A method for preparing water-proof polyester tire
By activating and epoxidizing sepiolite during the preparation of polyester tires and modifying its surface to form a firm combination with polyethylene terephthalate, the tensile and toughness of polyester tires is solved. The problem of insufficient water loss has achieved high performance anti-seepage effect and thermal stability.
Patent Information
- Application Number
- CN202411146995.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing polyester tires have shortcomings in tensile and toughness, especially after thermal aging, which significantly reduces its performance, limiting its performance.
By activating sepiolite and epoxidation, preparation of anti-seepage additives, mixtures, preparation of polyester grey cloth and post-treatment steps, the method of activating sepiolite and epoxy Its surface is modified and modified to form a firm combination with polyethylene terephthalate, improving its toughness and waterproofing properties.
The obtained water-resistant polyester tire has excellent tensile force and toughness, and still maintains high mechanical properties after thermal aging, and has good waterproof performance, high stability and strength.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester tires, and in particular relates to a method for preparing a water-proof polyester tire. Background Art
[0002] Polyester is a kind of non-woven fabric, also known as polyester felt base fabric. It has the advantages of high strength, puncture resistance, light weight and high tensile strength, and is widely used in the construction industry.
[0003] Polyester tires are mainly divided into long-fiber polyester tires and short-fiber polyester tires. Long-fiber polyester tires are made of polyester chips as raw materials, and are made through equipment spinning, needle punching reinforcement, and dipping and shaping; short-fiber polyester tires are a kind of non-woven fabric product made of 100% polyester staple fibers through processes such as combing into a web, needle punching reinforcement, and dipping and shaping; because long-fiber polyester tires have good elongation properties, they are widely used in the production of standard asphalt waterproofing membrane products.
[0004] CN113789610A discloses a highly toughened polyester tire and a preparation method thereof, specifically disclosing that the highly toughened polyester tire comprises polyester and a modified thermoplastic elastomer; wherein the modified thermoplastic elastomer is a thermoplastic elastomer grafted and modified by a modifier; the modifier is prepared by reacting 1,3,5-tris(3,3,3-trifluoropropyl)trimethylcyclotrisiloxane and epoxy-modified polysiloxane, and epoxy groups, siloxane bonds, cyclic structure groups, fluorine groups, etc. are introduced into the thermoplastic elastomer, thereby significantly improving the toughness, heat resistance and waterproof properties of the polyester tire.
[0005] However, the polyester tire produced by this patent has low tensile strength, and the tensile strength and toughness after heat aging are significantly reduced, which greatly limits the performance of use.
[0006] CN117604774A discloses a hydrophobic polyester tire base fabric, a preparation method and a waterproof coiled material. The hydrophobic polyester tire base fabric comprises a polyester grey cloth and a modified corn starch layer arranged on the surface of the polyester grey cloth. The polyester tire base fabric prepared by the method has good waterproof performance and good oleophilic effect, but low tensile strength, and the tensile strength and toughness after heat aging are significantly reduced. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a water-proof polyester tire, which has good waterproof performance, excellent tensile strength, and still has strong tensile strength and toughness after thermal aging.
[0008] In view of the above technical problems, the present invention adopts the following technical solutions:
[0009] A method for preparing a water-proof polyester tire comprises the steps of preparing carboxylated polyethylene terephthalate, epoxidizing sepiolite, preparing a water-proof additive, mixing materials, preparing a polyester grey cloth, and post-processing. The specific operations are as follows:
[0010] 1. Preparation of carboxylated polyethylene terephthalate
[0011] The polyethylene terephthalate is soaked in an isopropanol solution for 48-52 minutes, taken out after soaking, and then soaked in a sulfuric acid solution for 24-26 minutes. After soaking, the polyethylene terephthalate is washed and dried at 62-64° C. to obtain carboxylated polyethylene terephthalate;
[0012] The mass concentration of the isopropanol solution is 45-49%;
[0013] The mass concentration of the sulfuric acid solution is 16-20%;
[0014] The mass ratio of the polyethylene terephthalate, the isopropanol solution and the sulfuric acid solution is 9.8-10.3:50-55:66-70.
[0015] 2. Sepiolite Epoxidation
[0016] (1) Activation
[0017] The sepiolite is placed in a muffle furnace for calcination at a temperature of 275-284°C for 35-40 minutes. After the calcination, the temperature is naturally lowered to room temperature, an ethanol solution is added, and after stirring evenly, an activator is added, and the mixture is stirred for 32-38 minutes. After the stirring is completed, the mixture is filtered and dried to obtain the activated sepiolite.
[0018] The sepiolite is β-sepiolite with a particle size of 260-280 nm; the mass content of magnesium oxide in the sepiolite is 23.5-24.0%, and the mass content of silicon dioxide is 57.1-57.5%;
[0019] The mass concentration of the ethanol solution is 35-40%;
[0020] The mass ratio of the sepiolite, the ethanol solution and the activator is 12-14:85-90:1.0-1.2;
[0021] The activator is a mixture of sodium castor oil sulfonate and sodium dodecylaminopropionate, and the mass ratio of the sodium castor oil sulfonate to the sodium dodecylaminopropionate is 1.1-1.3:1.0;
[0022] (2) Epoxidation
[0023] The activated sepiolite is placed in anhydrous ethanol, mixed evenly, and then a silane coupling agent A172 is added for ultrasonic treatment, wherein the ultrasonic time is 13-15 minutes, the ultrasonic power is 134-145 W, and the ultrasonic frequency is 34-38 kHz. After the ultrasonic treatment, the temperature is raised to 68-72° C. for reaction, and the reaction time is 23-25 hours. After the reaction is completed, the reaction is filtered and dried to obtain vinyl-terminated sepiolite. The vinyl-terminated sepiolite is placed in a hydrogen peroxide solution for soaking, and the soaking time is 8.3-8.5 hours, and the soaking temperature is 61-65° C., and the solution is stirred while soaking, and the stirring speed is 134-151 rpm. After the soaking is completed, the solution is filtered, washed, and dried to obtain epoxidized sepiolite.
[0024] The mass ratio of the activated sepiolite, anhydrous ethanol and silane coupling agent A172 is 11.5-12.4:100-112:1.2-1.4;
[0025] The mass concentration of the hydrogen peroxide solution is 25-28%;
[0026] The mass ratio of the vinyl-terminated sepiolite to the hydrogen peroxide solution is 9.8-10.2:42-48.
[0027] 3. Preparation of anti-seepage additives
[0028] The sepiolite is soaked in a hydrofluoric acid solution for 42-48 minutes at a soaking temperature of 36-40°C. After the soaking, the sepiolite is washed and dried to obtain the soaked sepiolite; an ethanol solution is added to the soaked sepiolite, and then hexadecyltrimethylammonium bromide is added, and polyethylene glycol 6000 is added after stirring evenly, and the stirring is continued. After the mixing is evenly performed, the mixture is filtered and dried to obtain a primary anti-seepage water aid; the primary anti-seepage water aid is placed in an isopropanol solution, and perfluorooctanesulfonylaminopropyltrimethoxysilane is added, and the mixture is stirred for 23.5-24.5 hours at a stirring temperature of 27-30°C. After the stirring is completed, the mixture is filtered, washed, and dried to obtain the anti-seepage water aid;
[0029] The sepiolite is β-sepiolite with a particle size of 260-280 nm; the mass content of magnesium oxide in the sepiolite is 23.5-24.0%, and the mass content of silicon dioxide is 57.1-57.5%;
[0030] The mass concentration of the hydrofluoric acid solution is 26-30%;
[0031] The mass ratio of the sepiolite to the hydrofluoric acid solution is 9.6-10.3:62-68;
[0032] The mass ratio of the soaked sepiolite, ethanol solution, hexadecyltrimethylammonium bromide and polyethylene glycol 6000 is 9.0-9.4:82-87:0.6-0.8:0.7-0.9;
[0033] The mass concentration of the ethanol solution is 24-29%;
[0034] The mass ratio of the primary anti-seepage agent, isopropanol solution, and perfluorooctanesulfonylaminopropyltrimethoxysilane is 8.2-8.7:106-114:0.8-1.0;
[0035] The mass concentration of the isopropanol solution is 27-32%.
[0036] 4. Mixing
[0037] Mixing polyethylene terephthalate, carboxylated polyethylene terephthalate, epoxidized sepiolite, and an anti-seepage agent at a mixing speed of 967-995 rpm, and mixing evenly to obtain a mixture;
[0038] The mass ratio of the polyethylene terephthalate, the carboxylated polyethylene terephthalate, the epoxidized sepiolite and the anti-seepage auxiliary agent is 68-72:5.4-5.7:7.3-7.7:2.5-2.9.
[0039] 5. Preparation of polyester grey fabric
[0040] The mixed material is placed in a twin-screw extruder at 266-270° C. for melt extrusion, and then spun through a 48-hole spinneret and cooled to obtain filaments, and the filaments are evenly swung through a swinging plate according to the setting direction to a web laying machine for web laying to form a laid web, and the laid web is subjected to pre-needling and main needling steps to form a polyester grey cloth;
[0041] The polyester grey cloth has a gram weight of 158-162 g / m 2 .
[0042] 6. Post-processing
[0043] The polyester base cloth is hot-rolled and shaped to obtain a polyester base cloth, the thickness of the polyester base cloth is controlled to be 0.8-1.2 mm, the polyester base cloth is immersed in 3.8-4.2 times the mass of corn starch glue for 32-37 seconds, after the immersion is completed, the excess adhesive is squeezed out, and the polyester base cloth is dried to obtain a water-proof polyester tire;
[0044] The preparation method of the corn starch glue is as follows: corn starch is mixed with 9-12 times the mass of deionized water, the mixture is heated to 88-92° C. and stirred for 2.3-2.7 hours, and the corn starch glue is obtained after the stirring is completed.
[0045] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0046] 1. The present invention first performs an activation treatment on sepiolite, wherein the activator can improve the surface activation performance of sepiolite and improve the dispersibility, and then performs epoxidation on the sepiolite. In the epoxidation step, a terminal vinyl silane coupling agent is first used to graft the sepiolite so that one end of the sepiolite is a vinyl group. After being treated with hydrogen peroxide, one end of the sepiolite contains an epoxy group. In the melt extrusion step, the epoxy group of the sepiolite can react with the carboxyl group of polyethylene terephthalate, so that the sepiolite and the polyethylene terephthalate are firmly bonded, and the β-sepiolite is composed of very thin and short fibers or fiber-like The aggregate is composed of a plurality of materials, which has good toughening and strengthening properties for polyethylene terephthalate; then, a specific method is used to treat the sepiolite to prepare an anti-seepage auxiliary agent, firstly, the sepiolite is soaked in hydrofluoric acid, which can etch the sepiolite to a certain extent and change its surface structure, and then the treatment of hexadecyltrimethylammonium bromide and polyethylene glycol is combined to improve the surface activity of the sepiolite, and finally, perfluorooctanesulfonylaminopropyltrimethoxysilane is used for modification to form a stable hydrophobic structure on the surface of the sepiolite. The final product has good stability, high strength, strong toughness, good anti-seepage performance, and still has high mechanical properties after being soaked in water;
[0047] 2. The water-proof polyester tire prepared by the method of the present invention has a transverse tensile force of 718-724N / 50mm, a longitudinal tensile force of 741-746N / 50mm, a transverse elongation of 45.8-46.7%, a longitudinal elongation of 39.4-39.8%, a tear strength of 273-278N, a water absorption rate of 0.5-0.8% after impregnation, a transverse dimensional change rate of 0.47-0.52%, and a longitudinal dimensional change rate of 0.40-0.45%;
[0048] 3. The water-proof polyester tire prepared by the method of the present invention is placed under ultraviolet light with an intensity of 600W / cm 2 The samples were irradiated with ultraviolet light for 24 hours, and then placed at 90°C for 24 hours. The above operation was considered as one cycle. After 5 cycles, the samples were naturally cooled to room temperature and measured again. The transverse tensile force was 696-707N / 50mm, the longitudinal tensile force was 713-722N / 50mm, and the tear strength was 264-272N. DETAILED DESCRIPTION
[0049] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.
[0050] Example 1
[0051] 1. Preparation of carboxylated polyethylene terephthalate
[0052] 10g of polyethylene terephthalate was soaked in 53g of isopropanol solution for 50min, taken out after soaking, and then soaked in 68g of sulfuric acid solution for 25min, washed after soaking, and dried at 63°C to obtain carboxylated polyethylene terephthalate;
[0053] The mass concentration of the isopropanol solution is 47%;
[0054] The mass concentration of the sulfuric acid solution is 18%.
[0055] 2. Sepiolite Epoxidation
[0056] (1) Activation
[0057] 13g of sepiolite was placed in a muffle furnace for calcination at a temperature of 280°C for 37 minutes. After the calcination, the temperature was naturally lowered to room temperature, 87g of ethanol solution was added, and after stirring evenly, 1.1g of activator was added and stirred for 35 minutes. After the stirring was completed, the activated sepiolite was obtained by filtering and drying.
[0058] The sepiolite is β-sepiolite with a particle size of 270 nm; the mass content of magnesium oxide in the sepiolite is 23.8%, and the mass content of silicon dioxide is 57.3%;
[0059] The mass concentration of the ethanol solution is 37%;
[0060] The activator is a mixture of sodium castor oil sulfonate and sodium dodecylaminopropionate, and the mass ratio of the sodium castor oil sulfonate to the sodium dodecylaminopropionate is 1.2:1.0;
[0061] (2) Epoxidation
[0062] 12g of activated sepiolite was placed in 105g of anhydrous ethanol, and 1.3g of silane coupling agent A172 was added after mixing evenly, and ultrasonic treatment was performed. The ultrasonic time was 14min, the ultrasonic power was 140W, and the ultrasonic frequency was 36kHz. After the ultrasonic treatment, the temperature was raised to 70°C for reaction. The reaction time was 24h. After the reaction was completed, the reaction was filtered and dried to obtain vinyl-terminated sepiolite. 10g of vinyl-terminated sepiolite was placed in 45g of hydrogen peroxide solution for soaking. The soaking time was 8.4h and the soaking temperature was 63°C. Stirring was performed while soaking. The stirring speed was 142rpm. After the soaking was completed, filtering, washing, and drying were performed to obtain epoxidized sepiolite.
[0063] The mass concentration of the hydrogen peroxide solution is 26%.
[0064] 3. Preparation of anti-seepage additives
[0065] 10g of sepiolite is soaked in 65g of hydrofluoric acid solution for 45min at a temperature of 38°C. After the soaking, it is washed and dried to obtain the soaked sepiolite; 85g of ethanol solution is added to 9.2g of the soaked sepiolite, and then 0.7g of hexadecyltrimethylammonium bromide is added. After stirring, 0.8g of polyethylene glycol 6000 is added, and the stirring is continued. After mixing, the mixture is filtered and dried to obtain a primary anti-seepage water aid; 8.5g of the primary anti-seepage water aid is placed in 110g of isopropanol solution, 0.9g of perfluorooctanesulfonylaminopropyltrimethoxysilane is added, and the mixture is stirred for 24h at a temperature of 28°C. After the stirring is completed, the mixture is filtered, washed and dried to obtain an anti-seepage water aid;
[0066] The sepiolite is β-sepiolite with a particle size of 270 nm; the mass content of magnesium oxide in the sepiolite is 23.8%, and the mass content of silicon dioxide is 57.3%;
[0067] The mass concentration of the hydrofluoric acid solution is 28%;
[0068] The mass concentration of the ethanol solution is 27%;
[0069] The mass concentration of the isopropanol solution is 30%.
[0070] 4. Mixing
[0071] 70 g of polyethylene terephthalate, 5.6 g of carboxylated polyethylene terephthalate, 7.5 g of epoxidized sepiolite, and 2.7 g of an anti-seepage agent were mixed at a mixing speed of 980 rpm. After mixing evenly, a mixture was obtained.
[0072] 5. Preparation of polyester grey fabric
[0073] The mixed material is placed in a twin-screw extruder at 268° C. for melt extrusion, and then spun through a 48-hole spinneret and cooled to obtain filaments, and the filaments are evenly swung through a swinging plate according to the setting direction to a web laying machine for web laying to form a laid web, and the laid web is subjected to pre-needling and main needling steps to form a polyester grey fabric;
[0074] The polyester grey cloth has a gram weight of 160 g / m 2 .
[0075] 6. Post-processing
[0076] The polyester base cloth is hot-rolled and shaped to obtain a polyester base cloth, the thickness of the polyester base cloth is controlled to be 1.0 mm, and the polyester base cloth is immersed in 4 times the mass of corn starch glue for 35 seconds. After the immersion, the excess adhesive is squeezed out and dried to obtain a water-proof polyester tire;
[0077] The preparation method of the corn starch glue is as follows: corn starch is mixed with deionized water of 10 times the mass, the mixture is heated to 90° C. and stirred for 2.5 hours, and the corn starch glue is obtained after the stirring is completed.
[0078] Example 2
[0079] 1. Preparation of carboxylated polyethylene terephthalate
[0080] 9.8 g of polyethylene terephthalate was immersed in 50 g of isopropanol solution for 48 min, taken out after immersion, and then immersed in 66 g of sulfuric acid solution for 24 min, washed after immersion, and dried at 62° C. to obtain carboxylated polyethylene terephthalate;
[0081] The mass concentration of the isopropanol solution is 45%;
[0082] The mass concentration of the sulfuric acid solution is 16%.
[0083] 2. Sepiolite Epoxidation
[0084] (1) Activation
[0085] 12g of sepiolite was placed in a muffle furnace for calcination at a temperature of 275°C for 35 minutes. After the calcination, the temperature was naturally lowered to room temperature, 85g of ethanol solution was added, and after stirring evenly, 1.0g of activator was added and stirred for 32 minutes. After the stirring was completed, the activated sepiolite was obtained by filtering and drying.
[0086] The sepiolite is β-sepiolite with a particle size of 260 nm; in the sepiolite, the mass content of magnesium oxide is 23.5%, and the mass content of silicon dioxide is 57.1%;
[0087] The mass concentration of the ethanol solution is 35%;
[0088] The activator is a mixture of sodium castor oil sulfonate and sodium dodecylaminopropionate, and the mass ratio of the sodium castor oil sulfonate to the sodium dodecylaminopropionate is 1.1:1.0;
[0089] (2) Epoxidation
[0090] 11.5 g of activated sepiolite was placed in 100 g of anhydrous ethanol, and after being mixed evenly, 1.2 g of silane coupling agent A172 was added, and ultrasonic treatment was performed. The ultrasonic time was 13 min, the ultrasonic power was 134 W, and the ultrasonic frequency was 34 kHz. After the ultrasonic treatment, the temperature was raised to 68° C. for reaction. The reaction time was 23 h. After the reaction was completed, the reaction was filtered and dried to obtain vinyl-terminated sepiolite. 9.8 g of vinyl-terminated sepiolite was placed in 42 g of hydrogen peroxide solution for soaking. The soaking time was 8.3 h. The soaking temperature was 61° C., and the mixture was stirred while soaking. The stirring speed was 134 rpm. After the soaking was completed, the mixture was filtered, washed, and dried to obtain epoxidized sepiolite.
[0091] The mass concentration of the hydrogen peroxide solution is 25%.
[0092] 3. Preparation of anti-seepage additives
[0093] 9.6 g of sepiolite was immersed in 62 g of hydrofluoric acid solution for 42 min at a temperature of 36° C. After the immersion, the sepiolite was washed and dried to obtain the immersed sepiolite; 82 g of ethanol solution was added to 9.0 g of the immersed sepiolite, and then 0.6 g of hexadecyltrimethylammonium bromide was added, and after stirring, 0.7 g of polyethylene glycol 6000 was added, and the stirring was continued. After the stirring was uniform, the mixture was filtered and dried to obtain a primary anti-seepage water aid; 8.2 g of the primary anti-seepage water aid was placed in 106 g of isopropanol solution, 0.8 g of perfluorooctanesulfonylaminopropyltrimethoxysilane was added, and the mixture was stirred for 23.5 h at a temperature of 27° C. After the stirring was completed, the mixture was filtered, washed and dried to obtain a anti-seepage water aid;
[0094] The sepiolite is β-sepiolite with a particle size of 260 nm; in the sepiolite, the mass content of magnesium oxide is 23.5%, and the mass content of silicon dioxide is 57.1%;
[0095] The mass concentration of the hydrofluoric acid solution is 26%;
[0096] The mass concentration of the ethanol solution is 24%;
[0097] The mass concentration of the isopropanol solution is 27%.
[0098] 4. Mixing
[0099] 68 g of polyethylene terephthalate, 5.4 g of carboxylated polyethylene terephthalate, 7.3 g of epoxidized sepiolite, and 2.5 g of an anti-seepage agent were mixed at a mixing speed of 967 rpm. After mixing evenly, a mixture was obtained.
[0100] 5. Preparation of polyester grey fabric
[0101] The mixed material is placed in a twin-screw extruder at 266° C. for melt extrusion, and then spun through a 48-hole spinneret and cooled to obtain filaments, and the filaments are evenly swung through a swinging plate according to the setting direction to a web laying machine for web laying to form a laid web, and the laid web is subjected to pre-needling and main needling steps to form a polyester grey fabric;
[0102] The polyester grey cloth has a gram weight of 158 g / m 2 .
[0103] 6. Post-processing
[0104] The polyester base cloth is hot-rolled and shaped to obtain a polyester base cloth, the thickness of the polyester base cloth is controlled to be 0.8 mm, and the polyester base cloth is impregnated in 3.8 times the mass of corn starch glue for 32 seconds. After the impregnation, the excess adhesive is squeezed out and dried to obtain a water-proof polyester tire.
[0105] The preparation method of the corn starch glue is as follows: corn starch is mixed with 9 times the mass of deionized water, the mixture is heated to 88° C. and stirred for 2.3 hours, and the corn starch glue is obtained after the stirring is completed.
[0106] Example 3
[0107] 1. Preparation of carboxylated polyethylene terephthalate
[0108] 10.3 g of polyethylene terephthalate was immersed in 55 g of isopropanol solution for 52 min, taken out after immersion, and then immersed in 70 g of sulfuric acid solution for 26 min, washed after immersion, and dried at 64° C. to obtain carboxylated polyethylene terephthalate;
[0109] The mass concentration of the isopropanol solution is 49%;
[0110] The mass concentration of the sulfuric acid solution is 20%.
[0111] 2. Sepiolite Epoxidation
[0112] (1) Activation
[0113] 14 g of sepiolite was placed in a muffle furnace for calcination at a temperature of 284° C. for 40 min. After calcination, the temperature was naturally lowered to room temperature, 90 g of ethanol solution was added, and after stirring evenly, 1.2 g of activator was added, and stirred for 38 min. After stirring, the mixture was filtered and dried to obtain activated sepiolite.
[0114] The sepiolite is β-sepiolite with a particle size of 280 nm; the mass content of magnesium oxide in the sepiolite is 24.0%, and the mass content of silicon dioxide is 57.5%;
[0115] The mass concentration of the ethanol solution is 40%;
[0116] The activator is a mixture of sodium castor oil sulfonate and sodium dodecylaminopropionate, and the mass ratio of the sodium castor oil sulfonate to the sodium dodecylaminopropionate is 1.3:1.0;
[0117] (2) Epoxidation
[0118] 12.4 g of activated sepiolite was placed in 112 g of anhydrous ethanol, and after being mixed evenly, 1.4 g of silane coupling agent A172 was added, and ultrasonic treatment was performed. The ultrasonic time was 15 min, the ultrasonic power was 145 W, and the ultrasonic frequency was 38 kHz. After the ultrasonic treatment, the temperature was raised to 72° C. for reaction. The reaction time was 25 h. After the reaction was completed, the reaction was filtered and dried to obtain vinyl-terminated sepiolite. 10.2 g of vinyl-terminated sepiolite was placed in 48 g of hydrogen peroxide solution for soaking. The soaking time was 8.5 h. The soaking temperature was 65° C. The mixture was stirred while soaking. The stirring speed was 151 rpm. After the soaking was completed, the mixture was filtered, washed, and dried to obtain epoxidized sepiolite.
[0119] The mass concentration of the hydrogen peroxide solution is 28%.
[0120] 3. Preparation of anti-seepage additives
[0121] 10.3g of sepiolite was soaked in 68g of hydrofluoric acid solution for 48min at a temperature of 40°C. After the soaking, the sepiolite was washed and dried to obtain the soaked sepiolite; 87g of ethanol solution was added to 9.4g of the soaked sepiolite, and then 0.8g of hexadecyltrimethylammonium bromide was added. After stirring, 0.9g of polyethylene glycol 6000 was added, and the stirring was continued. After mixing, the mixture was filtered and dried to obtain a primary anti-seepage water aid; 8.7g of the primary anti-seepage water aid was placed in 114g of isopropanol solution, 1.0g of perfluorooctanesulfonylaminopropyltrimethoxysilane was added, and the mixture was stirred for 24.5h at a temperature of 30°C. After the stirring was completed, the mixture was filtered, washed and dried to obtain an anti-seepage water aid;
[0122] The sepiolite is β-sepiolite with a particle size of 280 nm; the mass content of magnesium oxide in the sepiolite is 24.0%, and the mass content of silicon dioxide is 57.5%;
[0123] The mass concentration of the hydrofluoric acid solution is 30%;
[0124] The mass concentration of the ethanol solution is 29%;
[0125] The mass concentration of the isopropanol solution is 32%.
[0126] 4. Mixing
[0127] 72 g of polyethylene terephthalate, 5.7 g of carboxylated polyethylene terephthalate, 7.7 g of epoxidized sepiolite, and 2.9 g of an anti-seepage agent were mixed at a mixing speed of 995 rpm. After mixing evenly, a mixture was obtained.
[0128] 5. Preparation of polyester grey fabric
[0129] The mixed material is placed in a twin-screw extruder at 270° C. for melt extrusion, and then spun through a 48-hole spinneret and cooled to obtain filaments, and the filaments are evenly swung through a swinging plate according to the setting direction to a web laying machine for web laying to form a laid web, and the laid web is subjected to pre-needling and main needling steps to form a polyester grey fabric;
[0130] The polyester grey cloth has a gram weight of 162 g / m 2 .
[0131] 6. Post-processing
[0132] The polyester base cloth is hot-rolled and shaped to obtain a polyester base cloth, the thickness of the polyester base cloth is controlled to be 1.2 mm, and the polyester base cloth is immersed in 4.2 times the mass of corn starch glue for 37 seconds. After the immersion is completed, the excess adhesive is squeezed out and dried to obtain a water-proof polyester tire;
[0133] The preparation method of the corn starch glue is as follows: corn starch is mixed with 12 times the mass of deionized water, the mixture is heated to 92° C. and stirred for 2.7 hours, and the corn starch glue is obtained after the stirring is completed.
[0134] Comparative Example 1
[0135] Based on Example 1, the changes are as follows:
[0136] (1) The step of preparing carboxylated polyethylene terephthalate is omitted; in the mixing step, an equal amount of polyethylene terephthalate is replaced by carboxylated polyethylene terephthalate;
[0137] (2) in the epoxidation step of sepiolite, the epoxidation step is omitted; in the mixing step, the epoxidized sepiolite in the epoxidation step is replaced by an equal amount of activated sepiolite;
[0138] The rest of the operations are the same.
[0139] Comparative Example 2
[0140] Based on Example 1, the changes are as follows:
[0141] (1) In the epoxidation step of sepiolite, the activation step is omitted; in the epoxidation step, the activated sepiolite is replaced by an equal amount of sepiolite without any treatment; the sepiolite is β-sepiolite with a particle size of 270 nm; the mass content of magnesium oxide in the sepiolite is 23.8%, and the mass content of silicon dioxide is 57.3%;
[0142] (2) The preparation method of the anti-seepage auxiliary agent is as follows: 10g of sepiolite is immersed in 65g of hydrofluoric acid solution for 45min at a temperature of 38°C. After the immersion, the sepiolite is washed and dried to obtain the immersed sepiolite; the sepiolite is β-sepiolite with a particle size of 270nm; the mass content of magnesium oxide in the sepiolite is 23.8%, and the mass content of silicon dioxide is 57.3%; the mass concentration of the hydrofluoric acid solution is 28%;
[0143] In the mixing step, an equal amount of the water-proofing agent is replaced with soaked sepiolite;
[0144] The rest of the operations are the same.
[0145] Performance Testing
[0146] 1. Mechanical properties
[0147] The products obtained in Examples 1-3 and Comparative Examples 1-2 were tested for mechanical properties, water absorption after immersion, and thermal stability. The test results are as follows:
[0148]
[0149] 2. Aging resistance
[0150] The products obtained in Examples 1-3 and Comparative Examples 1-2 were placed under ultraviolet light with an intensity of 600 W / cm 2 The samples were irradiated with ultraviolet light for 24 hours, and then placed at 90°C for 24 hours. The above operation was considered as one cycle. After 5 cycles, the samples were naturally cooled to room temperature and the mechanical properties were tested again. The test results are as follows:
[0151]
[0152] The invention first performs activation treatment on sepiolite, wherein the activator can improve the surface activation performance of sepiolite and improve the dispersibility, and then performs epoxidation on the sepiolite. In the epoxidation step, the sepiolite is first grafted with a terminal vinyl silane coupling agent so that one end of the sepiolite is a vinyl group. After being treated with hydrogen peroxide, one end of the sepiolite contains an epoxy group. In the melt extrusion step, the epoxy group of the sepiolite can react with the carboxyl group of polyethylene terephthalate, so that the sepiolite and the polyethylene terephthalate are firmly combined. In addition, the β-sepiolite is composed of very thin and short fibers or fiber-like aggregates. The composite composition has good toughening and strengthening properties for polyethylene terephthalate; then, a specific method is used to treat the sepiolite to prepare an anti-seepage agent, firstly, the sepiolite is soaked in hydrofluoric acid, which can etch the sepiolite to a certain extent and change its surface structure, and then the treatment with hexadecyltrimethylammonium bromide and polyethylene glycol is combined to improve the surface activity of the sepiolite, and finally, perfluorooctanesulfonylaminopropyltrimethoxysilane is used for modification to form a stable hydrophobic structure on the surface of the sepiolite. The final product has high strength, strong toughness, good anti-seepage performance, good stability, and still has high mechanical properties after thermal aging.
[0153] In Comparative Example 1, the step of preparing carboxylated polyethylene terephthalate is omitted, and in the step of epoxidation of sepiolite, the epoxidation step is omitted. The polyethylene terephthalate in Comparative Example 1 cannot be cross-linked with sepiolite, sepiolite has poor compatibility with polyethylene terephthalate, poor dispersibility, and the composition of the obtained product is uneven and the properties are unstable, thereby reducing the mechanical properties and aging resistance of the product.
[0154] In the epoxidation step of sepiolite in Comparative Example 2, the activation step was omitted. In the epoxidation step, the sepiolite had serious aggregation phenomenon, poor dispersibility, and insufficient epoxidation, which resulted in unstable bonding with polyethylene terephthalate. In addition, the anti-seepage auxiliary agent of Comparative Example 2 was only the soaked sepiolite, which had poor hydrophobicity and poor anti-seepage property, which resulted in high water absorption rate, uneven mechanical properties, and poor stability of the obtained product.
[0155] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.
[0156] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a water-proof polyester tire, characterized in that: The preparation method comprises the steps of preparing carboxylated polyethylene terephthalate, epoxidizing sepiolite, preparing an anti-seepage aid, mixing materials, preparing polyester grey cloth, and post-processing; The steps of preparing carboxylated polyethylene terephthalate are as follows: immersing polyethylene terephthalate in an isopropanol solution for 48-52 minutes, taking it out after immersion, and then immersing it in a sulfuric acid solution for 24-26 minutes, washing it after immersion, and drying it at 62-64° C. to obtain carboxylated polyethylene terephthalate; The mass concentration of the sulfuric acid solution is 16-20%; The sepiolite epoxidation comprises activation and epoxidation steps; The activation step comprises placing the sepiolite in a muffle furnace for calcination, naturally cooling the temperature to room temperature after the calcination, adding an ethanol solution, stirring evenly, adding an activator, stirring for 32-38 minutes, filtering and drying after the stirring is completed, and obtaining the activated sepiolite; The activator is a mixture of sodium castor oil sulfonate and sodium dodecylaminopropionate; The epoxidation step comprises placing the activated sepiolite in anhydrous ethanol, mixing evenly, adding silane coupling agent A172, performing ultrasonic treatment, heating to 68-72° C. for reaction after the ultrasonic treatment, and the reaction time is 23-25 hours. After the reaction is completed, filtering and drying are performed to obtain vinyl-terminated sepiolite; placing the vinyl-terminated sepiolite in a hydrogen peroxide solution for soaking, the soaking time is 8.3-8.5 hours, the soaking temperature is 61-65° C., stirring is performed while soaking, and the stirring speed is 134-151 rpm. After the soaking is completed, filtering, washing, and drying are performed to obtain epoxidized sepiolite; The steps of preparing the anti-seepage auxiliary agent are as follows: soaking sepiolite in a hydrofluoric acid solution for 42-48 minutes at a temperature of 36-40°C, washing and drying after soaking to obtain the soaked sepiolite; adding an ethanol solution to the soaked sepiolite, then adding hexadecyltrimethylammonium bromide, stirring evenly, adding polyethylene glycol 6000, continuing to stir, mixing evenly, filtering and drying to obtain a primary anti-seepage auxiliary agent; placing the primary anti-seepage auxiliary agent in an isopropanol solution, adding perfluorooctanesulfonylaminopropyltrimethoxysilane, stirring for 23.5-24.5 hours at a temperature of 27-30°C, filtering, washing and drying after stirring to obtain the anti-seepage auxiliary agent.
2. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: In the step of preparing carboxylated polyethylene terephthalate, the mass concentration of the isopropanol solution is 45-49%; The mass ratio of the polyethylene terephthalate, the isopropanol solution and the sulfuric acid solution is 9.8-10.3:50-55:66-70.
3. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: In the activation step, the calcination temperature is 275-284°C and the calcination time is 35-40min; The sepiolite is β-sepiolite with a particle size of 260-280 nm; the mass content of magnesium oxide in the sepiolite is 23.5-24.0%, and the mass content of silicon dioxide is 57.1-57.5%; The mass concentration of the ethanol solution is 35-40%; The mass ratio of the sepiolite, the ethanol solution and the activator is 12-14:85-90:1.0-1.2; In the activator, the mass ratio of the sodium castor oil sulfonate to sodium dodecylaminopropionate is 1.1-1.3:1.
0.
4. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: In the epoxidation step, the ultrasonic treatment has an ultrasonic time of 13-15 min, an ultrasonic power of 134-145 W, and an ultrasonic frequency of 34-38 kHz; The mass ratio of the activated sepiolite, anhydrous ethanol and silane coupling agent A172 is 11.5-12.4:100-112:1.2-1.4; The mass concentration of the hydrogen peroxide solution is 25-28%; The mass ratio of the vinyl-terminated sepiolite to the hydrogen peroxide solution is 9.8-10.2:42-48.
5. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: In the step of preparing the anti-seepage auxiliary agent, the sepiolite is β-sepiolite with a particle size of 260-280 nm; the mass content of magnesium oxide in the sepiolite is 23.5-24.0%, and the mass content of silicon dioxide is 57.1-57.5%; The mass concentration of the hydrofluoric acid solution is 26-30%; The mass ratio of the sepiolite to the hydrofluoric acid solution is 9.6-10.3:62-68; The mass ratio of the soaked sepiolite, ethanol solution, hexadecyltrimethylammonium bromide and polyethylene glycol 6000 is 9.0-9.4:82-87:0.6-0.8:0.7-0.9; The mass concentration of the ethanol solution is 24-29%; The mass ratio of the primary anti-seepage agent, isopropanol solution, and perfluorooctanesulfonylaminopropyltrimethoxysilane is 8.2-8.7:106-114:0.8-1.0; The mass concentration of the isopropanol solution is 27-32%.
6. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: The mixing step comprises mixing polyethylene terephthalate, carboxylated polyethylene terephthalate, epoxidized sepiolite, and an anti-seepage additive at a mixing speed of 967-995 rpm, and after mixing evenly, obtaining a mixture; The mass ratio of the polyethylene terephthalate, the carboxylated polyethylene terephthalate, the epoxidized sepiolite and the anti-seepage auxiliary agent is 68-72:5.4-5.7:7.3-7.7:2.5-2.
9.
7. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: The step of preparing the polyester grey cloth comprises placing the mixed material in a twin-screw extruder at 266-270° C. for melt extrusion, spinning the mixed material through a 48-hole spinneret, cooling the mixed material to obtain filaments, evenly swinging the filaments through a swinging plate according to its setting direction to a web laying machine for web laying to form a laid web, and subjecting the laid web to pre-needling and main needling steps to form the polyester grey cloth; The polyester grey cloth has a gram weight of 158-162 g / m 2 .
8. The method for preparing a water-proof polyester tire according to claim 1, characterized in that: The post-processing steps are: hot rolling and shaping the polyester grey cloth to obtain the polyester base cloth, controlling the thickness of the polyester base cloth to be 0.8-1.2 mm, dipping the polyester base cloth in 3.8-4.2 times the mass of corn starch glue for 32-37 seconds, squeezing out excess adhesive after dipping, and drying to obtain the waterproof polyester tire.
9. The method for preparing a water-proof polyester tire according to claim 8, characterized in that: The preparation method of the corn starch glue is as follows: corn starch is mixed with 9-12 times the mass of deionized water, the mixture is heated to 88-92° C. and stirred for 2.3-2.7 hours, and the corn starch glue is obtained after the stirring is completed.