Environmentally friendly water-based high and low temperature membrane and preparation method thereof

By combining the TPU base film, glue layer body and water-based coating, the stability and thermal insulation performance of TPU high and low temperature films under high and low temperature, ultraviolet and acid-corrosion conditions are solved by using multiple adjustments to improve the stabilization agent and nanomaterial. , achieves the coordination between flame retardant and thermal insulation.

CN118684928BActive Publication Date: 2024-11-26QUANZHOU SIMDA GARMENTS & SHOES MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411165121.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing TPU high and low temperature films have poor insulation performance under high and low temperature conditions, and the flame retardant performance is difficult to coordinate with insulation and heat insulation, and the stability is insufficient under ultraviolet and acid corrosion conditions.

Method used

The TPU base film is combined with the glue layer body and the water-based coating. The glue layer is composed of a stabilizer based on multiple adjustment improvements, silane coupling agent, epoxy resin and polyurethane adhesive. The water-based coating contains the coating matrix agent. , magnesium hydroxide, glass beads and doped nanosilicon dioxide enhance material properties through specific heat treatment and ultrasonic modification treatment.

Benefits of technology

It significantly improves the flame retardant, thermal insulation coordination of the product, and significantly improves the stability under high and low temperatures, ultraviolet and acid corrosion conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of TPU films, and specifically to an environmentally friendly water-based high and low temperature film and a preparation method thereof, comprising a TPU base film, wherein the TPU base film is immersed in a glue liquid agent to form a glue layer body, and the glue layer body is coated with a water-based coating agent to form a water-based coating layer, wherein the water-based coating layer, the glue layer body and the TPU base film are arranged in sequence from top to bottom. The environmentally friendly water-based high and low temperature film of the present invention is made by arranging a TPU base film, a glue layer body and a water-based coating layer in sequence, wherein the glue layer body is formed by immersing the TPU base film in a glue liquid agent, wherein the glue liquid agent is blended with a stabilizer based on multi-adjustment improvement, a silane coupling agent KH560, an epoxy resin, a polyurethane adhesive and an ethanol raw material, and at the same time, the water-based coating agent is blended with a coating base agent, magnesium hydroxide, glass microbeads and a modified agent doped with nano-silicon dioxide, and magnesium hydroxide and glass microbeads are used as functional additives to enhance the flame retardant and thermal insulation properties of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TPU films, and in particular to an environmentally friendly water-based high and low temperature film and a preparation method thereof. Background Art

[0002] Thermoplastic polyurethane (TPU) is a linear block polymer composed of chain extenders, diisocyanates, and polyols. The modulus of TPU is between that of plastic and rubber, so it has both plasticity and elasticity. It has excellent mechanical properties, excellent cold resistance, high wear resistance, oil resistance, and ozone resistance. It has been widely used in medical treatment, equipment, light industry, etc.

[0003] Although the existing TPU high and low temperature films can withstand high and low temperatures, they easily lead to poor thermal insulation performance of the product, and it is difficult to coordinate and improve the flame retardant and thermal insulation performance of the product. At the same time, the product has poor stability under ultraviolet and acid corrosion conditions, which further limits the product's use efficiency. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide an environmentally friendly aqueous high and low temperature membrane and a preparation method thereof to solve the problems raised in the above background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution:

[0006] The present invention provides an environmentally friendly water-based high and low temperature film, comprising a TPU base film, wherein the TPU base film is immersed in a glue liquid to form a glue layer, and a water-based coating is coated on the glue layer to form a water-based coating, wherein the water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom;

[0007] The thickness of the TPU base film is 10-15 mm, the thickness of the adhesive layer is 2-5 mm, and the thickness of the water-based coating is 1-3 mm;

[0008] The adhesive comprises the following raw materials in parts by weight: 7-11 parts of a stabilizer based on multi-adjustment improvement, 2-5 parts of a silane coupling agent KH560, 4-7 parts of an epoxy resin, 8-12 parts of a polyurethane adhesive, and 8-10 parts of ethanol;

[0009] The water-based coating comprises the following raw materials in parts by weight: 25-30 parts of a coating base agent, 4-7 parts of magnesium hydroxide, 3-5 parts of glass microbeads, and 4-6 parts of a modifier doped with nano-silicon dioxide.

[0010] Preferably, the coating base agent is prepared from epoxy resin with a weight average molecular weight of 5000-6000, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1.

[0011] Preferably, the preparation method of the stabilizer based on multi-adjustment improvement is:

[0012] S01: Preparation of nano-attapulgite liquid:

[0013] S011: heat treating the nano-attapulgite at 130-150° C. for 10-15 min;

[0014] S012: then heating to 230-250°C at a rate of 2-5°C / min, keeping the temperature for 5-10min, and then cooling to 55°C at a rate of 1-3°C / min, keeping the temperature, to obtain heat-treated nano-attapulgite;

[0015] S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid;

[0016] S02: The multi-adjustable stabilizer and nano-attapulgite liquid are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizer improved based on multi-adjustable.

[0017] Preferably, the mass fraction of the sodium alginate solution is 4-7%; and the pH value of the phosphate buffer solution is 5.5.

[0018] Preferably, the preparation method of the multi-adjusting stabilizer is:

[0019] 5-8 parts of silicon carbide whiskers, 1-3 parts of yttrium oxide, and 2-5 parts of sodium dodecylbenzene sulfonate solution are evenly mixed, and then 2-4 parts of boron nitride and 1-2 parts of stearic acid are added and mixed for ball milling. The ball milling speed is 1500-1700r / min, and the ball milling is performed for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a multi-adjustable stabilizer.

[0020] Preferably, the mass fraction of the sodium dodecylbenzene sulfonate solution is 4-7%.

[0021] Preferably, the preparation method of the nano-silicon dioxide-doped modifier is:

[0022] S11: 2-5 parts of lanthanum nitrate solution, 1-3 parts of nano-silica sol and 4-7 parts of 4% chitosan solution are uniformly mixed to obtain a modified solution A;

[0023] S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes;

[0024] 4-7 parts of dried flake graphene, 1-3 parts of silane coupling agent KH560 and 2-4 parts of sodium lignin sulfonate solution are fully mixed to obtain a modified solution B;

[0025] S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 2:(5-7) to obtain a modified blending agent;

[0026] The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

[0027] Preferably, the mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.

[0028] Preferably, the ultrasonic power of the first ultrasonic modification treatment is 450-550 W, and the ultrasonic time is 20-30 min; the ultrasonic power of the second ultrasonic modification treatment is 300-350 W, and the ultrasonic time is 45-55 min.

[0029] The present invention also provides a method for preparing an environmentally friendly aqueous high and low temperature membrane, comprising the following steps:

[0030] Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution;

[0031] Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent;

[0032] Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The environmentally friendly water-based high and low temperature film of the present invention is prepared by sequentially arranging a TPU base film, a glue layer body, and a water-based coating. The glue layer body is formed by immersing a TPU base film in a glue liquid agent. The glue liquid agent is blended with a stabilizer based on multi-adjustment improvement, a silane coupling agent KH560, an epoxy resin, a polyurethane adhesive, and an ethanol raw material. At the same time, the water-based coating agent is blended with a coating base agent, magnesium hydroxide, glass microbeads, and a modifier doped with nano-silicon dioxide. Magnesium hydroxide and glass microbeads are used as functional additives to enhance the flame retardancy and thermal insulation performance of the product. At the same time, the modifier doped with nano-silicon dioxide and the stabilizer based on multi-adjustment improvement are coordinated and synergistic, so that the flame retardancy and thermal insulation coordination of the product are enhanced, and the product has a significant stability effect under ultraviolet and acid corrosion conditions, and the product has significant high and low temperature stability performance;

[0035] 2. Based on the multi-adjustment improved stabilizer, nano-attapulgite is heat-treated at 130-150°C for 10-15min; then the temperature is raised to 230-250°C at a rate of 2-5°C / min, kept warm for 5-10min, and then cooled to 55°C at a rate of 1-3°C / min, kept warm, and segmented thermal improvement is used to optimize the activity efficiency of the nano-attapulgite and enhance the interlamellar spacing of the nano-attapulgite, and then the dispersibility of the nano-attapulgite prepared by mixing sodium alginate solution and phosphate buffer solution is enhanced, and the coordination of the multi-adjustment stabilizer and the nano-attapulgite is further enhanced and improved, so that the performance of the product is further improved;

[0036] 3. The multi-adjusting stabilizer uses silicon carbide whiskers as the matrix, and is evenly blended with yttrium oxide and sodium dodecylbenzene sulfonate solution, and then boron nitride and stearic acid are added for blending and ball milling. The raw materials in the multi-adjusting stabilizer are coordinated and blended with the whisker-like structure of silicon carbide whiskers to coordinate with raw materials such as boron nitride, thereby coordinating and improving nano-attapulgite. Through the coordination between the raw materials, the performance effect of the system product is further enhanced. The stabilizer based on the multi-adjusting improvement is used as the main material of the gel layer. The use of a lamellar structure can enhance the barrier stability of the system, thereby optimizing the product's stability under ultraviolet and acid corrosion conditions and high and low temperature resistance.

[0037] 4. The nano-silica doped modifier is prepared by uniformly mixing lanthanum nitrate solution, nano-silica sol and 4% by mass chitosan solution to obtain a modifier A, wherein the flaky graphene is firstly stirred and uniformly mixed in a sufficient amount of 5% by mass potassium permanganate solution to enhance the activity of the flaky graphene, and the silane coupling agent KH560 and the sodium lignin sulfonate solution are fully blended to obtain a modifier B, and a modifier blend is obtained by blending and coordinating the modifiers A and B, wherein flaky graphene is used as a flaky co-combining structure, nano-silica is coordinated and coordinated, and nano-silica with a high specific surface area is used as a synergistic modifier blend, thereby enhancing the interface compatibility between the raw materials, thereby enhancing the flame retardancy and thermal insulation of the product, and further reinforcing the adhesive layer of the water-based coating with the nano-silica doped modifier as the main material, thereby further improving the product performance. DETAILED DESCRIPTION

[0038] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] An environmentally friendly water-based high and low temperature film of this embodiment includes a TPU base film, the TPU base film is immersed in a glue liquid to form a glue layer, the glue layer is coated with a water-based coating to form a water-based coating, and the water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom;

[0040] The thickness of the TPU base film is 10-15 mm, the thickness of the adhesive layer is 2-5 mm, and the thickness of the water-based coating is 1-3 mm;

[0041] The adhesive comprises the following raw materials in parts by weight: 7-11 parts of a stabilizer based on multi-adjustment improvement, 2-5 parts of a silane coupling agent KH560, 4-7 parts of an epoxy resin, 8-12 parts of a polyurethane adhesive, and 8-10 parts of ethanol;

[0042] The water-based coating comprises the following raw materials in parts by weight: 25-30 parts of a coating base agent, 4-7 parts of magnesium hydroxide, 3-5 parts of glass microbeads, and 4-6 parts of a modifier doped with nano-silicon dioxide.

[0043] The coating base agent of this embodiment is prepared by epoxy resin with a weight average molecular weight of 5000-6000, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1.

[0044] The preparation method of the stabilizer based on multi-adjustment improvement in this embodiment is:

[0045] S01: Preparation of nano-attapulgite liquid:

[0046] S011: heat treating the nano-attapulgite at 130-150° C. for 10-15 min;

[0047] S012: then heating to 230-250°C at a rate of 2-5°C / min, keeping the temperature for 5-10min, and then cooling to 55°C at a rate of 1-3°C / min, keeping the temperature, to obtain heat-treated nano-attapulgite;

[0048] S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid;

[0049] S02: The multi-adjustable stabilizer and nano-attapulgite liquid are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizer improved based on multi-adjustable.

[0050] The mass fraction of the sodium alginate solution in this embodiment is 4-7%; the pH value of the phosphate buffer solution is 5.5.

[0051] The preparation method of the multi-adjustable stabilizer of this embodiment is:

[0052] 5-8 parts of silicon carbide whiskers, 1-3 parts of yttrium oxide, and 2-5 parts of sodium dodecylbenzene sulfonate solution are evenly mixed, and then 2-4 parts of boron nitride and 1-2 parts of stearic acid are added and mixed for ball milling. The ball milling speed is 1500-1700r / min, and the ball milling is performed for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a multi-adjustable stabilizer.

[0053] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 4-7%.

[0054] The preparation method of the nano-silicon dioxide-doped modifier of this embodiment is as follows:

[0055] S11: 2-5 parts of lanthanum nitrate solution, 1-3 parts of nano-silica sol and 4-7 parts of 4% chitosan solution are uniformly mixed to obtain a modified solution A;

[0056] S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes;

[0057] 4-7 parts of dried flake graphene, 1-3 parts of silane coupling agent KH560 and 2-4 parts of sodium lignin sulfonate solution are fully mixed to obtain a modified solution B;

[0058] S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 2:(5-7) to obtain a modified blending agent;

[0059] The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

[0060] The mass fraction of the lanthanum nitrate solution in this embodiment is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.

[0061] In the first ultrasonic modification treatment of this embodiment, the ultrasonic power is 450-550W, and the ultrasonic time is 20-30min; the ultrasonic power of the second ultrasonic modification treatment is 300-350W, and the ultrasonic time is 45-55min.

[0062] The method for preparing an environmentally friendly aqueous high and low temperature membrane of this embodiment comprises the following steps:

[0063] Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution;

[0064] Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent;

[0065] Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.

[0066] Embodiment 1: An environmentally friendly water-based high and low temperature film, comprising a TPU base film, wherein the TPU base film is immersed in a glue liquid to form a glue layer, and a water-based coating is coated on the glue layer to form a water-based coating, wherein the water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom;

[0067] The thickness of the TPU base film is 10 mm, the thickness of the adhesive layer is 2 mm, and the thickness of the water-based coating is 1 mm;

[0068] The adhesive comprises the following raw materials in parts by weight: 7 parts of a stabilizer based on multi-adjustment improvement, 2 parts of a silane coupling agent KH560, 4 parts of an epoxy resin, 8 parts of a polyurethane adhesive, and 8 parts of ethanol;

[0069] The water-based coating comprises the following raw materials in parts by weight: 25 parts of coating base agent, 4 parts of magnesium hydroxide, 3 parts of glass microbeads, and 4 parts of a modifying agent doped with nano-silicon dioxide.

[0070] The coating base agent of this embodiment is prepared by epoxy resin with a weight average molecular weight of 5000, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1.

[0071] The preparation method of the stabilizer based on multi-adjustment improvement in this embodiment is:

[0072] S01: Preparation of nano-attapulgite liquid:

[0073] S011: heat treating the nano-attapulgite at 130°C for 10 min;

[0074] S012: then heat to 230°C at a rate of 2°C / min, keep warm for 5 min, then cool to 55°C at a rate of 1°C / min, keep warm;

[0075] S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid;

[0076] S02: The multi-adjustable stabilizer and nano-attapulgite liquid are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizer based on multi-adjustable improvement.

[0077] The mass fraction of the sodium alginate solution in this embodiment is 4%; the pH value of the phosphate buffer solution is 5.5.

[0078] The preparation method of the multi-adjustable stabilizer of this embodiment is:

[0079] 5 parts of silicon carbide whiskers, 1 part of yttrium oxide, and 2 parts of sodium dodecylbenzene sulfonate solution are mixed evenly, and then 2 parts of boron nitride and 1 part of stearic acid are added and mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a multi-adjustable stabilizer.

[0080] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 4%.

[0081] The preparation method of the nano-silicon dioxide-doped modifier of this embodiment is as follows:

[0082] S11: 2 parts of lanthanum nitrate solution, 1 part of nano-silica sol and 4 parts of 4% chitosan solution are mixed evenly to obtain a modified solution A;

[0083] S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes;

[0084] 4 parts of dried flake graphene, 1 part of silane coupling agent KH560 and 2 parts of sodium lignin sulfonate solution were fully mixed to obtain a modified solution B;

[0085] S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 2:5 to obtain a modified blending agent;

[0086] The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

[0087] The mass fraction of the lanthanum nitrate solution in this embodiment is 2%; the mass fraction of the sodium lignin sulfonate solution is 3%.

[0088] In the present embodiment, the ultrasonic power of the first ultrasonic modification treatment is 450 W, and the ultrasonic time is 20 min; the ultrasonic power of the second ultrasonic modification treatment is 300 W, and the ultrasonic time is 45 min.

[0089] The method for preparing an environmentally friendly aqueous high and low temperature membrane of this embodiment comprises the following steps:

[0090] Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution;

[0091] Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent;

[0092] Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.

[0093] Embodiment 2: An environmentally friendly water-based high and low temperature film, comprising a TPU base film, wherein the TPU base film is immersed in a glue liquid to form a glue layer, and a water-based coating is coated on the glue layer to form a water-based coating, wherein the water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom;

[0094] The thickness of the TPU base film is 15 mm, the thickness of the adhesive layer is 5 mm, and the thickness of the water-based coating is 3 mm;

[0095] The adhesive comprises the following raw materials in parts by weight: 11 parts of a stabilizer based on multi-adjustment improvement, 5 parts of a silane coupling agent KH560, 7 parts of an epoxy resin, 12 parts of a polyurethane adhesive, and 10 parts of ethanol;

[0096] The water-based coating comprises the following raw materials in parts by weight: 30 parts of coating base agent, 7 parts of magnesium hydroxide, 5 parts of glass microspheres, and 6 parts of a modifying agent doped with nano-silicon dioxide.

[0097] The coating base agent of this embodiment is prepared by epoxy resin with a weight average molecular weight of 6000, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1.

[0098] The preparation method of the stabilizer based on multi-adjustment improvement in this embodiment is:

[0099] S01: Preparation of nano-attapulgite liquid:

[0100] S011: heat treating the nano-attapulgite at 150°C for 15 min;

[0101] S012: then heating to 250°C at a rate of 5°C / min, keeping the temperature for 10 minutes, and then cooling to 55°C at a rate of 3°C / min, keeping the temperature, to obtain heat-treated nano-attapulgite;

[0102] S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid;

[0103] S02: The multi-adjustable stabilizer and nano-attapulgite liquid are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizer based on multi-adjustable improvement.

[0104] The mass fraction of the sodium alginate solution in this embodiment is 7%; the pH value of the phosphate buffer solution is 5.5.

[0105] The preparation method of the multi-adjustable stabilizer of this embodiment is:

[0106] 8 parts of silicon carbide whiskers, 3 parts of yttrium oxide, and 5 parts of sodium dodecylbenzene sulfonate solution were evenly mixed, and then 4 parts of boron nitride and 2 parts of stearic acid were added and ball-milled at a speed of 1700 r / min for 2 hours. After the ball milling was completed, the mixture was washed with water and dried to obtain a multi-adjustable stabilizer.

[0107] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 7%.

[0108] The preparation method of the nano-silicon dioxide-doped modifier of this embodiment is as follows:

[0109] S11: 5 parts of lanthanum nitrate solution, 3 parts of nano-silica sol and 7 parts of 4% chitosan solution are mixed evenly to obtain a modified solution A;

[0110] S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes;

[0111] 7 parts of dried flake graphene, 3 parts of silane coupling agent KH560 and 4 parts of sodium lignin sulfonate solution were fully mixed to obtain a modified solution B;

[0112] S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 2:7 to obtain a modified blending agent;

[0113] The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

[0114] The mass fraction of the lanthanum nitrate solution in this embodiment is 5%; the mass fraction of the sodium lignin sulfonate solution is 6%.

[0115] In this embodiment, the ultrasonic power of the first ultrasonic modification treatment is 550 W, and the ultrasonic time is 30 min; the ultrasonic power of the second ultrasonic modification treatment is 350 W, and the ultrasonic time is 55 min.

[0116] The method for preparing an environmentally friendly aqueous high and low temperature membrane of this embodiment comprises the following steps:

[0117] Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution;

[0118] Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent;

[0119] Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.

[0120] Embodiment 3: An environmentally friendly water-based high and low temperature film, comprising a TPU base film, wherein the TPU base film is immersed in a glue liquid to form a glue layer, and a water-based coating is coated on the glue layer to form a water-based coating, wherein the water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom;

[0121] The thickness of the TPU base film is 12.5 mm, the thickness of the adhesive layer is 3.5 mm, and the thickness of the water-based coating is 2 mm;

[0122] The adhesive comprises the following raw materials in parts by weight: 8.5 parts of a stabilizer based on multi-adjustment improvement, 3.5 parts of a silane coupling agent KH560, 5.5 parts of an epoxy resin, 10 parts of a polyurethane adhesive, and 9 parts of ethanol;

[0123] The water-based coating comprises the following raw materials in parts by weight: 27.5 parts of coating base agent, 5.5 parts of magnesium hydroxide, 4 parts of glass microspheres, and 5 parts of a modifying agent doped with nano-silicon dioxide.

[0124] The coating base agent of this embodiment is prepared by epoxy resin with a weight average molecular weight of 5500, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1.

[0125] The preparation method of the stabilizer based on multi-adjustment improvement in this embodiment is:

[0126] S01: Preparation of nano-attapulgite liquid:

[0127] S011: heat treating the nano-attapulgite at 140°C for 12.5 min;

[0128] S012: then heating to 240°C at a rate of 3.5°C / min, keeping the temperature for 7.5min, and then cooling to 55°C at a rate of 2°C / min, keeping the temperature, to obtain heat-treated nano-attapulgite;

[0129] S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid;

[0130] S02: The multi-adjustable stabilizer and nano-attapulgite liquid are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1250 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizer based on multi-adjustable improvement.

[0131] The mass fraction of the sodium alginate solution in this embodiment is 5.5%; the pH value of the phosphate buffer solution is 5.5.

[0132] The preparation method of the multi-adjustable stabilizer of this embodiment is:

[0133] 6.5 parts of silicon carbide whiskers, 2 parts of yttrium oxide, and 3.5 parts of sodium dodecylbenzene sulfonate solution were evenly mixed, and then 3 parts of boron nitride and 1.5 parts of stearic acid were added and mixed and ball-milled at a speed of 1600 r / min for 2 hours. After the ball milling was completed, the mixture was washed with water and dried to obtain a multi-adjustable stabilizer.

[0134] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 5.5%.

[0135] The preparation method of the nano-silicon dioxide-doped modifier of this embodiment is as follows:

[0136] S11: 3.5 parts of lanthanum nitrate solution, 2 parts of nano-silica sol and 5.5 parts of 4% chitosan solution are uniformly mixed to obtain a modified solution A;

[0137] S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes;

[0138] 5.5 parts of dried flake graphene, 2 parts of silane coupling agent KH560 and 3 parts of sodium lignin sulfonate solution were fully mixed to obtain a modified solution B;

[0139] S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 1:3 to obtain a modified blending agent;

[0140] The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

[0141] The mass fraction of the lanthanum nitrate solution in this embodiment is 3.5%; the mass fraction of the sodium lignin sulfonate solution is 4.5%.

[0142] In the present embodiment, the ultrasonic power of the first ultrasonic modification treatment is 500 W, and the ultrasonic time is 25 min; the ultrasonic power of the second ultrasonic modification treatment is 320 W, and the ultrasonic time is 50 min.

[0143] The method for preparing an environmentally friendly aqueous high and low temperature membrane of this embodiment comprises the following steps:

[0144] Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution;

[0145] Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent;

[0146] Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.

[0147] Comparative Example 1:

[0148] The difference from Example 3 is that no stabilizer based on multi-adjustment improvement is added.

[0149] Comparative Example 2:

[0150] The difference from Example 3 is that the nano-attapulgite liquid treatment is not used in the preparation of the stabilizer based on multi-adjustment improvement.

[0151] Comparative Example 3:

[0152] The difference from Example 3 is that the nano-attapulgite liquid is not treated with S011 and S012.

[0153] Comparative Example 4:

[0154] The difference from Example 3 is that the multi-adjustment stabilizer treatment is not used in the preparation of the multi-adjustment improved stabilizer.

[0155] Comparative Example 5:

[0156] The difference from Example 3 is that no modifying agent of doped nano-silicon dioxide is added.

[0157] Comparative Example 6:

[0158] The difference from Example 3 is that the modifying agent is not treated with a modifying blending agent in the preparation of the modifying agent doped with nano-silicon dioxide.

[0159] Comparative Example 7:

[0160] The difference from Example 3 is that the adjusting liquid B is not added to the adjusting blending agent.

[0161] Comparative Example 8:

[0162] The difference from Example 3 is that the adjusting liquid A is not added to the adjusting blending agent.

[0163] Comparative Example 9:

[0164] The difference from Example 3 is that no dry flaky graphene is added to the modified solution B.

[0165] The products of Examples 1-3 and Comparative Examples 1-9 were placed under normal conditions to test flame retardancy and thermal insulation. At the same time, the products were treated at 65°C for 12 hours, then placed at -5°C for 12 hours, and the products were repeatedly tested 5 times to test the high and low temperature stability of the products; and the products were irradiated under ultraviolet conditions with a light intensity of 0.5W / m2 and a wavelength of 340nm for 12 hours. After the irradiation, the products were placed under 2% hydrochloric acid mist conditions for 12 hours, and the tests were repeated 5 times to test the acid corrosion resistance and ultraviolet stability of the products; the product performance test results are shown in Table 1.

[0166] Table 1: Product performance test results of Examples 1-3 and Comparative Examples 1-9

[0167]

[0168] It can be concluded from Table 1 that the product of Example 3 of the present invention has excellent thermal conductivity and limiting oxygen index under normal conditions, and the thermal insulation and flame retardancy of the product can be coordinated and improved. At the same time, the product has significant performance stability under high and low temperature conditions and UV resistance and acid corrosion conditions;

[0169] The product does not add any of the stabilizers based on multi-adjustment improvement or the modifiers doped with nano-silicon dioxide, and the performance of the product deteriorates significantly. The performance effect of the product is most obvious when the two are used in combination.

[0170] The performance of the products tended to deteriorate when the nano-attapulgite liquid treatment was not used in the preparation of the multi-adjustment improved stabilizer, the S011 and S012 treatment was not used in the nano-attapulgite liquid, and the multi-adjustment stabilizer treatment was not used in the preparation of the multi-adjustment improved stabilizer. The performance of the products tended to change greatly when the multi-adjustment stabilizer treatment and the nano-attapulgite liquid treatment were not used.

[0171] In the preparation of the modifier doped with nano-silica, no modifier blending agent was used for treatment, no modifier liquid B was added to the modifier blending agent, no modifier liquid A was added to the modifier blending agent, and no dried flaky graphene was added to the modifier liquid B. The performance of the product tended to deteriorate. The modifier blending agent prepared by combining the modifier liquid B obtained by the method of the present invention with the modifier liquid A had the most significant product performance effect. Other methods were not as obvious as the effect of the present invention.

[0172] Based on the fact that multi-adjustment stabilizers can significantly change the performance of the product, further research is conducted on this.

[0173] Experimental Example 1:

[0174] The only difference from Example 3 is that silicon carbide whiskers are not added in the preparation of the multi-adjusting stabilizer.

[0175] Experimental Example 2:

[0176] The only difference from Example 3 is that yttrium oxide is not added in the preparation of the multi-adjusting stabilizer.

[0177] Experimental Example 3:

[0178] The only difference from Example 3 is that no boron nitride is added in the preparation of the multi-adjusting stabilizer.

[0179] Experimental Example 4:

[0180] The only difference from Example 3 is that stearic acid is not added in the preparation of the multi-adjusting stabilizer, and deionized water is used instead of the sodium dodecylbenzene sulfonate solution.

[0181] The products of Experimental Examples 1-4 were placed under normal conditions to test flame retardancy and thermal insulation. At the same time, the products were treated at 65°C for 12 hours, then placed at -5°C for 12 hours, and the products were repeatedly tested 5 times to test the high and low temperature stability of the products; and the products were irradiated under ultraviolet conditions with a light intensity of 0.5W / m2 and a wavelength of 340nm for 12 hours. After the irradiation, the products were placed under 2% hydrochloric acid mist conditions for 12 hours, and the tests were repeated 5 times to test the acid corrosion resistance and ultraviolet stability of the products; the product performance test results are shown in Table 2.

[0182] Table 2: Product performance test results of Experimental Examples 1-4

[0183]

[0184] As can be seen from Table 2, silicon carbide whiskers are not added in the preparation of the multi-adjusting stabilizer. Under normal conditions, the thermal insulation and flame retardancy of the product are more obvious in the preparation factors of the multi-adjusting stabilizer. Boron nitride is not added in the preparation of the multi-adjusting stabilizer. The product performance deteriorates more obviously under high and low temperature, UV resistance and acid corrosion conditions. Silicon carbide whiskers and boron nitride can be coordinated and improved to optimize product performance effects. The multi-adjusting stabilizer made of yttrium oxide, stearic acid, and sodium dodecylbenzene sulfonate solution has the most significant performance effect. Other methods are not as obvious as the effect of the present invention.

[0185] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0186] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An environmentally friendly water-based high and low temperature film, comprising a TPU base film, characterized in that: The TPU base film is immersed in a glue liquid to form a glue layer, and a water-based coating is coated on the glue layer to form a water-based coating. The water-based coating, the glue layer and the TPU base film are arranged in sequence from top to bottom; The thickness of the TPU base film is 10-15 mm, the thickness of the adhesive layer is 2-5 mm, and the thickness of the water-based coating is 1-3 mm; The adhesive comprises the following raw materials in parts by weight: 7-11 parts of a stabilizer based on multi-adjustment improvement, 2-5 parts of a silane coupling agent KH560, 4-7 parts of an epoxy resin, 8-12 parts of a polyurethane adhesive, and 8-10 parts of ethanol; The water-based coating comprises the following raw materials in parts by weight: 25-30 parts of coating base agent, 4-7 parts of magnesium hydroxide, 3-5 parts of glass microspheres, and 4-6 parts of a modifier doped with nano-silicon dioxide; The coating base agent is prepared from epoxy resin with a weight average molecular weight of 5000-6000, xylene and 3-methyltetrahydrophthalic anhydride curing agent in a weight ratio of 4:11:1; The preparation method of the stabilizer based on multi-adjustment improvement is: S01: Preparation of nano-attapulgite liquid: S011: heat treating the nano-attapulgite at 130-150° C. for 10-15 min; S012: then heating to 230-250°C at a rate of 2-5°C / min, keeping the temperature for 5-10 minutes, and then cooling to 55°C at a rate of 1-3°C / min, keeping the temperature, to obtain heat-treated nano-attapulgite; S013: mixing the heat-treated nano-attapulgite, the sodium alginate solution and the phosphate buffer solution in a weight ratio of 3:5:1 to obtain a nano-attapulgite liquid; S02: The multi-adjustable stabilizer and the nano-attapulgite liquid are mixed in a weight ratio of 3:5 and subjected to ball milling treatment at a ball milling speed of 1000-1500 r / min for 2 h. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizer based on multi-adjustable improvement; The preparation method of the multi-adjusting stabilizer is: 5-8 parts of silicon carbide whiskers, 1-3 parts of yttrium oxide, and 2-5 parts of sodium dodecylbenzene sulfonate solution are uniformly mixed, and then 2-4 parts of boron nitride and 1-2 parts of stearic acid are added and mixed and ball milled at a ball milling speed of 1500-1700r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a multi-adjustable stabilizer; The preparation method of the nano-silicon dioxide-doped modifier is as follows: S11: 2-5 parts of lanthanum nitrate solution, 1-3 parts of nano-silica sol and 4-7 parts of 4% chitosan solution are uniformly mixed to obtain a modified solution A; S12: stirring and mixing the graphene flakes in a sufficient amount of a 5% by mass potassium permanganate solution, and then washing and drying the graphene flakes to obtain dry graphene flakes; 4-7 parts of dried flake graphene, 1-3 parts of silane coupling agent KH560 and 2-4 parts of sodium lignin sulfonate solution are fully mixed to obtain a modified solution B; S13: subjecting the modified liquid B and the modified liquid A to a first ultrasonic modification treatment at a weight ratio of 2:(5-7) to obtain a modified blending agent; The nano-silicon dioxide and the modifying agent are subjected to a second ultrasonic modification treatment in a weight ratio of 3:

7. After the ultrasonic treatment, the modified agent is washed with water, filtered and dried to obtain the modifying agent doped with nano-silicon dioxide.

2. The environmentally friendly water-based high and low temperature membrane according to claim 1, characterized in that: The mass fraction of the sodium alginate solution is 4-7%; the pH value of the phosphate buffer solution is 5.

5.

3. The environmentally friendly water-based high and low temperature membrane according to claim 1, characterized in that: The mass fraction of the sodium dodecylbenzene sulfonate solution is 4-7%.

4. The environmentally friendly water-based high and low temperature membrane according to claim 1, characterized in that: The mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.

5. The environmentally friendly water-based high and low temperature membrane according to claim 1, characterized in that: The ultrasonic power of the first ultrasonic modification treatment is 450-550W, and the ultrasonic time is 20-30min; the ultrasonic power of the second ultrasonic modification treatment is 300-350W, and the ultrasonic time is 45-55min.

6. A method for preparing an environmentally friendly water-based high-low temperature membrane, used for preparing the environmentally friendly water-based high-low temperature membrane as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, weighing the raw materials in the glue solution according to weight parts and mixing them thoroughly to obtain the glue solution; Step 2, immersing the TPU base film into the adhesive liquid to form an adhesive layer, and mixing the raw materials in the water-based coating agent sufficiently to obtain the water-based coating agent; Step three, coating the adhesive layer with a water-based coating agent to form a water-based coating to obtain an environmentally friendly water-based high and low temperature film.