% (j=1,2,3…) until the total rolling reduction is D2=12mm, that is, the total deformation is 90%, and the primary rolled plate of high damping titanium alloy is obtained;

[0080] S150, annealing

[0081] The primary rolled plate of the high damping titanium alloy obtained in the above step S142 is subjected to surface mechanical grinding and decontamination treatment to finally obtain a low-cost high damping titanium alloy material.

[0082] Among them, the primary rolled plate is annealed at a target temperature T4=770°C and a holding time t4=30min under the protection of flowing argon gas, and the annealed primary rolled plate is quickly taken out of the furnace and directly thrown into water for cooling, and then the surface of the cooled plate is mechanically decontaminated to finally obtain a low-cost and high-damping titanium alloy material.

[0083] Table 1 shows the measured element composition mass fractions of the low-cost and high-damping titanium alloy material prepared in Example 1 of the present invention, wherein the Fe element content is 1.87%, the Cr element content is 2.21%, the Mo element content is 3.14%, the O element is 0.84%, the N element is 0.016%, the H element is 0.0041%, the impurity Al element is 0.02%, and the rest is Ti element.

[0084] Figure 3 The solid line in FIG. 1 is the tensile performance curve of the low-cost high-damping titanium alloy material prepared in Example 1 of the present invention. The low-cost high-damping titanium alloy material prepared in Example 1 of the present invention adopts 5 x 10 -4 s -1 Quasi-static tensile rate, uniaxial tensile test was carried out at room temperature on a standard testing machine (Instron 8801). The test results show that the yield strength (σ 0.2 ) is 682MPa, and the tensile strength (σ b ) is 819MPa and uniform elongation (ε u ) is 38%, showing excellent strength and plasticity matching and has a wide range of application scenarios.

[0085] Figure 4 The solid line in is the damping coefficient curve of the low-cost high-damping titanium alloy material prepared in Example 1 of the present invention. The damping test was carried out using a dynamic thermal mechanical analyzer (DMA, TA Q800), and the three-point bending mode test was selected. The implementation conditions were a heating rate of 4°C / min, a frequency of 1Hz, an amplitude of 30μm, and a temperature range of room temperature ±400°C. The test results show that under the preparation conditions of Example 1 of the present invention, the alloy damping coefficient tanδ reaches a peak value of 0.044 at 232°C.

[0086] It can be seen from this that based on the preparation method of the low-cost high-damping titanium alloy developed in Example 1 of the present invention, the low-cost high-damping titanium alloy material can achieve high damping performance while taking into account high uniform tensile elongation, thereby obtaining a low-cost high-damping titanium alloy material with integrated high-performance functional structure.

[0087] Example 2

[0088] The method for preparing the low-cost high-damping titanium alloy according to Example 2 of the present invention specifically comprises the following steps:

[0089] S210, Ingot Melting

[0090] Sponge titanium, pure Cr flakes, pure Fe particles, pure Mo particles and TiO2 powder are used as raw materials for smelting alloys and are proportioned according to target mass percentages. After the raw materials are evenly mixed, a vacuum smelting method is used to smelt and prepare a high-damping titanium alloy material ingot with uniform composition;

[0091] S220, billet forging

[0092] The high damping titanium alloy ingot is mechanically ground after removing the head and tail and the surface, and then heated to the target temperature T0=1180°C and the holding time is t0=4h under the protection of flowing argon gas, and then directly subjected to two-pass upsetting and drawing treatments, followed by shaping and coiling, and then cooled in air to obtain a plate blank with a target thickness of D0=100mm;

[0093] S230, gradient high temperature treatment

[0094] The surface of the sheet blank was mechanically ground, and the allotropic transformation temperature of the alloy, i.e., T α / β =846°C; then, under the protection of flowing argon, the plate blank after grinding is heated with the furnace to the target temperature T1=880°C and the holding time is t1=30min, and is cooled with the furnace to the target temperature T2=820°C and the holding time is t2=90min at the target cooling rate v1=2min / °C, and the plate blank is taken out for cooling in the air;

[0095] S240, rolling processing

[0096] The surface of the plate blank after the gradient high temperature treatment is subjected to mechanical grinding processing; specifically including:

[0097] S241, medium temperature rolling stage

[0098] The sheet blank is directly placed in a heating furnace with a temperature of T3 = 580 ° C, and the temperature is kept for t3 = 8 min under the protection of flowing argon gas, and then a medium temperature rolling process is performed with a reduction of 2.0 mm (△ d = d i * 2%) (i=1,2,3…), put it into the furnace again for heat preservation, and repeat the rolling-heat preservation process until the total rolling reduction is D1=50mm, that is, the cumulative deformation ε1=50%, and cool the medium temperature rolled plate in air;

[0099] S242, room temperature rolling stage

[0100] The rolled plate obtained in step S241 is subjected to the same rolling reduction amount of △ d =d j * 3% (j=1,2,3…) until the total rolling reduction is D2=12mm, that is, the total deformation is 88%, and the primary rolled plate of high damping titanium alloy is obtained;

[0101] S250, annealing

[0102] The primary rolled plate of the high damping titanium alloy obtained in the above step S142 is subjected to surface mechanical grinding and decontamination treatment to finally obtain a low-cost high damping titanium alloy material;

[0103] Among them, the primary rolled plate is annealed at a target temperature T4=760°C and a holding time t4=20min under the protection of flowing argon gas, and the primary rolled plate is quickly taken out of the furnace and directly thrown into water for cooling treatment, and then the surface of the primary rolled plate after cooling treatment is mechanically decontaminated, finally obtaining a low-cost and high-damping titanium alloy material.

[0104] Table 1 shows the measured element composition mass fractions of a low-cost, high-damping titanium alloy prepared in Example 2, wherein the Fe element content is 2.07%, the Cr element content is 2.19%, the Mo element content is 2.26%, the O element is 0.83%, the N element is 0.013%, the H element is 0.0032%, the impurity Al element is 0.03%, and the rest is Ti element.

[0105] Figure 3 The dotted line in the figure is the tensile performance curve of the low-cost high-damping titanium alloy prepared in Example 2. The low-cost high-damping titanium alloy material prepared in Example 2 adopts 5 x 10 -4 s -1 The quasi-static tensile rate was used to perform uniaxial tensile tests at room temperature using a standard testing machine (Instron 8801). The test results show that the yield strength (σ 0.2 ) is 675MPa, and the tensile strength (σ b ) is 909MPa and uniform elongation (ε u ) is 26%, showing excellent matching of strength and plasticity.

[0106] Figure 4The dashed and solid lines in the figure are the damping coefficient curves of the high damping titanium alloy material prepared in Example 2. The damping test was performed using a dynamic thermal mechanical analyzer (DMA, TA Q800), and the three-point bending mode test was selected. The heating rate was 4°C / min, the frequency was 1Hz, the amplitude was 30μm, and the temperature range was room temperature ±400°C. The test results show that under the preparation conditions of Example 2, the alloy damping coefficient tanδ reached a peak value of 0.056 at 247°C.

[0107]

[0108] It can be seen from this that the preparation method of the low-cost high-damping titanium alloy developed based on Example 2, the low-cost high-damping titanium alloy takes into account both high uniform tensile elongation and tensile strength while maintaining high damping performance, thereby obtaining a high-performance functional structure integrated high-damping titanium alloy material, which has broad application prospects.

[0109] In view of the high cost and difficult preparation and processing of Snoek-type high-damping titanium alloys, the present invention adopts low-cost alloying elements to design alloy components, introduces deformation-induced dynamic twinning refinement structure and heterogeneous structure induction to produce additional work hardening effect, so as to improve the processing deformation ability of high-O content alloys and shorten the processing and preparation process, thereby achieving all-round cost reduction from alloy design to processing and preparation, and obtaining a titanium alloy material with high damping, high strength and high toughness.

[0110] The present invention adopts low-cost alloying elements and a short-process preparation and processing method, which greatly reduces the comprehensive cost of high-damping titanium alloy materials. In the preparation method of the present invention, the number and spatial distribution of precipitated phases are adjusted through gradient high-temperature treatment and rolling processing, thereby controlling the occurrence of deformation twins and stress-induced phase transformation, and obtaining a high-damping titanium alloy material with a heterogeneous lamellar structure of precipitated phases and recrystallized grains. The traditional dual-state structure or equiaxed structure of titanium alloy is converted into a heterogeneous lamellar structure, and the dynamic fine grain strengthening mechanism of deformation twins is utilized to shorten the preparation and processing flow, and the heterogeneous deformation-induced work hardening behavior is utilized to obtain a short-process, high-strength, high-damping titanium alloy material. The preparation method of the present invention is only processed through traditional heat treatment and rolling process, which reduces the actual production difficulty of high-oxygen titanium alloys, and at the same time reduces the alloy cost by combining the short-process technology, which is suitable for promotion and application in industrial production.

[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a low-cost high-damping titanium alloy, characterized in that: The main steps include: (1) Ingot Melting After the raw materials are evenly mixed, a high damping titanium alloy material ingot with uniform composition is prepared by a vacuum melting method; (2) Forging The surface of the high damping titanium alloy material ingot prepared in the above step (1) is mechanically ground, and then the sample after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace, the sample is heated to a target temperature T0 and kept at this temperature for a time of t0, and then upsetting and drawing treatment is performed and shaping and coiling is performed, and then cooling is performed in air to obtain a plate blank with a target thickness of D0; (3) Gradient high temperature treatment The surface of the plate blank obtained in the above step (2) is mechanically ground, and then the plate blank after mechanical grinding is placed in a heat treatment furnace and argon gas is flowed into the heat treatment furnace, the plate blank is heated to a target temperature T1 in the heat treatment furnace and kept at a temperature for a time of t1, and then cooled to a target temperature T2 and kept at a temperature for a time of t2 along with the heat treatment furnace at a target cooling rate v1, and the plate blank is taken out and cooled in air; (4) Rolling processing (4.1) Medium temperature rolling The plate blank after the gradient high temperature treatment in step (3) is directly placed in a heat treatment furnace at a temperature of T3, argon is introduced into the heat treatment furnace and the heat preservation time is t3, and then a medium temperature rolling process is performed, and the reduction amount is △ d , put it into the heat treatment furnace again for heat preservation, and repeat the steps of heat preservation and rolling again and again until the total rolling reduction is half of D0, that is, the cumulative rolling reduction is 50%, and the rolled plate is cooled in air; (4.2) Room temperature rolling The rolled plate obtained in the above step (4.1) is rolled with a reduction of △ d Performing reciprocating rolling treatment at room temperature until the total rolling reduction is 80-95%, thereby obtaining a primary rolled plate of a high damping titanium alloy; (5) Annealing The high damping titanium alloy primary rolled plate obtained in the above step (4.2) is placed in a heat treatment furnace at a temperature of T4 and flowing argon gas is introduced. After a holding time of t4, the plate is taken out for cooling and the flowing argon gas is turned off. The surface of the plate obtained after cooling is decontaminated, and finally a low-cost high damping titanium alloy material is obtained; Before the gradient high temperature treatment in step (3), the sheet blank must be subjected to thermal expansion analysis to obtain the α and β allotropic transition temperatures T of the alloy. α / β , in gradient high temperature treatment, T1=(T α / β +20~80)°C, T2=(T α / β -10~60) ° C, while the holding time t1 is 10min~60min, t2 is 20min~120min, and the rate ν1 of T1 cooling to T2 with the furnace is 1~5min / °C; The temperature T3 of the medium temperature rolling process in step (4.1) is 580-640°C, the holding time t3 is 3-20min; and the thickness of the plate blank before each rolling pass is d j , the amount of pressure per pass△ d = d j * (2%~5%); The low-cost high-damping titanium alloy material in step (5) is composed of the following elements in mass percentage: Fe: 2.0-2.5%, Cr: 1.5-2.2%, Mo: 1.5-3%, O: 0.7-0.9%, and the balance is Ti.

2. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that : The temperature T0 in step (2) is 1100°C~1200°C, and the insulation time t0 is 6h~8h.

3. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that: The target temperature T4 in the annealing treatment in step (5) is (T α / β -30~200)°C, and the insulation time t4 is 5~120min.

4. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that: The vacuum melting method in step (1) includes vacuum suspension melting, vacuum consumable melting and vacuum non-consumable melting.

5. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that: The upsetting and drawing process in step (2) is a multi-pass forging and drawing process using a high-speed forging machine, first forging and deforming the material in the height direction, then forging and deforming the material in the width direction, and then forging and deforming the material in the length direction, and the process is repeated multiple times to refine the grains.

6. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that: The low-cost high-damping titanium alloy material in step (5) has a tensile strength of ≥800 MPa, a yield strength of ≥650 MPa, a uniform elongation of ≥25%, and a fracture elongation of ≥30%.

7. The method for preparing a low-cost high-damping titanium alloy according to claim 1, characterized in that: The low-cost high-damping titanium alloy material in step (5) has a damping performance peak value exceeding 0.05, a peak temperature range of 220-260°C, and a half-peak width of 80-160°C.

Citation Information

Patent Citations

  • Method for manufacturing titanium and titanium alloy bars by means of hot continuous rolling

    CN104148382A

  • Preparation method of high-strength T9S titanium alloy plate

    CN110484758A

  • Preparation method of titanium alloy plate

    CN112795798A

  • Lightweight high-toughness high-damping titanium alloy and preparation method thereof

    CN116445762A

  • Titanium alloy having high elastic deformability and its manufacturing method