A continuous preparation process for PFA composite copper foil roll
The preparation of weather-resistant PFA film and modified copper foil through plasma treatment and ion implantation processes has solved the problems of poor dielectric performance and insufficient heat resistance of flexible high-frequency circuit board substrates in the prior art, and achieved high Frequency signal transmission and low heat characteristics.
Patent Information
- Application Number
- CN202410764907.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The prior art is difficult to prepare flexible high-frequency circuit board substrates and composite copper foil rolls with excellent performance. Traditional substrates have poor dielectric properties and poor heat resistance, and ethylene and tetrafluoroethylene copolymers are prone to cracking at high temperatures. Limits its application.
The weather-resistant PFA film is prepared by plasma treatment and ion implantation process, and rolled with the modified copper foil through the calendering process to form a PFA composite copper foil roll to improve its bonding performance and weather resistance.
It improves the tensile performance and high temperature resistance of PFA film, enhances the bonding performance between copper foil and PFA film, reduces the dielectric loss factor, is suitable for high-frequency and high-speed signal transmission, and reduces the heating of the circuit board.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper foil roll preparation, and in particular to a continuous preparation process of a PFA composite copper foil roll. Background Art
[0002] With the development of 5G mobile networks, satellite communications, navigation and other fields, aerospace electronic circuit products are gradually developing towards high frequency, miniaturization and low power consumption. The performance of dielectric materials used in electrical and electronic devices on spacecraft directly affects the reliability and life of instruments and equipment and even spacecraft operation. Flexible circuit boards are conducive to reducing the size and mass of devices and enhancing the retractable and mobile performance of devices. Polytetrafluoroethylene (PTFE) copper clad laminate is a commonly used substrate for flexible high-frequency circuit boards. It has excellent dielectric properties and extremely low radiation levels, but its extremely low surface activity and outstanding non-stickiness make it difficult to composite with matrix materials, limiting its application. The existing technology can only produce copper foil, and the production and preparation process of composite copper foil rolls is still immature. Therefore, the preparation of a substrate and composite copper foil roll for flexible high-frequency circuit boards with excellent performance has become a hot topic of current research.
[0003] Although traditional substrates such as phenolic / paper and epoxy / glass cloth have low costs and mature processes, they are increasingly exposed to defects such as poor dielectric properties, poor heat resistance, and high thermal expansion coefficient when used as base materials for high-performance flexible high-frequency circuit boards; ethylene and tetrafluoroethylene copolymer (ETFE) is synthesized by alternating copolymerization of ethylene and tetrafluoroethylene. It not only has the heat resistance, chemical resistance, and electrical insulation of traditional PTFE, but also has greatly improved density, radiation resistance, and mechanical properties. At the same time, it can be melt-processed and has a wide range of applications in the fields of wires and cables, anti-corrosion coatings, etc. The introduction of ethylene improves radiation resistance and its processing performance is also improved. At the same time, its adhesion to metal surfaces is greatly improved, making it possible to achieve a tight lining process between fluoroplastics and metals; but ETFE copolymers containing only tetrafluoroethylene and ethylene also have shortcomings. Small stresses at high temperatures can cause them to crack, greatly shortening their service life. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a continuous preparation process for a PFA composite copper foil roll. The novel PFA film is used as a matrix material, and plasma treatment and ion implantation processes are utilized. The modified copper foil is wound with a winding roller, and the rolled PFA film has the characteristics of strong weather resistance and anti-peeling performance.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A continuous preparation process of a PFA composite copper foil roll comprises the following steps:
[0007] (1) After ultrasonic cleaning of the weather-resistant PFA film with ethanol and acetone, the film was placed in a plasma generator and vacuumed for 10-20 minutes. The reaction gas was introduced and the vacuum degree was adjusted to 45-60Pa for low-temperature plasma treatment. The film was then placed in a magnetic filtration composite vacuum coating machine and an ion implantation method was used to deposit a metal transition layer on the surface. The ion implantation target was a nickel target and the ion energy was 8-12keV to obtain a weather-resistant high-viscosity PFA film.
[0008] (2) The weather-resistant high-viscosity PFA film is made into a 20-30 μm thick raw substrate by a calendering process, and the surface-modified copper foil is coated on both sides of the raw substrate. The substrate is pressed at 180-210°C for 1-3 hours and then rolled up by a winding roller to obtain a PFA composite copper foil roll.
[0009] Furthermore, the reaction gas in step (1) is nitrogen or oxygen generated by capacitively coupled glow discharge.
[0010] Furthermore, in step (1), the plasma gas treatment time is 5-10 minutes, and the plasma gas treatment power is 60-100W.
[0011] Furthermore, the pressing pressure in step (2) is 1.5-2.5 MPa.
[0012] Furthermore, the preparation process of the weather-resistant PFA film in step (1) comprises the following steps:
[0013] Step S1, under a nitrogen atmosphere, add perfluorobutanol and tetrahydrofuran to a reaction flask, stir evenly, add sodium hydride, stir evenly, add methylphenylvinylchlorosilane and tetrabutylammonium iodide, stir to react, after the reaction is completed, extract with ethyl acetate and deionized water, concentrate the organic phase, separate by column chromatography, and dry to obtain a fluorine-containing organosilicon olefin monomer. The preparation reaction formula is as follows:
[0014]
[0015] Step S2, under a nitrogen atmosphere, add tert-butyl alcohol, deionized water and ammonium persulfate to a high-pressure reactor, stir evenly, add tetrafluoroethylene monomer, ethylene monomer and fluorinated organosilicon monomer, stir to react, and after the reaction is completed, perform vacuum distillation, cast film formation, and obtain a weather-resistant PFA film.
[0016] Furthermore, in step S1, the ratio of perfluorobutanol, sodium hydride, methylphenylvinylchlorosilane, and tetrabutylammonium iodide is 1 mol: (1.1-1.3) mol: (1.05-1.2) mol: (0.05-0.1) mol.
[0017] Furthermore, in step S1, the reaction temperature is 20-35° C., and the reaction time is 8-16 h.
[0018] Furthermore, in step S2, the ratio of ammonium persulfate, tetrafluoroethylene monomer, ethylene monomer, and fluorinated organosilicon monomer is (0.02-0.05) mol:1 mol:(0.8-1.2) mol:(0.01-0.05) mol.
[0019] Furthermore, in step S2, the reaction temperature is 60-80° C., the reaction pressure is 2-3 MPa, and the reaction time is 5-10 h.
[0020] By adopting the above technical solution, the beneficial effects of the present invention are:
[0021] The invention firstly obtains a fluorine-containing organic silicon alkenyl monomer by reacting methylphenylvinyl chlorosilane with perfluorobutanol under the action of sodium hydride and tetrabutylammonium iodide, and then obtains a weather-resistant PFA film by reacting tetrafluoroethylene monomer and ethylene monomer under the initiation of ammonium persulfate, and then uses plasma treatment and ion implantation method to deposit a metal transition layer on the surface of the weather-resistant PFA film to obtain a weather-resistant high-viscosity PFA film, and finally uses a calendering molding process to roll up the weather-resistant high-viscosity PFA film and a surface-modified copper foil winding roller to obtain a PFA composite copper foil roll.
[0022] The organic groups in the fluorinated silicone alkenyl monomer molecules are structurally consistent with tetrafluoroethylene molecules and have good compatibility. They are polymerized with ethylene monomers and tetrafluoroethylene monomers, and by introducing a rigid benzene ring structure, the network crosslinking density of the system is increased, thereby enhancing the bonding strength between the matrixes, and significantly improving the tensile properties of the PFA film. The weather-resistant PFA film molecular structure contains silicon bonds and carbon bonds. The bond energy of silicon bonds is higher than that of carbon bonds, and can withstand higher temperature heat energy. At the same time, the bond length of silicon bonds is longer than that of carbon bonds, which makes the silicone have better flexibility and deformation properties. After being placed at 200°C for 24 hours, no cracking occurs, and it has good high temperature stability.
[0023] The treatment of thin film by plasma gas and ion implantation not only has the etching effect of physical sputtering, but also produces molecular activation and chemical reaction, which causes an increase in free radicals on the surface of the film and a substantial increase in surface energy, plays a role in energy transfer, and promotes the introduction of active groups such as -OH and COC on the surface of the film. Since -OH and COC are hydrophilic groups, the hydrophilicity and adhesion properties of the film are improved. After the rough surface of the ultra-thin copper foil is modified, the grain size on the surface of the copper foil is uniform and closely arranged, and many small "branches" grow on the grains. The existence of "branch" grains can greatly enhance the anchoring force of the copper foil, making it more tightly bonded to the weather-resistant PFA film, reducing the interface effect between the two, and improving the adhesion between the PFA film and the copper foil, laying a good foundation for the subsequent preparation of flexible circuit boards.
[0024] The composite copper foil roll prepared by the present invention has a low dielectric loss factor, which is conducive to complete and rapid transmission of signals, and can reduce the heating of the circuit board itself, which is very beneficial to the use of the circuit board under high frequency and high speed conditions; the surface modified copper foil is evenly coated on both sides of the weather-resistant and high-viscosity PFA film, and the PFA composite copper foil roll is obtained after winding, which can effectively prevent electronic breakdown, can improve the flexibility of the material, and has the characteristics of high safety and light weight. DETAILED DESCRIPTION
[0025] The preferred embodiments of the invention are described in detail below. The examples are for better illustrating the content of the invention, and the content of the invention is not limited to the examples. Non-essential improvements and adjustments to the implementation scheme according to the content of the invention still belong to the scope of the invention.
[0026] Ultra-thin copper foil: low-profile electrolytic copper foil, the roughness Rz of the electrolytic copper foil is 0.75μm, the thickness is 10μm, from Luxembourg, Germany.
[0027] Preparation of surface modified copper foil: Add 20 mL of ethanol and 80 mL of deionized water into a reaction flask, add 15 g of heptadecafluorodecyltriethoxysilane coupling agent while stirring, heat the mixed solution to 40°C, stir for 20 minutes, and obtain a solution that can be used for rough surface treatment of ultra-thin copper foil. Spray it evenly on the rough surface of the copper foil, and let it stand at room temperature for 8 hours to obtain a surface modified copper foil.
[0028] Example 1
[0029] (1) Under nitrogen atmosphere, 15 mmol perfluorobutanol and 60 mL tetrahydrofuran were added to a reaction flask. After stirring, 18 mmol sodium hydride was added. After stirring, 16.5 mmol methylphenylvinylsilyl chloride and 1.2 mmol tetrabutylammonium iodide were added. The mixture was reacted at 25°C for 12 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated, separated by column chromatography, and dried to obtain a fluorinated organosilicon monomer.
[0030] (2) Under nitrogen atmosphere, 45 mL of tert-butyl alcohol, 5 mL of deionized water and 0.3 mmol of ammonium persulfate were added to the autoclave. After stirring evenly, 10 mmol of tetrafluoroethylene monomer, 8 mmol of ethylene monomer and 0.1 mmol of fluorinated organosilicon monomer were added. The reaction was carried out at a temperature of 70 °C and a pressure of 2.2 MPa for 9 h. The film was then distilled under reduced pressure and cast to obtain a weather-resistant PFA film.
[0031] Example 2
[0032] (1) Under nitrogen atmosphere, 50 mmol perfluorobutanol and 150 mL tetrahydrofuran were added to a reaction flask. After stirring, 55 mmol sodium hydride was added. After stirring, 52.5 mmol methylphenylvinylsilyl chloride and 2.5 mmol tetrabutylammonium iodide were added. The mixture was reacted at 35° C. for 8 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated, separated by column chromatography, and dried to obtain a fluorinated organosilicon monomer.
[0033] (2) Under nitrogen atmosphere, 45 mL of tert-butyl alcohol, 5 mL of deionized water and 0.2 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer, 8 mmol of ethylene monomer and 0.2 mmol of fluorinated organosilicon monomer were added. The reaction was carried out at a temperature of 80 °C and a pressure of 3 MPa for 5 h. The film was then distilled under reduced pressure and cast to obtain a weather-resistant PFA film.
[0034] Example 3
[0035] (1) Under nitrogen atmosphere, add 20 mmol perfluorobutanol and 100 mL tetrahydrofuran to a reaction flask, stir well, then add 26 mmol sodium hydride, stir well, then add 24 mmol methylphenylvinylsilyl chloride and 1 mmol tetrabutylammonium iodide, react at 20 °C for 16 h, extract with ethyl acetate and deionized water, concentrate the organic phase, separate by column chromatography, and dry to obtain a fluorinated organosilicon monomer.
[0036] (2) Under nitrogen atmosphere, 45 mL of tert-butyl alcohol, 5 mL of deionized water and 0.5 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer, 12 mmol of ethylene monomer and 0.3 mmol of fluorinated organosilicon monomer were added. The reaction was carried out at a temperature of 60 °C and a pressure of 2 MPa for 10 h. The film was then distilled under reduced pressure and cast to obtain a weather-resistant PFA film.
[0037] Example 4
[0038] (1) Under nitrogen atmosphere, 35 mmol perfluorobutanol and 125 mL tetrahydrofuran were added to a reaction flask. After stirring, 42 mmol sodium hydride was added. After stirring, 40 mmol methylphenylvinylsilyl chloride and 2.8 mmol tetrabutylammonium iodide were added. The mixture was reacted at 30° C. for 15 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated, separated by column chromatography, and dried to obtain a fluorinated organosilicon monomer.
[0039] (2) Under nitrogen atmosphere, 45 mL of tert-butyl alcohol, 5 mL of deionized water and 0.4 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer, 11 mmol of ethylene monomer and 0.4 mmol of fluorinated organosilicon monomer were added. The reaction was carried out at a temperature of 75 °C and a pressure of 2.5 MPa for 9 h. The film was then distilled under reduced pressure and cast to obtain a weather-resistant PFA film.
[0040] Example 5
[0041] (1) Under nitrogen atmosphere, 30 mmol perfluorobutanol and 105 mL tetrahydrofuran were added to a reaction flask. After stirring, 37.5 mmol sodium hydride was added. After stirring, 33.6 mmol methylphenylvinylsilyl chloride and 1.8 mmol tetrabutylammonium iodide were added. The mixture was reacted at 35° C. for 12 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated, separated by column chromatography, and dried to obtain a fluorinated organosilicon monomer.
[0042] (2) Under nitrogen atmosphere, 45 mL of tert-butyl alcohol, 5 mL of deionized water and 0.35 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer, 10 mmol of ethylene monomer and 0.5 mmol of fluorinated organosilicon monomer were added. The reaction was carried out at a temperature of 65 °C and a pressure of 3 MPa for 10 h. The film was then distilled under reduced pressure and cast to obtain a weather-resistant PFA film.
[0043] Comparative Example 1
[0044] Under a nitrogen atmosphere, 45 mL of tert-butanol, 5 mL of deionized water and 0.3 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer and 8 mmol of ethylene monomer were added. The reaction was carried out at a temperature of 70°C and a pressure of 2.2 MPa for 9 h. The film was distilled under reduced pressure and cast into a film to obtain a PFA film.
[0045] Comparative Example 2
[0046] Under a nitrogen atmosphere, 45 mL of tert-butanol, 5 mL of deionized water and 0.3 mmol of ammonium persulfate were added to a high-pressure reactor. After stirring evenly, 10 mmol of tetrafluoroethylene monomer was added. The mixture was reacted at a temperature of 70°C and a pressure of 2.2 MPa for 9 h. The mixture was distilled under reduced pressure and cast into a film to obtain a PTFE film.
[0047] Tensile performance test: Referring to GB / T 1040.3-2006 standard, a universal material testing machine was used to test the tensile strength of the film at a tensile rate of 100 mm / min.
[0048] Stress cracking resistance test: Place the prepared film sample in an aging box at 200°C, observe the cracking of the film, record the time required for cracking, and judge the stress cracking resistance of the film.
[0049] Table 1 Film performance test
[0050]
[0051] It can be seen from the test results in the above table that with the increase of the content of fluorinated organosilicon alkenyl monomer, the tensile properties of the weather-resistant PFA film gradually increase, and the tensile strength in Example 4 reaches 16.40 MPa. This is because the organic groups in the fluorinated organosilicon alkenyl monomer molecules have structural consistency with the tetrafluoroethylene molecules and have good compatibility. They are polymerized with ethylene monomers and tetrafluoroethylene monomers, and a rigid benzene ring structure is introduced to improve the network crosslinking density of the system. Through chemical crosslinking and intermolecular forces, the bonding strength between the substrates is enhanced, and the tensile properties of the PFA film are significantly improved.
[0052] After being placed at 200°C for 24 hours, the weather-resistant PFA film did not crack and had good high-temperature stability. This is because the molecular structure of silicone contains silicon bonds and carbon bonds. The bond energy of silicon bonds is higher than that of carbon bonds, and it can withstand higher temperature heat. At the same time, the bond length of silicon bonds is longer than that of carbon bonds, which makes silicone have better flexibility and deformation performance. Therefore, even in a high-temperature environment, silicone can maintain excellent mechanical properties; Comparative Example 1 contains vinyl monomers, does not contain silicone and benzene rings, and the mechanical properties of the film after polymerization are poor; Comparative Example 2 is a pure polytetrafluoroethylene film without any modification, and its performance is the worst.
[0053] Example 6
[0054] The weather-resistant PFA film (prepared in Example 4) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 60 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target was a nickel target, and the ion energy was 10 keV, to obtain a weather-resistant and high-viscosity PFA film.
[0055] Example 7
[0056] The difference between this embodiment and embodiment 6 is that the plasma gas processing power is 70W, and other conditions remain the same.
[0057] The weather-resistant PFA film (prepared in Example 4) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 70 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target was a nickel target, and the ion energy was 10 keV, to obtain a weather-resistant and high-viscosity PFA film.
[0058] Example 8
[0059] The difference between this embodiment and embodiment 6 is that the plasma gas processing power is 80W, and other conditions remain the same.
[0060] The weather-resistant PFA film (prepared in Example 4) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 80 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target material was a nickel target, and the ion energy was 10 keV, to obtain a weather-resistant and high-viscosity PFA film.
[0061] Example 9
[0062] The difference between this embodiment and embodiment 6 is that the plasma gas processing power is 90W, and other conditions remain the same.
[0063] The weather-resistant PFA film (prepared in Example 4) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 90 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target material was a nickel target, and the ion energy was 10 keV, to obtain a weather-resistant and high-viscosity PFA film.
[0064] Example 10
[0065] The difference between this embodiment and embodiment 6 is that the plasma gas processing power is 100 W, and other conditions remain the same.
[0066] The weather-resistant PFA film (prepared in Example 4) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 100 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target material was a nickel target, and the ion energy was 10 keV, to obtain a weather-resistant and high-viscosity PFA film.
[0067] Comparative Example 3
[0068] The PFA film (prepared in Comparative Example 1) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, the vacuum degree was adjusted to 50 Pa, the plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 60 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target material was a nickel target, and the ion energy was 10 keV, to obtain a high-viscosity PFA film.
[0069] Comparative Example 4
[0070] The PTFE film (prepared in Comparative Example 2) was ultrasonically cleaned with ethanol and acetone, placed in a plasma generator, and evacuated for 20 minutes. Nitrogen generated by capacitively coupled glow discharge was introduced, and the vacuum degree was adjusted to 50 Pa. The plasma gas treatment time was 10 minutes, and the plasma gas treatment power was 60 W. Then, it was placed in a magnetic filtration composite vacuum coating machine, and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target material was a nickel target, and the ion energy was 10 keV, to obtain a high-viscosity PTFE film.
[0071] Contact angle test: A dynamic contact angle analyzer was used to test the contact angle of the film. The test temperature was 25°C and the test liquid was deionized water.
[0072] Table 2 Modified film wettability test
[0073]
[0074] The size of the contact angle of the film surface directly reflects the wetting effect of the copper foil on the film and the size of the adhesion work, and can also reflect the self-cleaning ability of the film. It can be seen from the test results in the above table that with the increase of the plasma gas treatment power, the surface contact angle of the film gradually decreases. The contact angle in Example 9 is 100.5°C, which has a certain self-cleaning effect. At the same time, the decrease in the contact angle indicates that the wettability of the film surface is improved and the adhesion work is gradually increased. This is because the treatment of the film by the plasma gas not only has the etching effect of physical sputtering, but also produces molecular activation and chemical reactions, causing an increase in free radicals on the film surface and a significant increase in surface energy, which plays a role in energy transfer and promotes the introduction of active groups such as -OH and COC on the film surface. Since -OH and COC are hydrophilic groups, the hydrophilicity and adhesion properties of the film are improved.
[0075] Embodiment 11
[0076] The weather-resistant high-viscosity PFA film (prepared in Example 9) was made into a 25 μm thick raw substrate by calendering process, and the surface-modified copper foil was coated on both sides of the raw substrate. The substrate was pressed at 200°C and 2 MPa for 2 h, and then rolled up by a winding roller to obtain a PFA composite copper foil roll.
[0077] Example 12
[0078] The weather-resistant high-viscosity PFA film (prepared in Example 9) was made into a 30 μm thick raw substrate by calendering process, and the surface-modified copper foil was coated on both sides of the raw substrate. The substrate was pressed at 210°C and a pressure of 2.5 MPa for 1 hour, and then wound up by a winding roller to obtain a PFA composite copper foil roll.
[0079] Embodiment 13
[0080] The weather-resistant high-viscosity PFA film (prepared in Example 9) was made into a 20 μm thick raw substrate by calendering process, and the surface-modified copper foil was coated on both sides of the raw substrate. The substrate was pressed at 180°C and a pressure of 1.5 MPa for 3 hours, and then rolled up by a winding roller to obtain a PFA composite copper foil roll.
[0081] Comparative Example 5
[0082] The difference between this comparative example and Example 11 is that the ultra-thin copper foil is not surface treated, and other conditions remain the same.
[0083] The weather-resistant high-viscosity PFA film (prepared in Example 4) was made into a 25 μm thick raw substrate by calendering process, and ultra-thin copper foil was covered on both sides of the raw substrate. The substrate was pressed at 200°C and a pressure of 2 MPa for 2 h, and then rolled up by a winding roller to obtain a PFA composite copper foil roll.
[0084] Peel strength test: Referring to the standard IPC-TM-650:2004, the prepared PFA composite copper foil roll was cut into a size of 10cm×5cm, and a 3mm wide acid-alkali resistant tape was pasted and then acid-corroded. Pressure was applied at a speed of 0.8mm / s, and the length was peeled off at least 7cm.
[0085] Dielectric loss factor test: Referring to the standard IPC-TM-650:2004, the prepared PFA composite copper foil roll was cut into a size of 30 mm×50 mm, the test frequency was 1-17 GHz, and the working pressure was 650 kg.
[0086] Table 3 Composite copper foil roll performance test
[0087]
[0088] It can be seen from the test results in the above table that, under the premise that the prepared weather-resistant PFA film has excellent wettability and mechanical strength, after the rough surface of the ultra-thin copper foil is modified, the grain size on the surface of the copper foil is uniform and closely arranged, and many small "branches" grow on the grains. The existence of "branch" grains can greatly improve the anchoring force of the copper foil, making it more tightly bonded to the weather-resistant PFA film, reducing the interface effect between the two, and improving the bonding performance between the PFA film and the copper foil, laying a good foundation for the subsequent preparation of circuit boards.
[0089] Dielectric loss is the most important indicator of a substrate. When transmitting signals, the dielectric loss factor of the substrate is required to be as low as possible. It can be seen from the test results in the above table that the composite copper foil roll prepared by the present invention has a lower dielectric loss factor, which is conducive to complete and rapid transmission of signals, and can also reduce the heating of the circuit board itself, which is very beneficial to the use of the circuit board under high frequency and high speed conditions.
[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A continuous preparation process for a PFA composite copper foil roll, characterized in that: The preparation process comprises the following steps: (1) After ultrasonic cleaning of the weather-resistant PFA film with ethanol and acetone, the film was placed in a plasma generator and vacuumed for 10-20 minutes. The reaction gas was introduced and the vacuum degree was adjusted to 45-60 Pa for low-temperature plasma treatment. The film was then placed in a magnetic filtration composite vacuum coating machine and a metal transition layer was deposited on the surface by ion implantation. The ion implantation target was a nickel target and the ion energy was 8-12 keV to obtain a weather-resistant and high-viscosity PFA film. (2) Using a calendering process, the weather-resistant high-viscosity PFA film is made into a 20-30 μm thick raw substrate, and the surface-modified copper foil is coated on both sides of the raw substrate. The substrate is pressed at 180-210 ° C for 1-3 hours and wound by a winding roller to obtain a PFA composite copper foil roll; The preparation process of the weather-resistant PFA film in step (1) comprises the following steps: Step S1: Under a nitrogen atmosphere, perfluorobutanol and tetrahydrofuran were added to a reaction flask, stirred evenly, and then sodium hydride was added. After stirring evenly, methylphenylvinylchlorosilane and tetrabutylammonium iodide were added, and the mixture was stirred for reaction. After the reaction was completed, the mixture was extracted with ethyl acetate and deionized water, and the organic phase was concentrated, separated by column chromatography, and dried to obtain a product having the structural formula: Fluorinated organosilicon vinyl monomers; Step S2: adding tert-butyl alcohol, deionized water, and ammonium persulfate to an autoclave under a nitrogen atmosphere, stirring evenly, and then adding tetrafluoroethylene monomer, ethylene monomer, and fluorinated organosilicon monomer, stirring for reaction. After the reaction is completed, performing vacuum distillation and casting to form a film to obtain a weather-resistant PFA film; The preparation method of the surface-modified copper foil in step (2) is as follows: 20 mL of ethanol and 80 mL of deionized water are added to a reaction flask, 15 g of heptadecafluorodecyltriethoxysilane coupling agent is added under stirring, the mixed solution is heated to 40° C., and stirred for 20 minutes to obtain a solution that can be used for rough surface treatment of ultra-thin copper foil, the solution is evenly sprayed on the rough surface of the copper foil, and the solution is allowed to stand at room temperature for 8 hours to obtain a surface-modified copper foil.
2. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: The reaction gas in step (1) is nitrogen or oxygen generated by capacitively coupled glow discharge.
3. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: In the step (1), the plasma gas treatment time is 5-10 minutes, and the plasma gas treatment power is 60-100W.
4. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: The pressing pressure in step (2) is 1.5-2.5 MPa.
5. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: In step S1, the ratio of perfluorobutanol, sodium hydride, methylphenylvinylchlorosilane, and tetrabutylammonium iodide is 1 mol: (1.1-1.3) mol: (1.05-1.2) mol: (0.05-0.1) mol.
6. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: In step S1, the reaction temperature is 20-35° C., and the reaction time is 8-16 h.
7. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: In the step S2, the ratio of ammonium persulfate, tetrafluoroethylene monomer, ethylene monomer, and fluorinated organic silicon olefin monomer is (0.02-0.05) mol:1 mol:(0.8-1.2) mol:(0.01-0.05) mol.
8. The continuous preparation process of the PFA composite copper foil roll according to claim 1, characterized in that: In step S2, the reaction temperature is 60-80° C., the reaction pressure is 2-3 MPa, and the reaction time is 5-10 h.
Citation Information
Patent Citations
Preparation method of novel flexible copper-clad plate
CN112677617A
Preparation method and application of polytetrafluoroethylene-based copper-clad plate
CN116494612A
Process for producing modified polymer, apparatus for producing modified polymer, and modified polymer
US20050053792A1