Preparation of a single-phase mullite sol and method for rapid gelation thereof
By combining modified polyvinyl alcohol solution and diluted nitric acid, the hydrolysis rate is controlled, and boric acid is added to the single-phase mullite sol, the problems of low hydrolysis efficiency and long gelation time of single-phase mullite are solved, and the problem of low hydrolysis efficiency and long gelation time of single-phase mullite is achieved. Fast gelation and efficient composite preparation.
Patent Information
- Application Number
- CN202411161758.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The hydrolysis efficiency of single-phase mullite sol is low, takes several days, and the gelation process takes more than ten to twenty hours, making it impossible to achieve rapid preparation of composite materials.
Modified polyvinyl alcohol solution is used as the water release agent, and the water required for hydrolysis of aluminum silicon source is provided through temperature control, dilute nitric acid is added as catalyst and pH adjuster, and boric acid is added as gelling in single-phase mullite sol to achieve rapid gelation.
The hydrolysis efficiency of single-phase mullite sol is significantly improved, the preparation cycle is shortened, and hydrolysis and gelation within a few hours is achieved, which improves the rapid preparation ability of composite materials.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of single-phase mullite sol, in particular to a preparation method of single-phase mullite sol and a rapid gelling method thereof. Background Art
[0002] Single-phase mullite sol has a low crystallization temperature and is an ideal matrix raw material for preparing alumina fiber reinforced composite materials. And because single-phase mullite sol can crystallize to form mullite phase below 1100°C, it causes less damage to the preform fiber during the preparation of the composite material. In order to further reduce the damage to the preform fiber, after the preform fiber is impregnated with the matrix sol, the sol is required to gel as soon as possible to achieve rapid preparation of the composite material.
[0003] However, it is difficult to control the hydrolysis rate during the preparation of the single-phase sol. In the prior art, aluminum nitrate nonahydrate and ethyl orthosilicate are usually used as aluminum source and silicon source, respectively, and ethanol is used as a dispersant. The crystal water in aluminum nitrate is used to provide the water source required for hydrolysis to achieve the control of the hydrolysis rate. However, the hydrolysis efficiency of the single-phase mullite sol is low, and it takes several days to hydrolyze. There are few studies on the gelation of single-phase mullite sol. According to the conventional method of heating to promote gelation, it takes more than ten to twenty hours. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a single-phase mullite sol and rapidly gelling the same, which can improve the hydrolysis efficiency of the single-phase mullite sol and achieve rapid gelation of the single-phase mullite sol.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a single-phase mullite sol comprises the following steps: aluminum nitrate pretreatment, aluminum nitrate solution preparation, aluminum silicon mixed solution preparation, single-phase mullite sol preparation, and concentration;
[0007] The aluminum nitrate pretreatment comprises taking aluminum nitrate and treating it at normal pressure and temperature of 60-90° C. until constant weight is obtained to obtain pretreated aluminum nitrate;
[0008] The aluminum nitrate solution is prepared by dissolving the pretreated aluminum nitrate in anhydrous ethanol and stirring until dissolved to obtain an aluminum nitrate solution;
[0009] In the preparation of the aluminum nitrate solution, the mass ratio of the pretreated aluminum nitrate to anhydrous ethanol is 1:10-15;
[0010] The temperature during stirring is 50-80°C;
[0011] The aluminum-silicon mixed solution is prepared by adding tetraethyl orthosilicate into an aluminum nitrate solution and stirring to obtain an aluminum-silicon mixed solution;
[0012] In the preparation of the aluminum-silicon mixed solution, the molar ratio of aluminum nitrate to tetraethyl orthosilicate is 2.8-3.2:1;
[0013] The temperature during stirring is 50-80°C and the time is 5-15 minutes;
[0014] The single-phase mullite sol preparation comprises the following steps: preparing a modified polyvinyl alcohol solution and mixing;
[0015] The modified polyvinyl alcohol solution is prepared by adding a modifier to a polyvinyl alcohol 1788 aqueous solution and stirring to obtain a modified polyvinyl alcohol solution;
[0016] In the preparation of the modified polyvinyl alcohol solution, the mass concentration of the polyvinyl alcohol 1788 aqueous solution is 10-15%;
[0017] The modifier is one or a combination of Tween 20, Tween 40, and nonylphenol polyoxyethylene ether;
[0018] The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.1-0.5%;
[0019] The stirring temperature is 25-40°C and the stirring time is 30-60 minutes;
[0020] The mixture is added with a modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, and then diluted nitric acid is added to adjust the pH to 2.5-5.5, and refluxed at 50-70° C.; heated to 70-90° C. and refluxed; heated to 90-120° C. and refluxed to obtain a transparent single-phase mullite sol stock solution;
[0021] In the mixing, the mass fraction of the modified polyvinyl alcohol solution to the silicon-aluminum mixed solution is 2-6%;
[0022] The molar concentration of the dilute nitric acid is 0.1-0.2 mol / L;
[0023] The addition rate of the dilute nitric acid is 1-3 mL / min;
[0024] The reflux time at 50-70°C is 0.5-1h; the reflux time at 70-90°C is 0.5-1h; the reflux time at 90-120°C is 0.3-0.5h;
[0025] The concentration is to concentrate the transparent single-phase mullite sol stock solution into a single-phase mullite sol by vacuum concentration;
[0026] During the concentration, the vacuum concentration temperature is 40-80° C. and the vacuum degree is 0-0.03 MPa;
[0027] The solid content of the unidirectional mullite sol is 20-35%.
[0028] A method for rapid gelation of a single-phase mullite sol, comprising adding a boric acid aqueous solution to the single-phase mullite sol, stirring at room temperature, heating to 60-120° C., and standing until complete gelation;
[0029] The concentration of the boric acid aqueous solution is 1-2wt%;
[0030] The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 0.5-1%;
[0031] The stirring time is 15-30 minutes.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The present invention introduces a modified polyvinyl alcohol solution as a water-releasing agent, and then gradually provides the water required for the hydrolysis of the aluminum source and the silicon source through temperature control, thereby controlling the reaction rate, shortening the preparation cycle of the single-phase mullite sol to several hours, and realizing stable regulation of the hydrolysis rate; and when the single-phase mullite sol is gelled, boric acid is added as a gelling agent to realize rapid gelation of the sol; dilute nitric acid is also added as a catalyst during the hydrolysis, which can adjust the pH of the aluminum-silicon mixed solution, and is conducive to the formation of a stable single-phase mullite sol within the pH range; on the other hand, the water in the dilute nitric acid can promote the progress of hydrolysis, further shortening the preparation time of the sol;
[0034] (2) The present invention can improve the hydrolysis efficiency of single-phase mullite sol. After adding a modified polyvinyl alcohol solution to an aluminum-silicon mixed solution and adding dilute nitric acid, the solution is refluxed at 50-70°C for 0.5-1h, refluxed at 70-90°C for 0.5-1h, and refluxed at 90-120°C for 0.3-0.5h to achieve hydrolysis and obtain a transparent single-phase mullite sol stock solution.
[0035] (3) The present invention can achieve rapid gelation of single-phase mullite sol. After adding boric acid aqueous solution to the single-phase mullite sol, the mixture is stirred evenly at room temperature, heated to 60-120°C, and stirred for 1-4 hours to achieve complete gelation. DETAILED DESCRIPTION
[0036] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0037] Example 1
[0038] A method for preparing a single-phase mullite sol, specifically comprising:
[0039] 1. Aluminum nitrate pretreatment
[0040] Take aluminum nitrate, treat it at normal pressure and temperature of 60°C until constant weight, and obtain pretreated aluminum nitrate;
[0041] 2. Preparation of Aluminum Nitrate Solution
[0042] The pretreated aluminum nitrate is dissolved in anhydrous ethanol, and stirred at 50° C. until dissolved to obtain an aluminum nitrate solution;
[0043] The mass ratio of aluminum nitrate to anhydrous ethanol after pretreatment is 1:10;
[0044] 3. Preparation of aluminum-silicon mixed solution
[0045] Add ethyl orthosilicate to the aluminum nitrate solution, stir at 50°C for 5 minutes to obtain an aluminum-silicon mixed solution;
[0046] The molar ratio of aluminum nitrate to tetraethyl orthosilicate is 2.8:1;
[0047] 4. Preparation of single-phase mullite sol
[0048] (1) Preparation of modified polyvinyl alcohol solution: add a modifier to a polyvinyl alcohol 1788 aqueous solution and stir at 25°C for 30 minutes to obtain a modified polyvinyl alcohol solution;
[0049] The mass concentration of the polyvinyl alcohol 1788 aqueous solution is 10%;
[0050] The modifier is Tween 20;
[0051] The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.1%;
[0052] (2) Mixing: Add the modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, then slowly add dilute nitric acid to adjust the pH to 2.5, reflux at 50°C for 0.5h; heat to 70°C, reflux for 0.5h; heat to 90°C, reflux for 0.3h, and obtain a transparent single-phase mullite sol solution;
[0053] The mass fraction of the modified polyvinyl alcohol solution in the silicon-aluminum mixed solution is 2%;
[0054] The molar concentration of the dilute nitric acid is 0.1 mol / L;
[0055] The addition rate of the dilute nitric acid is 1 mL / min;
[0056] 5. Concentration
[0057] The transparent single-phase mullite sol stock solution was concentrated by vacuum concentration at a temperature of 40° C. and a vacuum degree of 0 MPa to obtain a single-phase mullite sol with a solid content of 35%.
[0058] A method for rapid gelation of a single-phase mullite sol, specifically comprising: adding a boric acid aqueous solution to the single-phase mullite sol, stirring for 30 minutes at room temperature, heating to 60° C., and standing until complete gelation;
[0059] The mass concentration of the boric acid aqueous solution is 1%;
[0060] The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 0.5%;
[0061] The method for judging complete gelation is: place the container containing the single-phase mullite sol vertically at 90°, and if there is no fluidity, it is completely gelled;
[0062] The time required for complete gelation is 4 h.
[0063] Example 2
[0064] A method for preparing a single-phase mullite sol, specifically comprising:
[0065] 1. Aluminum nitrate pretreatment
[0066] Take aluminum nitrate, treat it at normal pressure and temperature of 70°C until constant weight, and obtain pretreated aluminum nitrate;
[0067] 2. Preparation of Aluminum Nitrate Solution
[0068] Dissolving the pretreated aluminum nitrate in anhydrous ethanol, stirring at 60° C. until dissolved, to obtain an aluminum nitrate solution;
[0069] The mass ratio of aluminum nitrate to anhydrous ethanol after pretreatment is 1:12;
[0070] 3. Preparation of aluminum-silicon mixed solution
[0071] Add ethyl orthosilicate to the aluminum nitrate solution, stir at 80°C for 10 minutes to obtain an aluminum-silicon mixed solution;
[0072] The molar ratio of aluminum nitrate to tetraethyl orthosilicate is 3:1;
[0073] 4. Preparation of single-phase mullite sol
[0074] (1) Preparation of modified polyvinyl alcohol solution: add a modifier to a polyvinyl alcohol 1788 aqueous solution and stir at 30°C for 40 minutes to obtain a modified polyvinyl alcohol solution;
[0075] The mass concentration of the polyvinyl alcohol 1788 aqueous solution is 12%;
[0076] The modifier is Tween 40;
[0077] The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.4%;
[0078] (2) Mixing: Add the modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, then slowly add dilute nitric acid to adjust the pH to 3, reflux at 60°C for 0.7h; heat to 80°C, reflux for 0.7h; heat to 100°C, reflux for 0.4h, and obtain a transparent single-phase mullite sol solution;
[0079] The mass fraction of the modified polyvinyl alcohol solution in the silicon-aluminum mixed solution is 3%;
[0080] The molar concentration of the dilute nitric acid is 0.1 mol / L;
[0081] The addition rate of the dilute nitric acid is 2 mL / min;
[0082] 5. Concentration
[0083] The transparent single-phase mullite sol stock solution was concentrated by vacuum concentration at a temperature of 50° C. and a vacuum degree of 0.01 MPa to obtain a single-phase mullite sol with a solid content of 20%.
[0084] A method for rapid gelation of a single-phase mullite sol comprises: adding a boric acid aqueous solution to the single-phase mullite sol, stirring for 15 minutes at room temperature, heating to 60° C., and standing until complete gelation.
[0085] The mass concentration of the boric acid aqueous solution is 2%;
[0086] The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 1%;
[0087] The method for judging complete gelation is: place the container containing the single-phase mullite sol vertically at 90°, and if there is no fluidity, it is completely gelled.
[0088] The time required for complete gelation is 3 h.
[0089] Example 3
[0090] A method for preparing a single-phase mullite sol, specifically comprising:
[0091] 1. Aluminum nitrate pretreatment
[0092] Take aluminum nitrate, treat it at normal pressure and temperature of 80°C until constant weight, and obtain pretreated aluminum nitrate;
[0093] 2. Preparation of Aluminum Nitrate Solution
[0094] The pretreated aluminum nitrate is dissolved in anhydrous ethanol, and stirred at 70° C. until dissolved to obtain an aluminum nitrate solution;
[0095] The mass ratio of aluminum nitrate to anhydrous ethanol after pretreatment is 1:14;
[0096] 3. Preparation of aluminum-silicon mixed solution
[0097] Add ethyl orthosilicate to the aluminum nitrate solution, stir at 70°C for 12 minutes to obtain an aluminum-silicon mixed solution;
[0098] The molar ratio of aluminum nitrate to tetraethyl orthosilicate is 3.1:1;
[0099] 4. Preparation of single-phase mullite sol
[0100] (1) Preparation of modified polyvinyl alcohol solution: add a modifier to a polyvinyl alcohol 1788 aqueous solution and stir at 35°C for 50 minutes to obtain a modified polyvinyl alcohol solution;
[0101] The mass concentration of the polyvinyl alcohol 1788 aqueous solution is 14%;
[0102] The modifier is nonylphenol polyoxyethylene ether;
[0103] The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.3%;
[0104] (2) Mixing: Add the modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, then slowly add dilute nitric acid to adjust the pH to 5, reflux at 65°C for 0.8h; heat to 85°C, reflux for 0.8h; heat to 110°C, reflux for 0.4h, and obtain a transparent single-phase mullite sol solution;
[0105] The mass fraction of the modified polyvinyl alcohol solution in the silicon-aluminum mixed solution is 5%;
[0106] The molar concentration of the dilute nitric acid is 0.15 mol / L;
[0107] The addition rate of the dilute nitric acid is 3 mL / min;
[0108] 5. Concentration
[0109] The transparent single-phase mullite sol stock solution was concentrated by vacuum concentration at a temperature of 70° C. and a vacuum degree of 0.02 MPa to obtain a single-phase mullite sol with a solid content of 35%.
[0110] A method for rapid gelation of a single-phase mullite sol comprises: adding a boric acid aqueous solution to the single-phase mullite sol, stirring for 20 minutes at room temperature, heating to 120° C., and standing until complete gelation.
[0111] The mass concentration of the boric acid aqueous solution is 1%;
[0112] The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 0.5%;
[0113] The method for judging complete gelation is: place the container containing the single-phase mullite sol vertically at 90°, and if there is no fluidity, it is completely gelled.
[0114] The time required for complete gelation is 2 h.
[0115] Example 4
[0116] A method for preparing a single-phase mullite sol, specifically comprising:
[0117] 1. Aluminum nitrate pretreatment
[0118] Taking aluminum nitrate, treating it under normal pressure and temperature of 90° C. until it reaches a constant weight, to obtain pretreated aluminum nitrate;
[0119] 2. Preparation of Aluminum Nitrate Solution
[0120] The pretreated aluminum nitrate is dissolved in anhydrous ethanol, and stirred at 80° C. until dissolved to obtain an aluminum nitrate solution;
[0121] The mass ratio of the pretreated aluminum nitrate to anhydrous ethanol is 1:15.
[0122] 3. Preparation of aluminum-silicon mixed solution
[0123] Add ethyl orthosilicate to the aluminum nitrate solution, stir at 80°C for 15 minutes to obtain an aluminum-silicon mixed solution;
[0124] The molar ratio of aluminum nitrate to tetraethyl orthosilicate is 3.2:1;
[0125] 4. Preparation of single-phase mullite sol
[0126] (1) Preparation of modified polyvinyl alcohol solution: Add a modifier to a polyvinyl alcohol 1788 aqueous solution with a mass concentration of 15%, and stir at 40°C for 60 minutes to obtain a modified polyvinyl alcohol solution;
[0127] The mass concentration of the polyvinyl alcohol 1788 aqueous solution is 15%;
[0128] The modifier is a mixture of Tween 20 and nonylphenol polyoxyethylene ether, wherein the mass ratio of Tween 20 to nonylphenol polyoxyethylene ether is 1:1;
[0129] The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.5%;
[0130] (2) Mixing: Add the modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, then slowly add dilute nitric acid to adjust the pH to 5.5, reflux at 70°C for 1 hour; heat to 90°C, reflux for 1 hour; heat to 120°C, reflux for 0.5 hour, and obtain a transparent single-phase mullite sol solution;
[0131] The mass fraction of the modified polyvinyl alcohol solution in the silicon-aluminum mixed solution is 6%;
[0132] The molar concentration of the dilute nitric acid is 0.2 mol / L;
[0133] The addition rate of the dilute nitric acid is 3 mL / min;
[0134] 5. Concentration
[0135] The transparent single-phase mullite sol stock solution was concentrated by vacuum concentration at a temperature of 80° C. and a vacuum degree of 0.03 MPa to obtain a single-phase mullite sol with a solid content of 20%.
[0136] A method for rapid gelation of a single-phase mullite sol comprises: adding a boric acid aqueous solution to the single-phase mullite sol, stirring for 20 minutes at room temperature, heating to 120° C., and standing until complete gelation.
[0137] The mass concentration of the boric acid aqueous solution is 2%;
[0138] The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 1%;
[0139] The method for judging complete gelation is: place the container containing the single-phase mullite sol vertically at 90°, and if there is no fluidity, it is completely gelled.
[0140] The time required for complete gelation was 1 h.
[0141] Comparative Example 1
[0142] On the basis of Example 1, in the preparation of the single-phase mullite sol, the first step of aluminum nitrate pretreatment is omitted, that is, the aluminum nitrate that has not been pretreated is directly used in the second step of aluminum nitrate solution preparation;
[0143] and omitting the step (1) of preparing the modified polyvinyl alcohol solution in the fourth step of preparing the single-phase mullite sol, and correspondingly omitting the addition of the modified polyvinyl alcohol solution in the second step of mixing;
[0144] The remaining operations are the same as those in Example 1.
[0145] In the mixing step (2) of the fourth step of preparing the single-phase mullite sol in this comparative example, after the temperature is raised to 90° C., a total of 6 days of reflux are required to obtain a transparent single-phase mullite sol stock solution.
[0146] Comparative Example 2
[0147] On the basis of Example 1, in the method for rapid gelation of single-phase mullite sol, the addition of boric acid aqueous solution is omitted;
[0148] The remaining operations are the same as those in Example 1.
[0149] The time required for complete gelation is 20 h.
[0150] Comparative Example 3
[0151] Based on Example 1, the following adjustments are made: in the fourth step of preparing the single-phase mullite sol, the addition of dilute nitric acid is omitted in the mixing step (2);
[0152] The remaining operations are the same as those in Example 1.
[0153] In this comparative example, a transparent single-phase mullite sol stock solution could not be obtained in the fourth step of preparing the single-phase mullite sol.
[0154] Unless otherwise specified, all percentages used in the present invention are by mass.
[0155] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a single-phase mullite sol, characterized in that: The method comprises the following steps: aluminum nitrate pretreatment, aluminum nitrate solution preparation, aluminum silicon mixed solution preparation, single-phase mullite sol preparation, and concentration; The aluminum nitrate pretreatment comprises taking aluminum nitrate and treating it at normal pressure and temperature of 60-90° C. until constant weight is obtained to obtain pretreated aluminum nitrate; The aluminum-silicon mixed solution is prepared by adding tetraethyl orthosilicate into an aluminum nitrate solution and stirring to obtain an aluminum-silicon mixed solution; In the preparation of the aluminum-silicon mixed solution, the molar ratio of aluminum nitrate to tetraethyl orthosilicate is 2.8-3.2:1; The single-phase mullite sol preparation comprises the following steps: preparing a modified polyvinyl alcohol solution and mixing; The modified polyvinyl alcohol solution is prepared by adding a modifier to a polyvinyl alcohol 1788 aqueous solution and stirring to obtain a modified polyvinyl alcohol solution; The mixture is added with a modified polyvinyl alcohol solution to the aluminum-silicon mixed solution, and then diluted nitric acid is added to adjust the pH to 2.5-5.5, and refluxed at 50-70° C. for 0.5-1 h; the mixture is heated to 70-90° C., and refluxed at 70-90° C. for 0.5-1 h; the mixture is heated to 90-120° C., and refluxed at 90-120° C. for 0.3-0.5 h to obtain a transparent single-phase mullite sol stock solution; In the mixing, the mass fraction of the modified polyvinyl alcohol solution in the silicon-aluminum mixed solution is 2-6%.
2. The method for preparing a single-phase mullite sol according to claim 1, characterized in that: The aluminum nitrate solution is prepared by dissolving the pretreated aluminum nitrate in anhydrous ethanol and stirring until dissolved to obtain an aluminum nitrate solution; In the preparation of the aluminum nitrate solution, the mass ratio of the pretreated aluminum nitrate to anhydrous ethanol is 1:10-15; The temperature during stirring is 50-80°C.
3. The method for preparing the single-phase mullite sol according to claim 1, characterized in that: During the preparation of the aluminum-silicon mixed solution, the stirring temperature is 50-80° C. and the stirring time is 5-15 minutes.
4. The method for preparing the single-phase mullite sol according to claim 1, characterized in that: In the preparation of the modified polyvinyl alcohol solution, the mass concentration of the polyvinyl alcohol 1788 aqueous solution is 10-15%; The modifier is one or a combination of Tween 20, Tween 40, and nonylphenol polyoxyethylene ether; The mass fraction of the modifier in the polyvinyl alcohol 1788 aqueous solution is 0.1-0.5%; The stirring temperature is 25-40°C and the stirring time is 30-60 minutes.
5. The method for preparing the single-phase mullite sol according to claim 1, characterized in that: In the mixing, the molar concentration of the dilute nitric acid is 0.1-0.2 mol / L; The addition rate of the dilute nitric acid is 1-3 mL / min.
6. The method for preparing the single-phase mullite sol according to claim 1, characterized in that: The concentration is to concentrate the transparent single-phase mullite sol stock solution into a single-phase mullite sol by vacuum concentration; During the concentration, the vacuum concentration temperature is 40-80° C. and the vacuum degree is 0-0.03 MPa; The solid content of the unidirectional mullite sol is 20-35%.
7. A method for rapid gelation of a single-phase mullite sol obtained by the preparation method according to any one of claims 1 to 6, characterized in that: Add boric acid aqueous solution to the single-phase mullite sol, stir at room temperature, heat to 60-120°C, and let stand until complete gelation.
8. The method for rapid gelation of single-phase mullite sol according to claim 7, characterized in that: The concentration of the boric acid aqueous solution is 1-2wt%; The mass fraction of the boric acid aqueous solution in the single-phase mullite sol is 0.5-1%; The stirring time is 15-30 minutes.