Safe prime coat slurry and preparation method thereof, positive plate and safe lithium battery

By using new safety primer slurry in lithium-ion batteries, the problems of high temperature, long circulation and large internal resistance of lithium batteries are solved, and more stable battery performance and safety performance are achieved, and the circulation and conductivity of the battery are enhanced.

CN119069714APending Publication Date: 2024-12-03CHONGQING ZIJIAN NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105260.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The safety coating of existing lithium batteries has problems such as long and poor circulation, large internal resistance and easy drop, which affects the safety performance of the battery.

Method used

A new type of safety primer slurry is adopted, including 45% primer slurry and 55% solvent. The primer slurry contains binder, conductive agent, silicone coupling agent and dispersant, and passes a specific stirring process Prepare to form a uniformly dispersed safety primer layer, reducing the internal resistance of the battery and improving safety performance.

Benefits of technology

It significantly improves the safety performance and long cycle performance of lithium-ion batteries, reduces the polarization effect of the safety coating, enhances the stability and conductivity of the battery, and avoids the battery thermal runaway and drop problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses novel safe prime coat slurry, which is prepared from the following components in percentage by mass: 40 to 50 percent of prime coat slurry and 50 to 60 percent of solvent, wherein the prime coat slurry comprises the following components in percentage by mass: 3.5% of a binder, 1-2.4% of a first conductive agent, 1-2.4% of a second conductive agent, 1-2% of a siloxane coupling agent, 1% of a dispersing agent and 90.7-93.5% of a safe prime coat main material. The invention also provides a preparation method of the safe prime coat slurry. The invention aims to solve the problems of poor high-temperature long circulation, large internal resistance, easy falling of the safe coating and the like of the safe lithium ion battery, and is a safe battery technology with both electrochemical performance and safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a safe primer slurry and a preparation method thereof, a positive electrode sheet and a safe lithium battery. Background Art

[0002] With the continuous development of consumer batteries, electric vehicles, energy storage and other fields, the requirements for the energy density and safety performance of lithium batteries are getting higher and higher. There are four modes of lithium-ion battery failure, namely, short circuit between the positive current collector and the negative current collector, short circuit between the positive active material and the negative active material, short circuit between the negative active material and the positive current collector, and short circuit between the positive active material and the negative current collector. Usually, the most dangerous safety failure mode of lithium batteries is the short circuit between the fully charged negative active material and the positive current collector. This short circuit mode will instantly generate a lot of heat, causing the battery to thermally run away and catch fire. In order to avoid short circuits within the battery, relevant researchers have improved many aspects of lithium-ion batteries to improve the overall safety performance of lithium-ion batteries.

[0003] At present, the more common technologies are mainly from two aspects. On the one hand, a safety coating is applied on the surface of the current collector, and on the other hand, flame retardants are added to the electrode material or flame retardant components are added to the electrolyte. The former requires the improvement of the fluid itself by adding an extra layer of safety coating between the electrode material and the current collector foil, while the latter only requires the addition of flame retardants when feeding. At present, the solutions for safety coating in the industry mainly include: (1) coating the surface of the positive aluminum foil with a lithium iron phosphate safety coating; (2) coating the surface of the positive current collector with an Al2O3 safety coating. Both methods can avoid direct contact between the bare aluminum foil and the active materials on the negative copper foil, thereby improving the safety performance of the battery. However, both methods have problems such as reduced battery capacity, deterioration at high temperature and long cycles, deterioration of internal resistance, and easy falling off of the safety coating.

[0004] Therefore, it is urgent to develop a new type of safe primer to solve the problems existing in the above methods. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned defects in the prior art and provide a new type of safety primer slurry and its preparation method to solve the problems of poor high temperature and long cycle of safe lithium-ion batteries, large internal resistance and easy falling of the safety coating. It is a safe battery technology that takes into account both electrochemical performance and safety performance.

[0006] To achieve the above object, the present invention provides a safe primer slurry, which comprises the following components by mass percentage: 45% primer slurry and 55% solvent;

[0007] The primer slurry comprises the following components by mass percentage: 3.5% binder, 1-2.4% first conductive agent, 1-2.4% second conductive agent, 1-2% siloxane coupling agent, 1% dispersant and 90.7-93.5% safety primer main material.

[0008] Furthermore, the binder includes one or more of PVDF (polyvinylidene fluoride), PVA (polyvinyl alcohol) when the content of the first conductive agent and the silane coupling agent remains unchanged), PTFE (polytetrafluoroethylene), SBR (styrene-butadiene rubber), PAN (polyacrylonitrile), PI (polyimide), PAA (polyacrylic acid), CMC (sodium carboxymethyl cellulose) and sodium alginate.

[0009] Further, the first conductive agent and the second conductive agent both include one or more of acetylene black, SP (conductive carbon black), Ketjen black, carbon black, vapor-grown carbon fiber, CNT (carbon nanotube)

[0010] Furthermore, the siloxane coupling agent includes one or more of methyl acyloxy siloxane, acyloxy siloxane, and vinyl siloxane.

[0011] Furthermore, the dispersant includes one or more of sodium carboxymethyl cellulose, polyacrylamide, polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, gum arabic, gelatin, acrylamide-acrylonitrile copolymer, acrylic acid-acrylamide copolymer, and acrylic acid-acrylamide-acrylonitrile copolymer.

[0012] Furthermore, the solvent includes one or more of NMP (N-methylpyrrolidone) solvent, ethanol, and acetone.

[0013] Furthermore, the main material of the safety primer is one or more of Al2O3 (aluminum oxide), LATP (lithium aluminum titanium phosphate), zirconium oxide, magnesium oxide, silicon oxide and boehmite.

[0014] A method for preparing a safety primer slurry comprises the following steps:

[0015] S1. Firstly, dissolve the binder in the solvent and stir at a uniform speed;

[0016] S2, then dissolving the first conductive agent and the second conductive agent in the solvent one by one while stirring;

[0017] S3, then add siloxane coupling agent under low temperature environment and stir evenly;

[0018] S4, the main material of the safety primer is evenly divided into two parts, the first part of the main material of the safety primer is added to the solvent of step S3 and continued to stir at a low speed, and then the second part of the main material of the safety primer is added and stirred at a high speed;

[0019] S5. Finally, add the dispersant and stir evenly;

[0020] S6. After the above stirring is completed, the viscosity of the obtained slurry is tested and judged; if the viscosity requirement is not met, continue to add solvent until the viscosity reaches the qualified level;

[0021] S7. After the viscosity is qualified, continue to stir slowly to finally obtain a safe primer slurry.

[0022] A positive electrode sheet comprises a positive electrode current collector, wherein both surfaces of the positive electrode current collector body are coated with the above-mentioned safety primer slurry. A safe lithium-ion battery comprises the above-mentioned positive electrode sheet.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1) The present invention has significant advantages in the pulping process of the safety primer slurry, that is, the oxygen atoms in the silicon-oxygen bonds in the siloxane coupling agent can form hydrogen bonds with the hydrogen atoms in the hydrogen-oxygen bonds on the surface of the safety primer main material, which will promote the first conductive agent and the second conductive agent in the safety primer slurry to be more evenly dispersed on the surface of the safety primer main material, thereby reducing the polarization effect of the safety primer layer and ultimately reducing the internal resistance of the battery.

[0025] 2) There is a relatively optimal range for the relative ratio of the first conductive agent and the second conductive agent in the safety primer slurry of the present invention, so that the repulsion strength between the safety primer main material particles and the first conductive agent and the second conductive agent particles in the safety primer slurry is maximized, that is, the Zeta potential is maximized, making the safety primer slurry system more stable, thereby improving the safety performance of the battery.

[0026] 3) The present invention can enhance the long cycle performance of the battery. DETAILED DESCRIPTION

[0027] The technical solution in this embodiment of the present invention will be described clearly and completely below. Obviously, the described embodiment is one embodiment of the present invention, not all embodiments of the present invention. Based on this embodiment of the present invention, all other embodiments of the present invention obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0029] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features.

[0030] The embodiments of the present invention provide a safe primer slurry and a preparation method thereof, a positive electrode sheet and a safe lithium-ion battery, as follows:

[0031] Example 1

[0032] This embodiment provides a safety primer slurry, which comprises the following components by mass percentage: 45% primer slurry and 55% solvent;

[0033] The primer slurry of this embodiment comprises the following components by mass percentage:

[0034] 3.5% binder, 1.6% first conductive agent, 1.6% second conductive agent, 1% siloxane coupling agent, 1% dispersant and 91.3% safety primer main material.

[0035] Furthermore, the solvent of this embodiment is NMP solvent, the binder is PVDF, the first conductive agent is CNT, the second conductive agent is SP, the siloxane coupling agent is methyl acyloxy siloxane, the dispersant is sodium carboxymethyl cellulose, and the main material of the safety primer is Al2O3.

[0036] In some embodiments, the above-mentioned binder can also be replaced by one or more of PVDF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), SBR (styrene-butadiene rubber), PAN (polyacrylonitrile), PI (polyimide), PAA (polyacrylic acid), CMC (sodium carboxymethyl cellulose) and sodium alginate.

[0037] In some embodiments, the first conductive agent and the second conductive agent may be replaced by one or more of acetylene black, Super-P (conductive carbon black), Ketjen black, carbon black, vapor-grown carbon fiber, and carbon nanotubes;

[0038] In some embodiments, the above-mentioned siloxane coupling agent can be replaced by one or more of methyl acyloxy siloxane, acyloxy siloxane, and vinyl siloxane.

[0039] In some embodiments, the above dispersant can be replaced by one or more of sodium carboxymethyl cellulose, polyacrylamide, polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, gum arabic, gelatin, acrylamide-acrylonitrile copolymer, acrylic acid-acrylamide copolymer, and acrylic acid-acrylamide-acrylonitrile copolymer.

[0040] In some embodiments, the above solvent can be replaced by one or more of NMP, ethanol, and acetone.

[0041] In some embodiments, the main material of the safety primer can be replaced by one or more of Al2O3 (aluminum oxide), LATP (lithium aluminum titanium phosphate), zirconium oxide, magnesium oxide, silicon oxide, and boehmite.

[0042] In some preferred embodiments, the binder may also be 1%, 1.2%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.6%, 3% or 3.2% by mass.

[0043] In some preferred real-time modes, the dispersant may also be 0.5%, 0.7%, 0.8%, 0.9%, 1.2%, 1.5%, 1.7%, 1.8% or 2% by mass.

[0044] A method for preparing a safety primer slurry comprises the following steps:

[0045] S1. First, dissolve 3.5% of the binder by mass in the solvent, and stir at a revolution speed of 25 rpm and a rotation speed of 2900 rpm for 130 min;

[0046] S2, then sequentially dissolving the first conductive agent and the second conductive agent in the solvent while stirring, specifically adding 1.6% by mass of the first conductive agent, stirring at a revolution speed of 58 rpm and a rotation speed of 4200 rpm for 60 min; continuing to add 1.6% by mass of the second conductive agent, stirring at a revolution speed of 32 rpm and a rotation speed of 1200 rpm for 10 min to scrape the cylinder, and then stirring at a revolution speed of 58 rpm and a rotation speed of 4200 rpm for 90 min;

[0047] S3, then under a low temperature environment of ≤5°C (the purpose of adding at low temperature is to improve the physical and mechanical strength of the material and enhance the interface bonding force), add 1% by weight of siloxane coupling agent, and stir at a revolution speed of 25 rpm and a rotation speed of 2900 rpm for 120 min;

[0048] S4, then add 91.3% of the safety primer main material by mass, the safety primer main material is evenly divided into two parts (to promote dispersion and eliminate the phenomenon of material agglomeration), first add the first part of the safety primer main material to the solution obtained in step S3, stir for 10 minutes at a revolution of 32rpm and a rotation speed of 1200rpm to scrape the cylinder, then add the second part of the safety primer main material, and stir for 150 minutes at a revolution speed of 58rpm and a rotation speed of 3044rpm until it is uniform;

[0049] S5, finally adding 1.0% by mass of a dispersant therein, and stirring at an orbital speed of 25 rpm and a rotational speed of 2900 rpm for 200 min;

[0050] S6. After the above stirring is completed, the viscosity of the obtained slurry is tested and judged; the viscosity is 300-1000 Pas, which is up to standard. If the viscosity requirement is not met, continue to add solvent until the viscosity is qualified;

[0051] S7. After the viscosity is qualified, continue to stir slowly for 20 minutes to finally obtain a safe primer slurry.

[0052] The mass percentage of the solvent can be adjusted according to the actual viscosity of the safety primer slurry in step S6. In addition to 55% in this embodiment, the content of the solvent can be added and adjusted according to the viscosity of the safety primer slurry. In terms of mass percentage, the solvent can also be 50%, 52%, 53%, 56%, 57% or 60%, and the corresponding mass ratio of the safety primer slurry is 50%, 48%, 47%, 44%, 43% or 40%.

[0053] A positive electrode current collector comprises a positive electrode current collector body, both surfaces of which are coated with the above-mentioned safety primer slurry.

[0054] A positive electrode sheet comprises a positive electrode current collector, wherein both surfaces of the positive electrode current collector body are coated with the above-mentioned safety primer slurry.

[0055] A safe lithium-ion battery comprises the above-mentioned positive electrode sheet.

[0056] Example 2

[0057] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0058] 3.5% binder, 1.6% first conductive agent, 1.6% second conductive agent, 2% siloxane coupling agent, 1% dispersant and 90.3% safety primer main material.

[0059] The rest is the same as in Example 1.

[0060] Example 3

[0061] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0062] 3.5% binder, 1.6% first conductive agent, 1% second conductive agent, 1% siloxane coupling agent, 1% dispersant and 91.9% safety primer main material.

[0063] The rest is the same as in Example 1.

[0064] Example 4

[0065] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0066] 3.5% binder, 1.6% first conductive agent, 2.4% second conductive agent, 1% siloxane coupling agent, 1% dispersant and 90.5% safety primer main material.

[0067] The rest is the same as in Example 1.

[0068] Example 5

[0069] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0070] 3.5% binder, 1% first conductive agent, 1.6% second conductive agent, 1% siloxane coupling agent, 1% dispersant and 91.9% safety primer main material.

[0071] The rest is the same as in Example 1.

[0072] Example 6

[0073] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0074] 3.5% binder, 2.4% first conductive agent, 1.6% second conductive agent, 1% siloxane coupling agent, 1% dispersant and 90.5% safety primer main material.

[0075] The rest is the same as in Example 1.

[0076] Example 7

[0077] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0078] 3.5% binder, 1.6% first conductive agent, 1.6% second conductive agent, 1.6% siloxane coupling agent, 1% dispersant and 90.7% safety primer main material.

[0079] The rest is the same as in Example 1.

[0080] Example 8

[0081] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0082] 3.5% binder, 1.6% first conductive agent, 1.6% second conductive agent, 1.2% siloxane coupling agent, 1% dispersant and 93.5% safety primer main material.

[0083] The rest is the same as in Example 1.

[0084] Comparative Example 1

[0085] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0086] 3.5% binder, 1.8% first conductive agent, 1.8% second conductive agent, 1% dispersant and 91.9% safety primer main material.

[0087] Comparative Example 2

[0088] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0089] 3.5% binder, 2.4% first conductive agent, 2.4% second conductive agent, 1% dispersant and 90.7% safety primer main material.

[0090] Comparative Example 3

[0091] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0092] 3.5% binder, 1% first conductive agent, 1% second conductive agent, 1% dispersant and 93.5% safety primer main material.

[0093] Comparative Example 4

[0094] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0095] 3.5% binder, 1.8% first conductive agent, 1% second conductive agent, 1% dispersant and 92.7% safety primer main material.

[0096] Comparative Example 5

[0097] The difference between this embodiment and embodiment 1 is that the primer slurry comprises the following components by mass percentage:

[0098] 3.5% binder, 1% first conductive agent, 1.8% second conductive agent, 1% dispersant and 92.7% safety primer main material.

[0099] The primer compositions of Examples 1 to 8 and Comparative Examples 1 to 5 are shown in Table 1. The safe lithium-ion batteries obtained in Examples 1 to 8 and Comparative Examples 1 to 5 were subjected to a needle puncture test, a heavy object impact test, a 25° C. cycle test, and a 45° C. cycle test. The test results are shown in Table 2:

[0100]

[0101] Table 1 Safety primer slurry formula for batteries in Examples 1 to 8 and Comparative Examples 1 to 5

[0102]

[0103]

[0104] Table 2 Test results of batteries of Examples 1 to 8 and Comparative Examples 1 to 5

[0105] From Table 1 and Table 2, we can see that:

[0106] By comparing Example 1 with Comparative Examples 1-5, it can be seen that the battery made of the primer foil coated with the safety primer slurry with the addition of silane coupling agent exhibits excellent characteristics in terms of safety, electrochemical performance and cycle performance.

[0107] By comparing Example 1 with Example 2, Example 7 and Example 8, it can be seen that, under the same first conductive agent and second conductive agent, the content of silane coupling agent gradually increases. On the one hand, the internal resistance of the battery gradually decreases. It can be seen that the increase in the content of silane coupling agent can promote the uniform dispersion of the conductive agent on the surface of the main material of the safety primer, thereby reducing the polarization effect of the safety primer layer and ultimately reducing the internal resistance of the battery; on the other hand, the cycle thickness expansion and cycle capacity retention rate of the battery gradually increase, indicating that the increase in the content of silane coupling agent is beneficial to enhancing the cycle performance of the battery.

[0108] By comparing Example 1 with Example 3 and Example 4, it can be seen that when the content of the first conductive agent and the silane coupling agent remains unchanged, the content of the second conductive agent gradually increases, and the cycle performance of the battery gradually improves. This shows that after adding the second conductive agent, the undercoated electrode has higher toughness, which can improve the peeling problem caused by the volume change of the material during the charge and discharge process, thereby improving the cycle life.

[0109] By comparing Example 1 with Example 5 and Example 6, it can be seen that when the contents of the second conductive agent and the silane coupling agent remain unchanged, the content of the first conductive agent gradually increases and the internal resistance of the battery gradually decreases, indicating that it can improve the conductivity of the battery, that is, it has good ionic and electronic conductivity, which helps to improve the electronic conductivity of the material.

[0110] By comparing Example 1 with Example 3, Example 4, Example 5 and Example 6, it can be seen that when the ratio of the first conductive agent to the second conductive agent is 1:1 under the condition that the content of the silane coupling agent remains unchanged, the needle puncture and heavy object impact performance of the battery are optimal, indicating that there is a relatively excellent range for the relative ratio of the first conductive agent and the second conductive agent in the safety primer slurry, so that the repulsion strength between the safety primer main material particles and the first conductive agent and the second conductive agent particles in the safety primer slurry is the largest, that is, the Zeta potential is the largest, which makes the safety primer slurry system more stable, thereby improving the safety performance of the battery.

[0111] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A safe primer slurry, It is characterized in that The composition comprises the following components by mass percentage: 40-50% of primer slurry and 50-60% of solvent; The primer slurry comprises the following components by mass percentage: 1-3.5% binder, 1-2.4% first conductive agent, 1-2.4% second conductive agent, 1-2% siloxane coupling agent, 0.5-2% dispersant and 90.7-93.5% safety primer main material.

2. The safety primer slurry according to claim 1, It is characterized in that The binder includes one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, styrene-butadiene rubber, polyacrylonitrile, polyimide, polyacrylic acid, sodium carboxymethyl cellulose and sodium alginate.

3. The safety primer slurry according to claim 1, It is characterized in that The first conductive agent and the second conductive agent both include one or more of acetylene black, conductive carbon black, Ketjen black, carbon black, vapor-grown carbon fiber, and carbon nanotubes.

4. The safety primer slurry according to claim 1, It is characterized in that The siloxane coupling agent includes one or more of methyl acyloxy siloxane, acyloxy siloxane and vinyl siloxane.

5. The safety primer slurry according to claim 1, It is characterized in that The dispersant includes one or more of sodium carboxymethyl cellulose, polyacrylamide, polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, gum arabic, gelatin, acrylamide-acrylonitrile copolymer, acrylic acid-acrylamide copolymer, and acrylic acid-acrylamide-acrylonitrile copolymer.

6. The safety primer slurry according to claim 1, It is characterized in that The solvent includes one or more of N-methylpyrrolidone solvent, ethanol, and acetone.

7. The safety primer slurry according to claim 1, It is characterized in that The main material of the safety primer is one or more of aluminum oxide, lithium aluminum titanium phosphate, zirconium oxide, magnesium oxide, silicon oxide, and boehmite.

8. The method for preparing the safety primer slurry according to any one of claims 1 to 7 comprises the following steps: S1. Firstly, dissolve the binder in the solvent and stir at a uniform speed; S2, then dissolving the first conductive agent and the second conductive agent in the solvent one by one while stirring; S3, adding siloxane coupling agent under low temperature environment and stirring evenly; S4, the main material of the safety primer is evenly divided into two parts, the first part of the main material of the safety primer is added to the solvent of step S3 and continued to stir at a low speed, and then the second part of the main material of the safety primer is added and stirred at a high speed; S5. Finally, add the dispersant and stir evenly; S6. After the above stirring is completed, the viscosity of the obtained slurry is tested and judged; if the viscosity requirement is not met, continue to add solvent until the viscosity reaches the qualified level; S7. After the viscosity is qualified, continue to stir slowly to finally obtain a safe primer slurry.

9. A positive electrode sheet, It is characterized in that It comprises a positive electrode current collector, both surfaces of which are coated with the safety primer slurry according to claim 8.

10. A safe lithium-ion battery, It is characterized in that Including the positive electrode sheet as described in claim 9.