Method for determining element content using energy dispersive X-ray spectrometry
Through the combination of energy dispersion X-ray spectrometer and inductively coupled plasma generation spectrometer, a correction method was established, which solved the problem of accuracy and efficiency in the determination of element content of the positive electrode material of lithium batteries, and achieved rapid and accurate element content measurement to meet the lithium battery industry demand.
Patent Information
- Application Number
- CN202411062941.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing methods for determining the element content of the cathode material of lithium batteries, including traditional chemical analysis and instrument analysis methods, are complicated to operate, long time, or have poor test accuracy and precision, making it difficult to meet the rapid development needs of the lithium battery industry.
Using energy dispersion X-ray spectrometer (EDX) combined with inductively coupled plasma generation spectrometer (ICP-OES), the average response value of multiple standard samples is obtained, and the calibration method is established, and the EDX measurement results are corrected, so as to accurately measure the elements in the sample to be tested. content.
It significantly improves testing efficiency, reduces experimental operation burden, provides higher accuracy and precision, and the results match the industry's general ICP-OES measurement results and meet industry standards.
Smart Images

Figure CN118671116B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery material detection, and in particular to a method for determining element content using an energy dispersive X-ray spectrometer. Background Art
[0002] In the current energy storage field, lithium batteries have become one of the most widely used energy storage media due to their advantages such as high energy density, long life and stability, and the market demand is huge. The production of lithium-ion batteries depends on a variety of raw materials, among which the quality of the positive electrode material directly affects the performance and quality of the battery. The content of elements in the positive electrode material, such as nickel, cobalt, manganese, etc., is one of the key factors that determine the performance of the battery. Therefore, accurately determining the content of these elements in the positive electrode material is of vital importance to ensure the quality of lithium battery products.
[0003] At present, the methods used to determine the element content in positive electrode materials mainly include traditional chemical analysis methods and instrumental analysis methods. Traditional chemical analysis methods, such as using EDTA to titrate the total metal content, and then determining the content of specific elements by precipitation method and redox method respectively, are cumbersome to operate and take a long time to analyze, which is difficult to meet the needs of the rapidly developing lithium battery industry. Instrumental analysis methods, such as inductively coupled plasma spectrometer analysis, can shorten the analysis time, but due to the large dilution factor and the sensitivity of the instrument to environmental conditions, its test accuracy and precision are poor, which limits its widespread application in the lithium battery manufacturing industry. Summary of the invention
[0004] In view of this, the present application provides a method for determining element content using an energy dispersive X-ray spectrometer to solve the above technical problems.
[0005] A method for determining element content using an energy dispersive X-ray spectrometer comprises the following steps: obtaining a first average response value of an element to be measured in a plurality of standard samples by means of an energy dispersive X-ray spectrometer, and obtaining a second average response value of the element to be measured in the plurality of standard samples by means of an inductively coupled plasma spectrometer; obtaining a calibration method of the energy dispersive X-ray spectrometer according to the first average response value and the second average response value; obtaining a first actual response value of the element to be measured in the sample to be measured by means of the energy dispersive X-ray spectrometer, and calibrating the first actual response value according to the calibration method to obtain the content value of the element to be measured in the sample to be measured.
[0006] In some possible embodiments, the step of "obtaining a first average response value of the element to be measured in multiple standard samples by an energy dispersive X-ray spectrometer" includes: providing multiple standard samples, each standard sample having a different content of the element to be measured; for each standard sample, obtaining multiple first response values of the element to be measured therein by multiple measurements by an energy dispersive X-ray spectrometer, and averaging the multiple first response values to obtain a first average response value.
[0007] In some possible embodiments, the step of "obtaining a second average response value of the element to be measured in multiple standard samples by using an inductively coupled plasma spectrometer" includes: providing multiple standard samples, each standard sample having a different content of the element to be measured; performing multiple measurements on each standard sample by using an inductively coupled plasma spectrometer to obtain multiple second response values of the element to be measured, and averaging the multiple second response values to obtain a second average response value.
[0008] In some possible implementations, the content of the element to be measured in the sample to be measured is within a preset range, and the preset range is defined by the maximum content and the minimum content of the element to be measured in a plurality of standard samples.
[0009] In some possible implementations, the number of multiple measurements is 2-10 times.
[0010] In some possible embodiments, the step of "obtaining a correction method for an energy dispersive X-ray spectrometer based on the first average response value and the second average response value" includes: taking the first average response value as an independent variable and the second average response value as a dependent variable, performing linear fitting on the first average response value and the second average response value to obtain a linear regression equation.
[0011] In some possible implementations, the step of “correcting the first actual response value according to the correction method” includes: substituting the first actual response value into the independent variable side of the linear regression equation, and using the calculation result as the content value of the element to be measured.
[0012] In some possible implementations, the method further includes the steps of: obtaining a second actual response value of the element to be measured in the sample to be measured as a verification value by using an inductively coupled plasma spectrometer; and evaluating the accuracy of the content value using the verification value.
[0013] In some possible implementations, the number of standard samples is 3-8.
[0014] In some possible embodiments, the standard sample and the sample to be tested are both nickel-cobalt-manganese ternary positive electrode materials, and the element to be tested is nickel, cobalt or manganese; or, the standard sample and the sample to be tested are both lithium manganese iron phosphate positive electrode materials, and the element to be tested is iron or manganese.
[0015] The present application provides a method for determining the content of an element using an energy dispersive X-ray spectrometer, which obtains a first average response value of an element to be measured in a plurality of standard samples by an energy dispersive X-ray spectrometer, and obtains a second average response value of an element to be measured in a plurality of standard samples by an inductively coupled plasma spectrometer. A calibration method for the energy dispersive X-ray spectrometer is obtained based on the first average response value and the second average response value. A first actual response value of the element to be measured in the sample to be measured is obtained by the energy dispersive X-ray spectrometer, and the first actual response value is calibrated based on the calibration method to obtain the content value of the element to be measured in the sample to be measured. Compared with the complex sample pretreatment and long test cycle required by the inductively coupled plasma spectrometer, the energy dispersive X-ray spectrometer can provide faster analysis results, significantly improve the test efficiency and reduce the burden of experimental operations. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 FIG. 1 is a flow chart of an embodiment of a method for determining element content using an energy dispersive X-ray spectrometer according to the present application. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0019] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0020] In this application, Energy-Dispersive X-ray Spectroscopy (EDX) is an important tool for elemental analysis of material surfaces, often used in conjunction with scanning electron microscopes (SEM) or transmission electron microscopes (TEM) to obtain elemental composition and chemical information of samples. Energy-dispersive X-ray spectrometers can quickly and non-destructively perform qualitative and quantitative analysis on samples.
[0021] In this application, Inductively Coupled PlasmaOptical Emission Spectrometry (ICP-OES) is an analytical technique for measuring element concentrations. It is particularly suitable for rapid analysis of multiple elements and simultaneous quantification, and can handle almost all types of aqueous solution samples. It is widely used in environmental monitoring, food safety, pharmaceutical analysis, geological research and other fields. ICP-OES requires pretreatment of the sample to be tested, such as digestion, dilution, etc. At the same time, the test results of ICP-OES are easily affected by the external environment.
[0022] See also Figure 1 , Figure 1 This is a schematic flow chart of an embodiment of a method for determining element content using an energy dispersive X-ray spectrometer provided in the present application. The method includes the following steps S11-S13.
[0023] S11, obtaining a first average response value of the element to be measured in a plurality of standard samples by EDX, and obtaining a second average response value of the element to be measured in a plurality of standard samples by ICP-OES.
[0024] For lithium battery positive electrode materials, the current standard practice is to use ICP-OES to determine the element content. Although EDX can be used for quantitative analysis of elements, due to the lack of standard samples suitable for EDX, it cannot match the ICP-OES measurement results commonly used in the industry, and the test accuracy cannot be guaranteed.
[0025] The present application proposes a method for using EDX to determine the element content in the positive electrode material, and the determination result can match the ICP-OES determination result commonly used in the industry. First, it is necessary to analyze the content of the specified elements to be measured by EDX and ICP-OES for multiple standard samples respectively. The multiple standard samples are prepared according to the sample preparation standard GBT22554-2010 applicable to ICP-OES, and there can be multiple elements to be measured. Both EDX and ICP-OES can obtain the content of multiple elements at the same time in one measurement. EDX is directly used to detect multiple standard samples to obtain the content of the elements to be measured (such as cobalt, manganese, and nickel), that is, the first average response value F. At the same time, ICP-OES is used to analyze the element content of the above multiple standard samples to obtain the second average response value C of the same elements to be measured in these multiple standard samples.
[0026] S12, establishing an EDX calibration method according to the first average response value and the second average response value.
[0027] After obtaining the content of the element to be measured in the standard sample, i.e., the first average response value and the second average response value, respectively, by EDX and ICP-OES, the EDX calibration method is established by the multiple first average response values and the multiple second average response values, so as to facilitate the subsequent matching of the EDX measurement results corresponding to the sample to be measured with the ICP-OES. For example, the distribution curves of the two can be drawn to obtain the point-to-point deviation value, and then averaged, or linear regression can be performed.
[0028] S13, obtaining a first actual response value of the element to be measured in the sample to be measured by EDX, and correcting the first actual response value according to a correction method to obtain a content value of the element to be measured in the sample to be measured.
[0029] Furthermore, the element content of the sample to be tested is analyzed by EDX to obtain the first actual response value of the element to be tested, and then the correction method is used to correct it, and the corrected result is used as the content value of the element to be tested in the sample to be tested. The content value at this time matches the ICP-OES measurement result commonly used in the industry standard, which is equivalent to using the correction method to simply convert the EDX measurement result to replace the ICP-OES measurement result, and the correction method can be implanted in the EDX processor and corrected in the background, so as to directly obtain the content value of the element to be tested in the sample to be tested.
[0030] The method of using EDX to determine the element content in the positive electrode material provided in this embodiment can directly obtain the detection results that match the general ICP-OES in the industry, and conform to the industry standards. In terms of detection method, compared with ICP-OES, EDX can directly detect powdered positive electrode materials without the need for pre-treatment processes such as heating digestion and dilution. The test time is shorter, the test process is more stable, the test results are more accurate, and it is non-destructive to the sample.
[0031] In some embodiments, the “obtaining a first average response value of the element to be measured in a plurality of standard samples by EDX” in the above step S11 specifically includes the following steps S21-S22.
[0032] S21, providing a plurality of standard samples, each of which has a different content of the element to be measured.
[0033] The multiple standard samples are lithium battery positive electrode materials, prepared according to the standard GBT22554-2010. The content of the element to be tested in each standard sample is different. The content of the element to be tested in the sample to be tested is within a preset range, which is defined by the maximum and minimum contents of the element to be tested in the multiple standard samples. When preparing standard samples, standard samples with the widest possible coverage of the content of the element to be tested can be selected to make more applicable samples to be tested.
[0034] For example, a lithium battery ternary positive electrode material is selected to prepare multiple standard samples, and the elements to be tested include cobalt, manganese and nickel. Among them, the mass of cobalt accounts for 2%~23% of the total mass of the standard sample, the mass of manganese accounts for 12%~20% of the total mass of the standard sample, and the mass of nickel accounts for 20%~47% of the total mass of the standard sample, and the content of the elements to be tested in each standard sample is different. For example, a lithium manganese iron phosphate positive electrode material is selected to prepare multiple standard samples, and the elements to be tested include manganese and iron. The mass of manganese accounts for 13%~22% of the total mass of the standard sample, and the mass of iron accounts for 13%~22% of the total mass of the standard sample, and the content of the elements to be tested in each standard sample is different.
[0035] S22, for each standard sample, performing multiple EDX measurements to obtain multiple first response values of the element to be measured therein, and averaging the multiple first response values to obtain a first average response value.
[0036] After preparing multiple standard samples, for each standard sample, multiple first response values of the elements to be measured are obtained by EDX time-sharing multiple times, and the multiple first response values are averaged to obtain a first average response value, and the number of multiple measurements is 2-10 times. For example, for multiple standard samples prepared from the above-mentioned ternary positive electrode material, each standard sample is measured multiple times by EDX time-sharing, and each measurement can obtain a first response value of the elements cobalt, manganese and nickel to be measured. After all the measurements are completed, the multiple first response values are averaged to obtain the first average response values of the elements cobalt, manganese and nickel to be measured.
[0037] By measuring each element to be measured multiple times at different times and then taking the average value as the first average response value, the random error and uncertainty in a single measurement can be reduced. For example, there may be a situation where a certain measurement is interfered by the outside world or the instrument is unstable for a moment. Multiple measurements and averaging can effectively reduce the influence of these accidental factors, so that the measurement results are closer to the true value and the accuracy of the measurement is improved.
[0038] In some embodiments, the “obtaining a second average response value of the element to be measured in multiple standard samples by ICP-OES” in the above step S11 specifically includes the following steps S31-S32.
[0039] S31, providing a plurality of standard samples, each of which has a different content of the element to be measured. This step is the same as the above step S21, and will not be repeated here.
[0040] S32, for each standard sample, obtain multiple second response values of the element to be measured therein by ICP-OES multiple times, and average the multiple second response values to obtain a second average response value.
[0041] After preparing multiple standard samples, for each standard sample, multiple measurements are performed by ICP-OES in time division multiple times to obtain multiple second response values of the elements to be measured, and the multiple second response values are averaged to obtain the second average response value, and the number of multiple measurements is 2-10 times. For example, for multiple standard samples prepared from the above-mentioned ternary positive electrode material, each standard sample is measured multiple times by ICP-OES in time division, and each measurement can obtain a second response value of the elements cobalt, manganese and nickel to be measured. After all the measurements are completed, the multiple second response values are averaged to obtain the second average response values of the elements cobalt, manganese and nickel to be measured.
[0042] Similarly, by measuring each standard element multiple times at different times, the random error and uncertainty in a single measurement can be reduced, making the measurement result closer to the true value and improving the accuracy of the measurement.
[0043] In some embodiments, the above step S12 “establishing an EDX calibration method according to the first average response value and the second average response value” specifically includes:
[0044] The first average response value is used as an independent variable and the second average response value is used as a dependent variable. The first average response value and the second average response value are linearly fitted to obtain a linear regression equation. Specifically, Mintab software can be used for linear fitting to obtain a linear regression equation with high accuracy and reliability.
[0045] Furthermore, the step S13 of “correcting the first actual response value according to the correction method to obtain the content value of the element to be measured in the sample to be measured” specifically includes:
[0046] Substitute the first actual response value into the independent variable side of the linear regression equation, and use the calculated result as the content value of the element to be measured.
[0047] This embodiment uses a linear fitting method to correct the first actual response value measured by EDX to obtain a detection result that matches the general ICP-OES in the industry, meets industry standards, and has a shorter test time, a more stable test process, and a higher accuracy test result.
[0048] In some embodiments, the method of measuring the element content in the positive electrode material using an energy dispersive X-ray spectrometer in the present application also includes the following steps S41-S42.
[0049] S41, obtaining a second actual response value of the element to be measured in the sample to be measured by ICP-OES as a verification value.
[0050] In a manner similar to the above steps S31-S32, a sample to be tested is prepared and a second actual response value of the element to be tested in the sample to be tested is obtained by ICP-OES. The second actual response value is also preferably an average value obtained by multiple measurements.
[0051] S42, using the verification value to evaluate the accuracy of the content to be measured.
[0052] The second actual response value is further used as a verification value to evaluate the accuracy of the previously obtained content value of the element to be measured in the sample to be measured. For example, the accuracy can be evaluated by using the difference between the content value and the verification value.
[0053] After using EDX to obtain the content value of the element to be measured in the sample to be measured, this embodiment uses the verification value obtained by ICP-OES to evaluate its accuracy, further verifying the feasibility and reliability of the method of measuring the element content using an energy dispersive X-ray spectrometer.
[0054] The performance improvement brought about by the technical solution provided in this application is explained below with reference to specific embodiments and comparative examples.
[0055] Example 1
[0056] 1) Select 8 ternary lithium battery positive electrode materials with Co content of 2%~23%, Mn content of 12%~20%, and Ni content of 20%~47% to prepare standard samples. The standard samples are made of nickel-cobalt-manganese ternary positive electrode materials with different ratios. The elements to be tested are Co, Mn, and Ni. The sample preparation standard can be found in GBT22554-2010.
[0057] 2) For each standard sample, take part of the standard sample into the sample cup, reaching more than 2 / 3 of the sample cup volume, and manually compact it with a quartz glass rod, which takes 30 seconds. The EDX test time is set to 200 seconds. The test is carried out on different days and repeated twice to obtain the two first response values f of the three elements to be measured in the standard sample. The first average response value F is obtained after averaging. Among them, for nickel, the first average response value is recorded as F1, for cobalt, the first average response value is recorded as F2, and for manganese, the first average response value is recorded as F3.
[0058] 3) For each standard sample, weigh 1.25g of the standard sample, add 20mL of 50% dilute hydrochloric acid, heat and digest at 250℃ on a hot plate, cool the mixture to room temperature after digestion and clarification, transfer it to a 250mL volumetric flask, dilute to the mark with pure water, shake well and transfer 5mL to a 100mL volumetric flask, and then transfer 5mL to a 50mL volumetric flask, and measure on ICP-OES. Perform pretreatment and test once a day, repeat 10 times, and obtain 10 second response values c of the three elements to be measured in the standard sample, and obtain the second average response value C after averaging. Among them, for nickel, the second average response value is recorded as C1, for cobalt, the second average response value is recorded as C2, and for manganese, the second average response value is recorded as C3.
[0059] 4) Using the second average response value C corresponding to the 8 standard samples as the dependent variable and the first average response value F as the independent variable, linear fitting was performed using Mintab software to obtain a linear regression equation with better goodness of fit index and smaller error standard deviation. For nickel, the linear regression equation is expressed as Formula 1: C1=-0.1481+1.008×F1 (R 2 =0.9997); for cobalt, the linear regression equation is recorded as Formula 2: C2=0.07819+1.018×F2 (R 2 =0.9989); for manganese, the linear regression equation is recorded as Formula 3: C3=0.01184+0.989×F3 (R 2 =0.9981). Among them, R 2 The coefficient of determination is used to measure the degree to which the independent variable explains the dependent variable, and its value ranges from 0 to 1. The closer the R² value is to 1, the higher the degree to which the independent variable explains the dependent variable, and the better the goodness of fit of the model. For example, an R² value of 0.9997 means that the independent variable can explain 98.97% of the variability of the dependent variable.
[0060] 5) Prepare two samples to be tested according to step 1), and use EDX to test them according to step 2) to obtain the first actual response value f' of Ni, Co, and Mn in the two samples to be tested.
[0061] 6) Obtain the content values c' of the three elements to be tested, Ni, Co and Mn, respectively, according to the above formulas 1, 2 and 3 and the first actual response values f' of Ni, Co and Mn in the two samples to be tested. That is, substitute the first actual response value f' of each element to be tested into the independent variable side of the corresponding linear regression equation, and then use the calculated result as the content value c' of the element to be tested.
[0062] In this embodiment, EDX with higher test efficiency is used to obtain the content value of the element to be tested in the sample to be tested. In order to verify the accuracy of the test result, two samples to be tested are further tested by ICP-OES according to the above step 3) to obtain the verification values u of the three elements to be tested, Ni, Co, and Mn in the samples to be tested. For specific results, please refer to Table 1 and Table 2.
[0063] Table 1 Comparison of the content values measured by EDX and the verification values measured by ICP-OES for sample 1
[0064]
[0065] Table 2 Comparison of the content values measured by EDX and the verification values measured by ICP-OES for sample 2
[0066]
[0067] The results show:
[0068] a) For nickel (Ni), cobalt (Co) and manganese (Mn), the difference between the average value of the content value c' measured by EDX and the average value of the verification value u measured by ICP-OES is very small, which indicates that the content value of the element to be measured obtained by the method for determining the element content in the positive electrode material using EDX provided in the present application is very close to the verification value obtained using ICP-OES in the prior art. The method of the present application can be used instead of the method of the prior art to obtain the same accurate test effect, while significantly improving the test efficiency and reducing the burden of experimental operations.
[0069] b) The standard deviation of the content value c' measured by EDX is much smaller than the standard deviation of the verification value u measured by ICP-OES, which indicates that the content value c' is very consistent and accurate, that is, the repeatability of EDX test is better than that of ICP-OES, and the test accuracy is higher.
[0070] Example 2
[0071] 1) Select three standard samples with Mn content of 13-22% and Fe content of 13-22%. The standard samples are made of lithium manganese iron phosphate positive electrode materials with different proportions. The elements to be tested are Fe and Mn. The sample preparation standard can be found in GBT22554-2010.
[0072] 2) For each standard sample, dig the standard sample into the sample cup to more than 2 / 3 of the sample volume, and manually compact it with a quartz glass rod. It takes 30 seconds, and the EDX test time is set to 300 seconds. Test on different days, repeat the measurement twice, and obtain the two first response values f of the two elements to be measured in the standard sample. After averaging, the first average response value F is obtained. Among them, for iron, the first average response value is recorded as F4, and for manganese, the first average response value is recorded as F5.
[0073] 3) For each standard sample, weigh 0.4 g of the standard sample, add 5 mL of 70% perchloric acid, shake well, heat and dissolve on an electric furnace until white smoke is gone, remove and cool to room temperature, transfer to a 100 mL volumetric flask, dilute to the mark with pure water, shake well and transfer 1 mL to a 100 mL volumetric flask, measure on ICP-OES, perform pretreatment and test once a day, repeat 10 times, measure 10 second response values c, and average to obtain the second average response value C. Among them, for iron, the second average response value is recorded as C4, and for manganese, the second average response value is recorded as C5.
[0074] 4) Using the second average response value C corresponding to the three standard samples as the dependent variable and the first average response value F as the independent variable, linear fitting was performed using Mintab software to obtain a linear regression equation with better goodness of fit index and smaller error standard deviation. Among them, for iron, the linear regression equation is recorded as Formula 4: C4=0.0983+1.0001×F4 (R 2 =0.998), for manganese, the linear regression equation is recorded as Formula 5, C5=0.6827+1.0172×F5 (R2=0.998).
[0075] 5) Prepare a sample to be tested according to step 1), and test the sample to be tested according to step 2), and obtain the first actual response value f'' of Fe and Mn in the sample to be tested by EDX testing.
[0076] 6) Obtain the content values c'' of the two elements Fe and Mn in the sample according to the above formula 4, formula 5 and the first actual response value f'' of the sample. That is, substitute the first actual response value f'' of each element into the independent variable side of the corresponding linear regression equation, and then use the calculated result as the content value c'' of the element to be measured.
[0077] In this embodiment, EDX with higher testing efficiency is used to obtain the content value of the element to be tested in the sample to be tested. In order to verify the accuracy of the test result, the sample to be tested is further tested by ICP-OES according to step 3) to obtain the verification value u' of each of the elements Fe and Mn to be tested. For specific results, please refer to Table 3.
[0078] Table 3 Comparison of the content values measured by EDX and the verification values measured by ICP-OES for sample 3
[0079]
[0080] The results show:
[0081] a) For iron (Fe) and manganese (Mn), the difference between the average value of the content value c'' measured by EDX and the average value of the verification value u' measured by ICP-OES is very small, which indicates that the content value of the element to be measured obtained by the method for determining the element content in the positive electrode material using EDX provided in the present application is very close to the verification value obtained using ICP-OES in the prior art. The method of the present application can be used instead of the method of the prior art to obtain the same accurate test effect, while significantly improving the test efficiency and reducing the burden of experimental operations.
[0082] b) The standard deviation of the content value c'' measured by EDX is smaller than the standard deviation of the verification value u' measured by ICP-OES, which indicates that the content value c'' is very consistent and accurate, that is, the repeatability of EDX test is better than that of ICP-OES, and the test accuracy is higher.
[0083] The above description is only a preferred embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural changes made under the concept of the present application using the contents of the present application specification and drawings, or directly / indirectly used in other related technical fields are included in the patent protection scope of the present application.
Claims
1. A method for determining element content using an energy dispersive X-ray spectrometer, characterized in that: Includes steps: Providing a plurality of standard samples, each of which has a different content of the element to be measured; For each of the standard samples, the energy dispersive X-ray spectrometer is used to measure multiple times to obtain multiple first response values of the element to be measured, and the multiple first response values are averaged to obtain a first average response value, and Performing multiple measurements on each of the standard samples by an inductively coupled plasma spectrometer to obtain multiple second response values of the element to be measured, and averaging the multiple second response values to obtain a second average response value; Taking the first average response value as an independent variable and the second average response value as a dependent variable, performing a linear fit on the first average response value and the second average response value to obtain a linear regression equation; The first actual response value of the element to be measured in the sample to be measured is obtained by the energy dispersive X-ray spectrometer, the first actual response value is substituted into the independent variable side of the linear regression equation, and the calculation result is used as the content value of the element to be measured to obtain the content value of the element to be measured in the sample to be measured.
2. The method according to claim 1, characterized in that The content of the element to be measured in the sample to be measured is within a preset range, and the preset range is defined by the maximum content and the minimum content of the element to be measured in the multiple standard samples.
3. The method according to claim 1, characterized in that The number of multiple measurements ranges from 2 to 10 times.
4. The method according to claim 1, characterized in that Also includes the steps: Obtaining a second actual response value of the element to be measured in the sample to be measured as a verification value by the inductively coupled plasma spectrometer; The verification value is used to evaluate the accuracy of the content value.
5. The method according to claim 1, characterized in that The number of the standard samples is 3-8.
6. The method according to claim 1, characterized in that The standard sample and the sample to be tested are both nickel-cobalt-manganese ternary positive electrode materials, and the element to be tested is nickel, cobalt or manganese; or, the standard sample and the sample to be tested are both lithium manganese iron phosphate positive electrode materials, and the element to be tested is iron or manganese.