Light emitting diode epitaxial wafer and preparation method thereof, LED
By designing alternately stacked quantum well layers and quantum barrier layers structures in light emitting diodes, adjusting the doping casting concentration and layer thickness, the problems of active layer polarization effect and low carrier recombination efficiency are solved, and a higher Luminous efficiency.
Patent Information
- Application Number
- CN202411147433.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The active layer polarization effect of existing light emitting diodes is large, resulting in increased electron overflow and low carrier recombination efficiency, thereby reducing luminous efficiency.
Design a light emitting diode epitaxial sheet, adopting alternating stacked long-wave, medium-wave and short-wave quantum well layers and quantum barrier layers, and by adjusting doping concentration and layer thickness, the polarization effect is reduced, the barrier height is increased, and the carriers are promoted. Evenly distributed and compounded.
It effectively reduces the polarization effect of the active layer, reduces electron overflow, improves the recombination efficiency of carriers in the active layer, and improves the luminous efficiency of the light emitting diode.
Smart Images

Figure CN118676273B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optoelectronic technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. Background Art
[0002] The recombination efficiency of electrons and holes in the active layer is closely related to the luminous efficiency of the light-emitting diode. The active layer includes a quantum well layer and a quantum barrier layer. In order to improve the wave function coupling between electrons and holes, reduce the overflow of electrons into the P-type layer, and improve the uniform distribution of electrons and holes in the active layer, the quantum barrier layer usually uses AlGaN material. Since the In components of InGaN in quantum wells of different bands are different in the three-band active layer, if the same quantum barrier structure is used, the lattice mismatch between the quantum well layer and the quantum barrier layer increases, and the quantum well polarization effect is enhanced, causing the electrons and holes to be spatially separated in the quantum well, reducing the radiation recombination efficiency. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer, which can reduce the polarization effect of the active layer, increase the barrier height, reduce electron overflow, promote the uniform distribution of carriers in the active layer, improve the recombination efficiency of carriers in the active layer, and improve the luminous efficiency of the light-emitting diode.
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a light emitting diode epitaxial wafer, which has a simple process and can stably prepare a light emitting diode epitaxial wafer with good luminous efficiency.
[0005] In order to solve the above technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged;
[0006] The active layer includes at least one group of alternatingly stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternatingly stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternatingly stacked short-wave quantum well layers and short-wave quantum barrier layers. The wavelength range of photons emitted when carriers in the long-wave quantum well layers and long-wave quantum barrier layers are 460nm~470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers and medium-wave quantum barrier layers are 450nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers and short-wave quantum barrier layers are 440nm~450nm.
[0007] In some embodiments, the long-wave quantum barrier layer includes a first C-doped GaN layer, a first C / Si co-doped GaN layer, a second C-doped GaN layer, a second C / Si co-doped GaN layer, and a third C-doped GaN layer stacked in sequence.
[0008] In some embodiments, the thickness of the long-wave quantum barrier layer is 5 nm to 20 nm;
[0009] The thickness of the first C-doped GaN layer: the thickness of the first C / Si co-doped GaN layer: the thickness of the second C-doped GaN layer: the thickness of the second C / Si co-doped GaN layer: the third C-doped GaN layer=1:(1-10):1:(1-10):1;
[0010] The C doping concentration of the first C-doped GaN layer, the first C / Si co-doped GaN layer, the second C-doped GaN layer, the second C / Si co-doped GaN layer, or the third C-doped GaN layer is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 ;
[0011] The Si doping concentration of the first C / Si co-doped GaN layer or the second C / Si co-doped GaN layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0012] In some embodiments, the medium-wave quantum barrier layer includes a first AlN layer, a fourth C-doped GaN layer, a first C / Si co-doped AlGaN layer, and a fifth C-doped GaN layer stacked in sequence.
[0013] In some embodiments, the thickness of the medium-wave quantum barrier layer is 5 nm to 18 nm;
[0014] The thickness of the first AlN layer: the thickness of the fourth C-doped GaN layer: the first C / Si co-doped AlGaN layer: the fifth C-doped GaN layer=1: (2-10): (10-50): (2-10);
[0015] The C doping concentration of the fourth C-doped GaN layer, the first C / Si co-doped AlGaN layer, or the fifth C-doped GaN layer is 1×10 16 atoms / cm 3 ~9×10 17 atoms / cm 3 ;
[0016] The Si doping concentration of the first C / Si co-doped AlGaN layer is 2×10 17 atoms / cm 3 ~1×1018 atoms / cm 3 .
[0017] In some embodiments, the short-wave quantum barrier layer includes a second AlN layer, a sixth C-doped GaN layer, a second C / Si co-doped AlGaN layer, and a seventh C-doped GaN layer stacked in sequence.
[0018] In some embodiments, the thickness of the short-wave quantum barrier layer is 5 nm to 15 nm;
[0019] The thickness of the second AlN layer: the thickness of the sixth C-doped GaN layer: the thickness of the second C / Si co-doped AlGaN layer: the thickness of the seventh C-doped GaN layer=1: (2-10): (10-50): (2-10);
[0020] The C doping concentration of the sixth C-doped GaN layer, the second C / Si co-doped AlGaN layer, or the seventh C-doped GaN layer is 1×10 16 atoms / cm 3 ~8×10 17 atoms / cm 3 ;
[0021] The Si doping concentration of the second C / Si co-doped AlGaN layer is 3×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0022] In some embodiments, the long-wave quantum well layer, the medium-wave quantum well layer, or the short-wave quantum well layer is an InGaN layer.
[0023] In order to solve the above technical problems, the present invention also provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0024] S1. providing a substrate;
[0025] S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence;
[0026] The active layer includes at least one group of alternatingly stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternatingly stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternatingly stacked short-wave quantum well layers and short-wave quantum barrier layers. The wavelength range of photons emitted when carriers in the long-wave quantum well layers and long-wave quantum barrier layers are 460nm~470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers and medium-wave quantum barrier layers are 450nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers and short-wave quantum barrier layers are 440nm~450nm.
[0027] The implementation of the present invention has the following beneficial effects:
[0028] The light-emitting diode epitaxial wafer provided by the present invention has an active layer comprising at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0029] Furthermore, the long-wave quantum barrier layer is a GaN layer that does not contain Al, which can reduce the polarization effect caused by the lattice mismatch of the long-wave quantum well high-In component InGaN layer. The higher C doping concentration can also expand the V-Pits opening, and the lower Si doping modulated quantum well polarization effect can improve the recombination efficiency of carrier injection into the quantum well layer.
[0030] The medium-wave quantum barrier layer reduces the electron overflow to the P-type GaN layer and reduces the non-radiative recombination of the light-emitting diode by setting multiple high-potential barrier layers. The medium-wave quantum barrier layer includes a first AlN layer, a fourth C-doped GaN layer, a first C / Si co-doped AlGaN layer, and a fifth C-doped GaN layer stacked in sequence. On the one hand, it can shield the defects of the epitaxial layer and improve the crystal quality. On the other hand, it can also regulate the C-Si doping concentration to shield the piezoelectric field effect in the quantum well. It can also regulate the injection depth of holes, improve the uniformity of carriers in the active area, increase the overlap of the wave functions of electrons and holes, and improve the luminous efficiency of the light-emitting diode.
[0031] The short-wave quantum barrier layer is thinner and has a higher Al component to increase the potential barrier and reduce electron overflow. In addition, its low C doping concentration reduces the V-pits opening, increases the light-emitting area of the short-wave quantum well layer, and improves the light-emitting efficiency.
[0032] In summary, the present invention designs a high-quality quantum well layer, and electrons and holes are localized in the quantum well layer, thereby improving the radiation recombination efficiency of the quantum well layer. A multi-period active layer is grown to improve the quantum confinement effect, and electrons and holes are localized in multiple quantum wells, thereby increasing the overlap of electron and hole wave functions, thereby increasing the radiation recombination rate. The present invention sets different band barrier layers to reduce the polarization effect of the active layer, increase the barrier height, reduce electron overflow, promote uniform distribution of carriers in the active layer, improve the recombination efficiency of carriers in the active layer, and improve the luminous efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic structural diagram of the light emitting diode epitaxial wafer provided by the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0035] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0036] In the description of the present invention, it is necessary to understand that the orientations or positional relationships indicated by the terms "upper", "lower", "back surface", "front surface", etc. are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0037] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0038] In the present invention, “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the protection scope of the present invention.
[0039] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0040] In the present invention, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.
[0041] To solve the above problems, the present invention provides a light emitting diode epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, an active layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are sequentially arranged;
[0042] The active layer 500 includes at least one group of alternatingly stacked long-wave quantum well layers 511 and long-wave quantum barrier layers 512, at least one group of alternatingly stacked medium-wave quantum well layers 521 and medium-wave quantum barrier layers 522, and at least one group of alternatingly stacked short-wave quantum well layers 531 and short-wave quantum barrier layers 532. The wavelength range of photons emitted when carriers in the long-wave quantum well layers 511 and the long-wave quantum barrier layers 512 are 460nm~470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers 521 and the medium-wave quantum barrier layers 522 are 450nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers 531 and the short-wave quantum barrier layers 532 are 440nm~450nm.
[0043] The present invention creatively designs the quantum barrier layer of the active layer 500. The specific structure of the quantum barrier layer provided by the present invention is as follows:
[0044] First, the technical details of the long-wave quantum barrier layer 512 are as follows:
[0045] In some embodiments, the long-wave quantum barrier layer 512 includes a first C-doped GaN layer, a first C / Si co-doped GaN layer, a second C-doped GaN layer, a second C / Si co-doped GaN layer, and a third C-doped GaN layer stacked in sequence.
[0046] In some embodiments, the thickness of the long-wave quantum barrier layer 512 is 5nm~20nm; the exemplary thickness of the long-wave quantum barrier layer 512 is 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, but not limited thereto. Preferably, the thickness of the first C-doped GaN layer: the thickness of the first C / Si co-doped GaN layer: the thickness of the second C-doped GaN layer: the thickness of the second C / Si co-doped GaN layer: the third C-doped GaN layer = 1: (1~10): 1: (1~10): 1.
[0047] In some embodiments, the C doping concentration of the first C-doped GaN layer or the first C / Si co-doped GaN layer or the second C-doped GaN layer or the second C / Si co-doped GaN layer or the third C-doped GaN layer is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The Si doping concentration of the first C / Si co-doped GaN layer or the second C / Si co-doped GaN layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0048] The long-wave quantum barrier layer is a GaN layer that does not contain Al, which can reduce the polarization effect caused by the lattice mismatch of the long-wave quantum well high-In component InGaN layer. The higher C doping concentration can expand the V-Pits opening, and the lower Si doping modulated quantum well polarization effect can improve the recombination efficiency of carrier injection into the quantum well layer.
[0049] Secondly, the technical details of the medium-wave quantum barrier layer 522 are as follows:
[0050] In some embodiments, the medium-wave quantum barrier layer 522 includes a first AlN layer, a fourth C-doped GaN layer, a first C / Si co-doped AlGaN layer, and a fifth C-doped GaN layer stacked in sequence.
[0051] In some embodiments, the thickness of the medium-wave quantum barrier layer 522 is 5nm to 18nm; the exemplary thickness of the medium-wave quantum barrier layer 522 is 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, but not limited thereto. Preferably, the thickness of the first AlN layer: the thickness of the fourth C-doped GaN layer: the first C / Si co-doped AlGaN layer: the fifth C-doped GaN layer = 1: (2 to 10): (10 to 50): (2 to 10).
[0052] In some embodiments, the C doping concentration of the fourth C-doped GaN layer or the first C / Si co-doped AlGaN layer or the fifth C-doped GaN layer is 1×10 16 atoms / cm 3 ~9×10 17 atoms / cm 3 ; The Si doping concentration of the first C / Si co-doped AlGaN layer is 2×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0053] The medium-wave quantum barrier layer reduces the electron overflow to the P-type GaN layer and reduces the non-radiative recombination of the light-emitting diode by setting multiple high-potential barrier layers. The medium-wave quantum barrier layer can shield the defects of the epitaxial layer and improve the crystal quality. On the other hand, it can also adjust the C-Si doping concentration to shield the piezoelectric field effect in the quantum well, and can also adjust the injection depth of holes, improve the uniformity of carriers in the active area, increase the wave function overlap of electrons and holes, and improve the luminous efficiency of the light-emitting diode.
[0054] Finally, the technical details of the short-wave quantum barrier layer 532 are as follows:
[0055] In some embodiments, the short-wave quantum barrier layer 532 includes a second AlN layer, a sixth C-doped GaN layer, a second C / Si co-doped AlGaN layer, and a seventh C-doped GaN layer stacked in sequence.
[0056] In some embodiments, the thickness of the short-wave quantum barrier layer 532 is 5 nm to 15 nm; the exemplary thickness of the short-wave quantum barrier layer 532 is 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, but not limited thereto. Preferably, the thickness of the second AlN layer: the thickness of the sixth C-doped GaN layer: the thickness of the second C / Si co-doped AlGaN layer: the seventh C-doped GaN layer = 1: (2 to 10): (10 to 50): (2 to 10).
[0057] In some embodiments, the C doping concentration of the sixth C-doped GaN layer, the second C / Si co-doped AlGaN layer, or the seventh C-doped GaN layer is 1×10 16 atoms / cm 3 ~8×10 17 atoms / cm 3 ; The Si doping concentration of the second C / Si co-doped AlGaN layer is 3×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0058] The short-wave quantum barrier layer is thinner and has a higher Al component to increase the potential barrier and reduce electron overflow. In addition, its low C doping concentration reduces the V-pits opening, increases the light-emitting area of the short-wave quantum well layer, and improves the light-emitting efficiency.
[0059] Comparing the long-wave quantum barrier layer 512, the medium-wave quantum barrier layer 522 and the short-wave quantum barrier layer 532, the following features are found:
[0060] In some embodiments, the thickness of the long-wave quantum barrier layer 512 is greater than the thickness of the medium-wave quantum barrier layer 522 and greater than the thickness of the short-wave quantum barrier layer 532 .
[0061] In some embodiments, the C doping concentration of the long-wave quantum barrier layer 512 is greater than the C doping concentration of the medium-wave quantum barrier layer 522 and greater than the C doping concentration of the short-wave quantum barrier layer 532 .
[0062] In some embodiments, the Si doping concentration of the long-wave quantum barrier layer 512 is less than the Si doping concentration of the medium-wave quantum barrier layer 522 and less than the Si doping concentration of the short-wave quantum barrier layer 532 .
[0063] In some embodiments, the Al component content of the medium-wave quantum barrier layer 522 is less than the Al component content of the short-wave quantum barrier layer 532 .
[0064] In addition to the quantum barrier layer, other technical features of the active layer 500 are described below.
[0065] In some embodiments, the long-wave quantum well layer 511 or the medium-wave quantum well layer 521 or the short-wave quantum well layer 531 is an InGaN layer.
[0066] In some embodiments, the active layer 500 includes, in sequence:
[0067] h alternately stacked long-wave quantum well layers 511 and long-wave quantum barrier layers 512,
[0068] j alternately stacked medium-wave quantum well layers 521 and medium-wave quantum barrier layers 522,
[0069] k alternately stacked short-wave quantum well layers 531 and short-wave quantum barrier layers 532;
[0070] h≥1, j≥1, k≥1.
[0071] Preferably, 1≤h≤20, 1≤j≤20, and 1≤k≤20.
[0072] In summary, the present invention designs a high-quality quantum well layer, and electrons and holes are localized in the quantum well layer, thereby improving the radiation recombination efficiency of the quantum well layer. A multi-period active layer is grown to improve the quantum confinement effect, and electrons and holes are localized in multiple quantum wells, thereby increasing the overlap of electron and hole wave functions, thereby increasing the radiation recombination rate. The present invention sets different band barrier layers to reduce the polarization effect of the active layer, increase the barrier height, reduce electron overflow, promote uniform distribution of carriers in the active layer, improve the recombination efficiency of carriers in the active layer, and improve the luminous efficiency of the light-emitting diode.
[0073] Accordingly, the present invention provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0074] S1, providing a substrate 100;
[0075] In some embodiments, the substrate 100 may be selected from one of a sapphire substrate, a SiO2 sapphire composite substrate, a silicon substrate, a silicon carbide substrate, a gallium nitride substrate, and a zinc oxide substrate. Preferably, the substrate 100 is a sapphire substrate, which is a commonly used GaN-based LED substrate material. The sapphire substrate has a mature preparation process, a low price, is easy to clean and handle, and has good stability at high temperatures.
[0076] S2, depositing a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, an active layer 500, an electron blocking layer 600, and a P-type GaN layer 700 in sequence on the substrate 100.
[0077] Specifically, the above preparation method comprises the following steps:
[0078] S21 , depositing the buffer layer 200 on the substrate 100 .
[0079] In some embodiments, the buffer layer 200 is an AlN buffer layer.
[0080] S22 , depositing the undoped GaN layer 300 on the buffer layer 200 .
[0081] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, N source and Ga source are introduced, and a non-doped GaN layer with a thickness of 1 μm to 5 μm is grown.
[0082] S23 , depositing the N-type GaN layer 400 on the undoped GaN layer 300 .
[0083] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.
[0084] S24 , depositing the active layer 500 on the N-type GaN layer 400 .
[0085] The active layer 500 includes at least one group of alternatingly stacked long-wave quantum well layers 511 and long-wave quantum barrier layers 512, at least one group of alternatingly stacked medium-wave quantum well layers 521 and medium-wave quantum barrier layers 522, and at least one group of alternatingly stacked short-wave quantum well layers 531 and short-wave quantum barrier layers 532. The wavelength range of photons emitted when carriers in the long-wave quantum well layers 511 and the long-wave quantum barrier layers 512 are 460nm~470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers 521 and the medium-wave quantum barrier layers 522 are 450nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers 531 and the short-wave quantum barrier layers 532 are 440nm~450nm.
[0086] In some embodiments, the growth pressure of the long-wave quantum barrier layer 512 is 50 torr to 500 torr, and the growth temperature is 800° C. to 1000° C.;
[0087] The growth pressure of the medium-wave quantum barrier layer 522 is 50 torr to 500 torr, and the growth temperature is 800° C. to 1000° C.;
[0088] The growth pressure of the short-wave quantum barrier layer 532 is 50 torr to 500 torr, and the growth temperature is 800° C. to 1000° C.
[0089] S25, depositing the electron blocking layer 600 on the active layer 500;
[0090] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1000° C., the pressure is controlled at 100 torr to 300 torr, N source, Al source, Ga source, and In source are introduced, and an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm is grown.
[0091] S26 , depositing the P-type GaN layer 700 on the electron blocking layer 600 .
[0092] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1050° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Mg source, and a Ga source are introduced to grow the P-type GaN layer.
[0093] Accordingly, the present invention further provides an LED, which comprises the above-mentioned light-emitting diode epitaxial wafer, wherein the photoelectric efficiency of the LED is effectively improved and other electrical properties are good.
[0094] The present invention is further described below with specific embodiments:
[0095] Example 1
[0096] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0097] The active layer includes at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0098] The long-wave quantum barrier layer includes a first C-doped GaN layer, a first C / Si co-doped GaN layer, a second C-doped GaN layer, a second C / Si co-doped GaN layer, and a third C-doped GaN layer stacked in sequence. The thickness of the long-wave quantum barrier layer is 12 nm; the thickness of the first C-doped GaN layer: the thickness of the first C / Si co-doped GaN layer: the thickness of the second C-doped GaN layer: the thickness of the second C / Si co-doped GaN layer: the thickness of the third C-doped GaN layer = 1:6:1:6:1. The C doping concentration of the long-wave quantum barrier layer is 6×10 16 atoms / cm 3 The Si doping concentration of the long-wave quantum barrier layer is 3×10 17 atoms / cm 3 .
[0099] The medium-wave quantum barrier layer includes a first AlN layer, a fourth C-doped GaN layer, a first C / Si co-doped AlGaN layer, and a fifth C-doped GaN layer stacked in sequence. The thickness of the medium-wave quantum barrier layer is 10 nm; the thickness of the first AlN layer: the thickness of the fourth C-doped GaN layer: the first C / Si co-doped AlGaN layer: the fifth C-doped GaN layer = 1:4:16:4. The C doping concentration of the medium-wave quantum barrier layer is 4×1016 atoms / cm 3 The Si doping concentration of the medium-wave quantum barrier layer is 4×10 17 atoms / cm 3 .
[0100] The short-wave quantum barrier layer comprises a second AlN layer, a sixth C-doped GaN layer, a second C / Si co-doped AlGaN layer, and a seventh C-doped GaN layer stacked in sequence. The thickness of the short-wave quantum barrier layer is 9 nm;
[0101] The thickness of the second AlN layer: the thickness of the sixth C-doped GaN layer: the thickness of the second C / Si co-doped AlGaN layer: the seventh C-doped GaN layer = 1:4:16:4. The C doping concentration of the short-wave quantum barrier layer is 3×10 16 atoms / cm 3 The Si doping concentration of the short-wave quantum barrier layer is 5×10 18 atoms / cm 3 .
[0102] The long-wave quantum well layer, the medium-wave quantum well layer, or the short-wave quantum well layer is an InGaN layer.
[0103] Example 2
[0104] This embodiment provides a light-emitting diode epitaxial wafer, which is different from Embodiment 1 in that: the thickness of the long-wave quantum barrier layer is 15nm; the thickness of the medium-wave quantum barrier layer is 12nm; the thickness of the short-wave quantum barrier layer is 10nm, and the rest is the same as Embodiment 1.
[0105] Example 3
[0106] This embodiment provides a light-emitting diode epitaxial wafer, which is different from Embodiment 1 in that: the thickness of the long-wave quantum barrier layer is 9nm; the thickness of the medium-wave quantum barrier layer is 8nm; the thickness of the short-wave quantum barrier layer is 7nm, and the rest is the same as Embodiment 1.
[0107] Example 4
[0108] This embodiment provides a light-emitting diode epitaxial wafer, which is different from the embodiment 1 in that the C doping concentration of the long-wave quantum barrier layer is 5×10 16 atoms / cm 3 The C doping concentration of the medium-wave quantum barrier layer is 3.5×10 16 atoms / cm 3 The C doping concentration of the short-wave quantum barrier layer is 3×10 16 atoms / cm 3, the rest are the same as in Example 1.
[0109] Example 5
[0110] This embodiment provides a light-emitting diode epitaxial wafer, which is different from the embodiment 1 in that the C doping concentration of the long-wave quantum barrier layer is 6.5×10 16 atoms / cm 3 The C doping concentration of the medium-wave quantum barrier layer is 5×10 16 atoms / cm 3 The C doping concentration of the short-wave quantum barrier layer is 3.5×10 16 atoms / cm 3 , the rest are the same as in Example 1.
[0111] Example 6
[0112] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 1 in that the Si doping concentration of the long-wave quantum barrier layer is 3.5×10 17 atoms / cm 3 The Si doping concentration of the medium-wave quantum barrier layer is 5×10 17 atoms / cm 3 The Si doping concentration of the short-wave quantum barrier layer is 6×10 17 atoms / cm 3 , the rest are the same as in Example 1.
[0113] Example 7
[0114] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 1 in that the Si doping concentration of the long-wave quantum barrier layer is 3×10 17 atoms / cm 3 The Si doping concentration of the medium-wave quantum barrier layer is 3.8×10 17 atoms / cm 3 The Si doping concentration of the short-wave quantum barrier layer is 4.5×10 17 atoms / cm 3 , the rest are the same as in Example 1.
[0115] Comparative Example 1
[0116] This comparative example provides a light emitting diode epitaxial wafer, which is different from the other embodiment 1 in that its active layer includes alternately stacked InGaN quantum well layers and AlGaN quantum barrier layers, and the rest is the same as the first embodiment.
[0117] The light-emitting diode epitaxial wafers prepared in Examples 1 to 7 and Comparative Example 1 were prepared into 10 mil×24 mil chips using the same chip process conditions. 300 LED chips were respectively extracted and tested at a current of 120 mA. Compared with the LED prepared in Comparative Example 1, the luminous efficiency improvement rate of each example was calculated. The specific test results are shown in Table 1.
[0118] Table 1 Performance test results of LEDs obtained from Examples 1 to 7
[0119]
[0120] From the above results, it can be seen that the light-emitting diode epitaxial wafer provided by the present invention, by designing a high-quality quantum well layer, electrons and holes are localized in the quantum well layer, thereby improving the radiation recombination efficiency of the quantum well layer. The multi-period active layer is grown to improve the quantum confinement effect, and electrons and holes are localized in the multi-quantum well, thereby increasing the overlap of the electron and hole wave functions, thereby increasing the radiation recombination rate. The present invention sets different band barrier layers to reduce the polarization effect of the active layer, increase the barrier height, reduce electron overflow, promote uniform distribution of carriers in the active layer, improve the recombination efficiency of carriers in the active layer, and improve the luminous efficiency of the light-emitting diode.
[0121] In the description of this specification, the description with reference to the terms "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0122] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; The active layer comprises at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers, the wavelength range of photons emitted when carriers in the long-wave quantum well layers and long-wave quantum barrier layers are 460nm-470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers and medium-wave quantum barrier layers are 450nm-460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers and short-wave quantum barrier layers are 440nm-450nm; The long-wave quantum barrier layer comprises a first C-doped GaN layer, a first C / Si co-doped GaN layer, a second C-doped GaN layer, a second C / Si co-doped GaN layer, and a third C-doped GaN layer stacked in sequence; The medium-wave quantum barrier layer comprises a first AlN layer, a fourth C-doped GaN layer, a first C / Si co-doped AlGaN layer, and a fifth C-doped GaN layer stacked in sequence; The short-wave quantum barrier layer includes a second AlN layer, a sixth C-doped GaN layer, a second C / Si co-doped AlGaN layer, and a seventh C-doped GaN layer which are stacked in sequence.
2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the long-wave quantum barrier layer is 5nm~20nm; The thickness of the first C-doped GaN layer: the thickness of the first C / Si co-doped GaN layer: the thickness of the second C-doped GaN layer: the thickness of the second C / Si co-doped GaN layer: the third C-doped GaN layer=1:(1-10):1:(1-10):1; The C doping concentration of the first C-doped GaN layer, the first C / Si co-doped GaN layer, the second C-doped GaN layer, the second C / Si co-doped GaN layer, or the third C-doped GaN layer is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The Si doping concentration of the first C / Si co-doped GaN layer or the second C / Si co-doped GaN layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the medium-wave quantum barrier layer is 5nm to 18nm; The thickness of the first AlN layer: the thickness of the fourth C-doped GaN layer: the first C / Si co-doped AlGaN layer: the fifth C-doped GaN layer=1: (2-10): (10-50): (2-10); The C doping concentration of the fourth C-doped GaN layer, the first C / Si co-doped AlGaN layer, or the fifth C-doped GaN layer is 1×10 16 atoms / cm 3 ~9×10 17 atoms / cm 3 ; The Si doping concentration of the first C / Si co-doped AlGaN layer is 2×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
4. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the short-wave quantum barrier layer is 5nm~15nm; The thickness of the second AlN layer: the thickness of the sixth C-doped GaN layer: the thickness of the second C / Si co-doped AlGaN layer: the thickness of the seventh C-doped GaN layer=1: (2-10): (10-50): (2-10); The C doping concentration of the sixth C-doped GaN layer, the second C / Si co-doped AlGaN layer, or the seventh C-doped GaN layer is 1×10 16 atoms / cm 3 ~8×10 17 atoms / cm 3 ; The Si doping concentration of the second C / Si co-doped AlGaN layer is 3×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
5. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The long-wave quantum well layer, the medium-wave quantum well layer, or the short-wave quantum well layer is an InGaN layer.
6. A method for preparing a light emitting diode epitaxial wafer according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. providing a substrate; S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence; The active layer includes at least one group of alternatingly stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternatingly stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternatingly stacked short-wave quantum well layers and short-wave quantum barrier layers. The wavelength range of photons emitted when carriers in the long-wave quantum well layers and long-wave quantum barrier layers are 460nm~470nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layers and medium-wave quantum barrier layers are 450nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layers and short-wave quantum barrier layers are 440nm~450nm.
7. An LED, characterized in that: The LED comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 5.