Acrylic resin coating for marine engineering and preparation method thereof

Through the grafting technology of eugenol and graphene oxide in modified acrylic resin coatings, the problems of toxicity and unsustainable antifouling performance of existing marine antifouling coatings are solved, environmentally friendly and long-term antifouling effects are achieved, and meet the requirements of marine engineering anti-fouling needs.

CN118685089BActive Publication Date: 2024-10-25安徽三旺化学有限公司
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411165112.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-25
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing marine antifouling coatings have toxic and ecological impacts during long-term use, and their antifouling properties are not durable enough, making it difficult to meet the long-term antifouling needs of marine projects.

Method used

Modified acrylic resin coating is used, and by introducing eugenol, quaternary ammonium cationic groups and graphene oxide, a coating with excellent antibacterial and antifouling properties is formed. The uniformity and adhesion of the coating are improved through grafting technology, and the coating is extended. The duration of the layer.

Benefits of technology

It achieves environmentally friendly and long-term antifouling performance, improves the adhesion and antifouling effect of the coating, reduces the chance of pollutants adhering, enhances the ability to inhibit bacteria, and meets the antifouling needs of marine engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of coatings, and in particular to an acrylic resin coating for marine engineering and a preparation method thereof. The acrylic resin coating for marine engineering of the present invention comprises the following raw materials in parts by weight: 60-75 parts of modified acrylic resin solution, 3-5 parts of pigments and fillers, 15-20 parts of organic solvents, 1-2 parts of dispersants, 0.5-2 parts of defoamers, and 0.5-1 parts of leveling agents. The coating after coating has good adhesion and hardness, and the mechanical properties can meet the requirements of actual use, and it has excellent antibacterial and antifouling properties, and can achieve long-term sustained release, and has good lasting antifouling effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to an acrylic resin coating for marine engineering and a preparation method thereof. Background Art

[0002] Marine biofouling refers to the adverse accumulation of marine organisms on the surface of artificial equipment submerged in seawater due to their growth and adhesion. It is a natural phenomenon and a hazard that humans must face when engaging in marine activities. At present, marine antifouling methods can be divided into three categories: physical antifouling methods, chemical antifouling methods and biological antifouling methods.

[0003] Applying antifouling paint has become the most commonly used chemical antifouling method. It mainly involves applying antifouling paint on the surface of the structure and using the characteristics of the coating itself or the antifouling agent that seeps out of the coating to kill or inhibit the growth and adhesion of fouling organisms.

[0004] Patent technical document CN202110280343.8 discloses a self-polishing graphene antifouling coating and a preparation method thereof. The invention can fix copper ions on the main chain of the resin through a complex while retaining part of the cuprous oxide, thereby ensuring the antibacterial and antifouling effect of the copper ions and avoiding the weakening of the lasting antifouling performance caused by the excessive loss of copper ions. Secondly, the compatibility of the graphene in the coating is improved by modifying the added graphene. However, when zinc oxide, cuprous oxide, etc. are used for biological antifouling, they will cause harm to marine organisms, thereby affecting the marine ecology.

[0005] Patent technical document CN202211018445.3 discloses a self-polishing antifouling coating embedded with crushed Zanthoxylum bungeanum, and its preparation method and application. The invention adds crushed Zanthoxylum bungeanum as an antifouling agent to the self-polishing antifouling coating, which can effectively inhibit the attachment of different algae and other marine organisms. It is green and non-toxic, the coating has good weather resistance, and has good marine antifouling effect. However, as hydrolysis proceeds, its continuous action time is not long, which is not conducive to long-term use. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide an acrylic resin coating for marine engineering and a preparation method thereof, so as to provide an acrylic resin coating which is environmentally friendly and has long-term antifouling performance.

[0007] Based on the above purpose, the present invention provides an acrylic resin coating for marine engineering, comprising the following raw materials in parts by weight: 60-75 parts of modified acrylic resin solution, 3-5 parts of pigments and fillers, 15-20 parts of organic solvents, 1-2 parts of dispersants, 0.5-2 parts of defoamers, and 0.5-1 parts of leveling agents;

[0008] The preparation steps of the modified acrylate solution are as follows:

[0009] S1: Mixing graphene oxide with ethanol, ultrasonicating for 1 h to obtain a graphene oxide dispersion; then dissolving 11-mercaptoundecyltrimethoxysilane in ethanol, adjusting the pH to 3.5-4, standing for 1 h, and then mixing it with the graphene oxide dispersion, reacting at 20-30°C for 20-24 h, centrifuging, washing, and drying to obtain thiolated graphene oxide;

[0010] Further, in step S1, the weight ratio of graphene oxide, 11-mercaptoundecyltrimethoxysilane and ethanol is 0.2-0.4:1.5-2:280-300;

[0011] Furthermore, the pH in step S1 is adjusted using hydrochloric acid;

[0012] Furthermore, the number of graphene oxide sheets in step S1 is 15-20 sheets.

[0013] S2: dissolving eugenol and benzophenone in dichloromethane, then adding thiolated graphene oxide, irradiating under ultraviolet light for 3-4 hours, and purifying to obtain modified eugenol;

[0014] Further, in step S2, the weight ratio of eugenol, thiolated graphene oxide, benzophenone and dichloromethane is 1-2:2.5-4.5:0.01:10-20;

[0015] S3: Mixing modified eugenol, allyl bromide, potassium carbonate and acetone, reacting at room temperature for 20-24 hours, extracting, drying and purifying to obtain a pre-reaction monomer;

[0016] Further, in step S3, the weight ratio of the modified eugenol, allyl bromide, potassium carbonate and acetone is 1.6-2:1.3-1.5:1.3-1.4:20-30;

[0017] Furthermore, the extraction in step S3 is performed by adding water and dichloromethane for extraction;

[0018] S4: Methyl methacrylate, hexafluorobutyl methacrylate, butyl acrylate, pre-reaction monomer, 2-methoxyethyl acrylate, acryloyloxyethyl trimethylammonium chloride solution, chain transfer agent MSD, AIBN and DMF are mixed, and slowly added dropwise to DMF under a nitrogen atmosphere, and reacted at 80-90° C. for 5 h. BPO is then dissolved in DMF, and added dropwise to the reaction system, and the temperature is kept constant for 2 h to obtain a modified acrylic resin solution;

[0019] Furthermore, in step S4, the weight ratio of methyl methacrylate, hexafluorobutyl methacrylate, butyl acrylate, 2-methoxyethyl acrylate, acryloyloxyethyl trimethylammonium chloride solution, pre-reaction monomer, chain transfer agent MSD, AIBN and BPO is 14-15: 2.5-3: 7-8: 0.6-1: 2-3: 1-1.2: 0.04-0.06: 0.05-0.06: 0.01.

[0020] Furthermore, the pigment filler is one of organic bentonite, barium sulfate, red iron oxide, zinc oxide, and silicon dioxide.

[0021] Furthermore, the organic solvent is xylene.

[0022] Furthermore, the dispersant is one of BYK103, BYK104, BYK163 and BYK104S.

[0023] Furthermore, the defoaming agent is one of BYK051, BYK052 and BYK066.

[0024] Furthermore, the leveling agent is one of Levaslip435 and BYK354.

[0025] Furthermore, the solid content of the modified acrylic resin solution is 45-50%.

[0026] Furthermore, the present invention also provides a method for preparing an acrylic resin coating for marine engineering, comprising the following steps:

[0027] The above raw materials are mixed according to proportions and stirred evenly to obtain acrylic resin coating for marine engineering.

[0028] Beneficial effects of the present invention:

[0029] (1) The present invention introduces eugenol, quaternary ammonium cationic groups and graphene oxide by synthesizing modified acrylic resin, so that the coating has excellent antibacterial and antifouling properties, and can be released continuously for a long time, and has excellent long-lasting antifouling properties.

[0030] (2) The present invention adds modified graphene oxide by grafting, so that the graphene oxide is dispersed more evenly, so that the mechanical properties of the coating, such as adhesion, are improved, and a smoother and more uniform coating surface can be formed, thereby reducing the surface energy, reducing the chance of adhesion of pollutants, and improving the anti-fouling performance.

[0031] (3) The present invention grafts thiolated graphene oxide onto the surface of eugenol and then participates in the cross-linking of acrylate. Although the mechanical properties of the coating are slightly reduced compared to grafting eugenol and graphene onto the main chain of acrylate, the hydrolysis rate of the main chain is greatly reduced compared to grafting eugenol and graphene onto the main chain of acrylate, thereby increasing the durability of the coating. At the same time, the eugenol and graphene oxide in the side chains can better play an anti-fouling role. DETAILED DESCRIPTION

[0032] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0033] The graphene oxide used in the examples and comparative examples of the present invention was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with the item number G476611; 11-mercaptoundecyltrimethoxysilane was purchased from Shanghai Myrel Biochemical Technology Co., Ltd.

[0034] Example 1: An acrylic resin coating for marine engineering, the specific preparation steps are as follows:

[0035] (1) 2 g of graphene oxide was mixed with 1400 g of ethanol and ultrasonicated for 1 h to obtain a graphene oxide dispersion; then 15 g of 11-mercaptoundecyltrimethoxysilane was dissolved in 1400 g of ethanol, the pH was adjusted to 3.5 with hydrochloric acid, and the mixture was allowed to stand for 1 h. The mixture was then mixed with the graphene oxide dispersion and reacted at 20 °C for 20 h. The mixture was centrifuged, washed, and dried to obtain thiolated graphene oxide;

[0036] (2) Dissolve 1 g of eugenol and 0.01 g of benzophenone in 10 g of dichloromethane, then add 2.5 g of thiolated graphene oxide, irradiate under ultraviolet light for 3-4 h, and purify to obtain modified eugenol;

[0037] (3) 1.6 g of modified eugenol, 1.3 g of allyl bromide, 1.3 g of potassium carbonate and 20 g of acetone were mixed, reacted at room temperature for 20 h, extracted, dried and purified to obtain a pre-reaction monomer;

[0038] (4) 14 g of methyl methacrylate, 2.5 g of hexafluorobutyl methacrylate, 7 g of butyl acrylate, 1 g of pre-reaction monomer, 0.6 g of 2-methoxyethyl acrylate, 2 g of acryloyloxyethyl trimethylammonium chloride solution, 0.04 g of chain transfer agent MSD, 0.05 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 80° C. for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant for 2 h to obtain a modified acrylic resin solution with a solid content of 45%;

[0039] (5) Mix 60 g of modified acrylic resin solution, 5 g of organic bentonite, 20 g of xylene, 2 g of BYK103, 2 g of BYK052, and 1 g of Levaslip435, and stir evenly to obtain an acrylic resin coating for marine engineering.

[0040] Example 2: An acrylic resin coating for marine engineering, the specific preparation steps are as follows:

[0041] (1) 3 g of graphene oxide was mixed with 1450 g of ethanol and ultrasonicated for 1 h to obtain a graphene oxide dispersion; then 18 g of 11-mercaptoundecyltrimethoxysilane was dissolved in 1450 g of ethanol, the pH was adjusted to 3.8 with hydrochloric acid, and the mixture was allowed to stand for 1 h. The mixture was then mixed with the graphene oxide dispersion and reacted at 25 °C for 22 h. The mixture was centrifuged, washed, and dried to obtain thiolated graphene oxide;

[0042] (2) 1.5 g of eugenol and 0.01 g of benzophenone were dissolved in 15 g of dichloromethane, and then 3.5 g of thiolated graphene oxide was added. The mixture was irradiated under ultraviolet light for 4 h and purified to obtain modified eugenol.

[0043] (3) 1.8 g of modified eugenol, 1.4 g of allyl bromide, 1.4 g of potassium carbonate and 26 g of acetone were mixed, reacted at room temperature for 22 h, extracted, dried and purified to obtain a pre-reaction monomer;

[0044] (4) 14.5 g of methyl methacrylate, 2.8 g of hexafluorobutyl methacrylate, 7.5 g of butyl acrylate, 1.1 g of pre-reaction monomer, 0.8 g of 2-methoxyethyl acrylate, 2.5 g of acryloyloxyethyl trimethylammonium chloride solution, 0.05 g of chain transfer agent MSD, 0.05 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 85° C. for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant and the mixture was reacted for 2 h to obtain a modified acrylic resin solution with a solid content of 48%;

[0045] (5) Mix 70 g of modified acrylic resin solution, 4 g of red iron oxide, 18 g of xylene, 2 g of BYK103, 1 g of BYK052, and 1 g of Levaslip435, and stir evenly to obtain an acrylic resin coating for marine engineering.

[0046] Example 3: An acrylic resin coating for marine engineering, the specific preparation steps are as follows:

[0047] (1) 3 g of graphene oxide was mixed with 1480 g of ethanol and ultrasonicated for 1 h to obtain a graphene oxide dispersion; then 18 g of 11-mercaptoundecyltrimethoxysilane was dissolved in 1480 g of ethanol, the pH was adjusted to 3.9 with hydrochloric acid, and the mixture was allowed to stand for 1 h. The mixture was then mixed with the graphene oxide dispersion and reacted at 28 °C for 23 h. The mixture was centrifuged, washed, and dried to obtain thiolated graphene oxide;

[0048] (2) 1.8 g of eugenol and 0.01 g of benzophenone were dissolved in 20 g of dichloromethane, followed by adding 4 g of thiolated graphene oxide, irradiating under ultraviolet light for 4 h, and purifying to obtain modified eugenol;

[0049] (3) 1.8 g of modified eugenol, 1.4 g of allyl bromide, 1.4 g of potassium carbonate and 27 g of acetone were mixed and reacted at room temperature for 21 h, and then extracted, dried and purified to obtain a pre-reaction monomer;

[0050] (4) 15 g of methyl methacrylate, 2.5 g of hexafluorobutyl methacrylate, 8 g of butyl acrylate, 1 g of pre-reaction monomer, 1 g of 2-methoxyethyl acrylate, 3 g of acryloyloxyethyl trimethylammonium chloride solution, 0.04 g of chain transfer agent MSD, 0.06 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 87°C for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant for 2 h to obtain a modified acrylic resin solution with a solid content of 49%;

[0051] (5) Mix 72 g of modified acrylic resin solution, 5 g of organic bentonite, 20 g of xylene, 1 g of BYK103, 2 g of BYK052, and 1 g of Levaslip435, and stir evenly to obtain an acrylic resin coating for marine engineering.

[0052] Example 4: An acrylic resin coating for marine engineering, the specific preparation steps are as follows:

[0053] (1) 4 g of graphene oxide was mixed with 1500 g of ethanol and ultrasonicated for 1 h to obtain a graphene oxide dispersion; then 20 g of 11-mercaptoundecyltrimethoxysilane was dissolved in 1500 g of ethanol, the pH was adjusted to 4 with hydrochloric acid, and the mixture was allowed to stand for 1 h. The mixture was then mixed with the graphene oxide dispersion and reacted at 30 ° C for 24 h. The mixture was centrifuged, washed, and dried to obtain thiolated graphene oxide;

[0054] (2) 2 g of eugenol and 0.01 g of benzophenone were dissolved in 20 g of dichloromethane, followed by the addition of 4.5 g of thiolated graphene oxide, irradiation under ultraviolet light for 4 h, and purification to obtain modified eugenol;

[0055] (3) 2 g of modified eugenol, 1.5 g of allyl bromide, 1.4 g of potassium carbonate and 30 g of acetone were mixed, reacted at room temperature for 24 h, extracted, dried and purified to obtain a pre-reaction monomer;

[0056] (4) 15 g of methyl methacrylate, 3 g of hexafluorobutyl methacrylate, 8 g of butyl acrylate, 1.2 g of pre-reaction monomer, 1 g of 2-methoxyethyl acrylate, 3 g of acryloyloxyethyl trimethylammonium chloride solution, 0.06 g of chain transfer agent MSD, 0.06 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 90° C. for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant for 2 h to obtain a modified acrylic resin solution with a solid content of 50%;

[0057] (5) Mix 75 g of modified acrylic resin solution, 3 g of barium sulfate, 15 g of xylene, 1 g of BYK103, 0.5 g of BYK052, and 0.5 g of Levaslip435, and stir evenly to obtain an acrylic resin coating for marine engineering.

[0058] Comparative Example 1: An acrylic resin coating, the specific preparation steps are as follows:

[0059] (1) 1.8 g of eugenol, 1.4 g of allyl bromide, 1.4 g of potassium carbonate and 26 g of acetone were mixed, reacted at room temperature for 22 h, and extracted, dried and purified to obtain a pre-reaction monomer;

[0060] (2) 14.5 g of methyl methacrylate, 2.8 g of hexafluorobutyl methacrylate, 7.5 g of butyl acrylate, 1.1 g of pre-reaction monomer, 0.8 g of 2-methoxyethyl acrylate, 2.5 g of acryloyloxyethyl trimethylammonium chloride solution, 0.05 g of chain transfer agent MSD, 0.05 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 85 °C for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant for 2 h to obtain a modified acrylic resin solution with a solid content of 48%;

[0061] (3) 70 g of modified acrylic resin solution, 4 g of red iron oxide, 18 g of xylene, 2 g of BYK103, 1 g of BYK052, 1 g of Levaslip435 and 3 g of graphene oxide are mixed and stirred evenly to obtain an acrylic resin coating for marine engineering.

[0062] Comparative Example 2: An acrylic resin coating, the specific preparation steps are as follows:

[0063] (1) 3 g of graphene oxide was mixed with 1450 g of ethanol and ultrasonicated for 1 h to obtain a graphene oxide dispersion; then 15 g of KH-570 was dissolved in 1450 g of ethanol, the pH was adjusted to 3.8 with hydrochloric acid, and the mixture was allowed to stand for 1 h. The mixture was then mixed with the graphene oxide dispersion and reacted at 25 °C for 22 h. The modified graphene oxide was obtained by centrifugation, washing, and drying.

[0064] (2) 1.8 g of eugenol, 1.4 g of allyl bromide, 1.4 g of potassium carbonate and 26 g of acetone were mixed, reacted at room temperature for 22 h, and extracted, dried and purified to obtain a pre-reaction monomer;

[0065] (4) 14.5 g of methyl methacrylate, 2.8 g of hexafluorobutyl methacrylate, 7.5 g of butyl acrylate, 1.1 g of pre-reaction monomer, 0.8 g of 2-methoxyethyl acrylate, 2.5 g of acryloyloxyethyl trimethylammonium chloride solution, 3 g of modified graphene oxide, 0.05 g of chain transfer agent MSD, 0.05 g of AIBN and DMF were mixed, and slowly added dropwise to DMF under a nitrogen atmosphere. The mixture was reacted at 85 °C for 5 h. Subsequently, 0.01 g of BPO was dissolved in DMF and added dropwise to the reaction system. The temperature was kept constant for 2 h to obtain a modified acrylic resin solution with a solid content of 48%;

[0066] (5) Mix 70 g of modified acrylic resin solution, 4 g of red iron oxide, 18 g of xylene, 2 g of BYK103, 1 g of BYK052, and 1 g of Levaslip435, and stir evenly to obtain an acrylic resin coating for marine engineering.

[0067] Comparative Example 3: An acrylic resin coating, the specific preparation steps are as follows:

[0068] The difference from Example 2 is that 18 g of 11-mercaptoundecyltrimethoxysilane in step (1) is replaced by 1.2 g of mercaptopropyltrimethoxysilane, and the remaining steps are the same as Example 2.

[0069] Performance Test:

[0070] Coating adhesion: According to the ASTM D4541-09 test standard, a layer of connecting paint was applied to the surface of the epoxy resin board. After drying, the samples obtained in the embodiment and the comparative example were evenly coated on the surface of the epoxy primer with a thickness of about 150 μm. Five positions were randomly selected for testing, and the test results were averaged. The test results are shown in Table 1.

[0071] Coating hardness: According to the ASTM D3363 test standard, a set of Chinese drawing pencils is used, and the hardness grades include: 6B-5B-4B-3B-2B-B-HB-H-2H-3H-4H-5H-6H. Each sample is measured 5 times and the difference between the results each time does not exceed one pencil grade unit. The result is reliable. The test results are shown in Table 1.

[0072] Determination of coating weight loss rate: Take a stainless steel sheet of size 2.5 cm×1.8 cm, clean the surface with ethanol and dry it, weigh the mass of the stainless steel sheet with an analytical balance, record it as w0; then spin-coat the samples obtained in the embodiment and comparative example on the surface of the stainless steel sheet, and weigh the mass of the steel sheet with the polymer coating after drying, record it as w1. Soak the steel sheet in a fish tank filled with artificial seawater at room temperature, take it out after 30 days, rinse the surface with water, soak it in deionized water for 30 minutes with ultrasound to remove impurities such as sea salt, dry it, and measure the mass of the stainless steel sheet, w2. The calculation formula of the percentage W (%) of the remaining mass after the coating is soaked and lost weight is as follows:

[0073] ,

[0074] The test results are shown in Table 1.

[0075] Test of the coating's ability to inhibit bacterial adhesion: Escherichia coli was selected as the model bacteria for the experiment. The specific operation is as follows:

[0076] (1) The samples obtained in the examples and comparative examples were evenly coated on the surface of a glass slide, and after drying, they were irradiated with ultraviolet light for 30 minutes to fully sterilize;

[0077] (2) The samples obtained in the examples and comparative examples were then coated in a culture dish that had also been irradiated with an ultraviolet lamp, and 10 mL of Luria Bertani (LB) liquid culture medium and a certain concentration of bacterial solution were added. The addition ratio was adjusted so that the concentration of the bacterial solution was 10 5 -10 6 CFU / mL. Seal the surface dish with sealing film and place it in a constant temperature incubator (37°C) for 24 hours.

[0078] (3) Place the culture dish in a culture dish sterilization barrel, dry-heat sterilize in an oven at 160°C for 4 hours, pour hot solid culture medium into the culture dish, cool it under ultraviolet light, turn it upside down, and seal it with sealing film for later use. Heat and sterilize the metal tweezers over the flame of an alcohol lamp and cool it. Then use the tweezers to remove the sample piece from the culture dish after the culture is completed. Slowly rinse the coating surface with 20mL LB culture medium to remove the residual bacterial solution, then quickly rinse the coating with 10mL liquid culture medium, and then dilute the 10mL culture solution that has been rinsed to the original 10 3Then take 10 μL of the dilution and spread it evenly on the solid culture medium. After spreading evenly, put it into a constant temperature and light incubator at 37℃ for 12-24h, take pictures and count.

[0079] The number of bacteria on the coating surface was determined by the plate counting method. The number of bacteria adhering to the surface of the test sample was recorded as N1, and the number of bacteria adhering to the surface of the control blank sample was recorded as N2. The inhibition efficiency of the coating on bacterial adhesion (A) was calculated by the following formula. Each group of samples was tested three times and the average value was taken. The test results are shown in Table 1.

[0080] ,

[0081] The bacterial growth concentration was calculated by measuring the absorbance using an ultraviolet spectrophotometer, and the bacterial liquid concentration was calculated by the OD value at a wavelength of 600 nm.

[0082] Coating antifouling performance test: The samples obtained in the embodiment and the comparative example were respectively coated on low-carbon steel plates with epoxy anticorrosive primer to make samples. After being fully dried at room temperature, a shallow sea hanging test was carried out. Each test sample and a blank control sample were placed at a depth of 1m below the sea level for a static real sea hanging test. The test site was the sea area of ​​Qingdao City, Shandong Province. The test results are shown in Table 1.

[0083] Table 1 Performance test results:

[0084]

[0085] Data analysis shows that the acrylic resin coating for marine engineering of the present invention has good adhesion and hardness after coating, and its mechanical properties can meet the requirements of actual use. In addition, it has excellent antibacterial and antifouling properties, and can achieve long-term sustained release, and has good lasting antifouling effect.

[0086] It can be seen from Example 2 and Comparative Example 1 that the modified graphene oxide is added by grafting, which can participate in the cross-linking process of acrylate, so that the graphene oxide can be dispersed more evenly, and its agglomeration can be prevented, so that the mechanical properties such as adhesion of the coating are improved; and the evenly dispersed and stably bonded graphene oxide helps to form a smoother and more uniform coating surface, reduces the chance of adhesion of pollutants, and improves the anti-fouling performance.

[0087] It can be seen from Example 2 and Comparative Examples 1 and 2 that by grafting thiolated graphene oxide onto the surface of eugenol and then participating in the cross-linking of acrylate, eugenol and graphene oxide are both on the side chains of the cross-linked network. Although the mechanical properties of the coating are slightly reduced compared to grafting both eugenol and graphene onto the main chain of acrylate, the hydrolysis rate of the main chain is greatly reduced compared to grafting both eugenol and graphene onto the main chain of acrylate, so that the durability of the coating is increased. At the same time, eugenol and graphene oxide on the side chains can better play an anti-fouling role. This may be because when graphene is on the main chain, its activity is restricted, and when it is on the side chain of the network, its ability to kill bacteria is stronger, thereby improving the anti-fouling performance of the coating.

[0088] It can be seen from Example 2 and Comparative Example 3 that, compared with short chains, longer side chains can better exert the antibacterial and antifouling properties of graphene oxide. This is probably because longer side chains make the scope of action of graphene oxide wider, thereby causing greater damage to bacteria such as Escherichia coli.

[0089] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0090] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An acrylic resin coating for marine engineering, It is characterized in that The invention comprises the following raw materials in parts by weight: 60-75 parts of modified acrylic resin solution, 3-5 parts of pigments and fillers, 15-20 parts of organic solvents, 1-2 parts of dispersants, 0.5-2 parts of defoamers, and 0.5-1 parts of leveling agents; The preparation steps of the modified acrylic resin solution are as follows: S1: Mixing graphene oxide with ethanol, ultrasonicating for 1 h to obtain a graphene oxide dispersion; then dissolving 11-mercaptoundecyltrimethoxysilane in ethanol, adjusting the pH to 3.5-4, standing for 1 h, and then mixing it with the graphene oxide dispersion, reacting at 20-30°C for 20-24 h, centrifuging, washing, and drying to obtain thiolated graphene oxide; S2: dissolving eugenol and benzophenone in dichloromethane, then adding thiolated graphene oxide, irradiating under ultraviolet light for 3-4 hours, and purifying to obtain modified eugenol; S3: Mixing modified eugenol, allyl bromide, potassium carbonate and acetone, reacting at room temperature for 20-24 hours, extracting, drying and purifying to obtain a pre-reaction monomer; S4: Methyl methacrylate, hexafluorobutyl methacrylate, butyl acrylate, pre-reaction monomer, 2-methoxyethyl acrylate, acryloyloxyethyl trimethylammonium chloride solution, chain transfer agent MSD, AIBN and DMF are mixed, and slowly added dropwise into DMF under a nitrogen atmosphere, and reacted at 80-90°C for 5 hours. Subsequently, BPO is dissolved in DMF, and added dropwise into the reaction system, and the temperature is kept constant for 2 hours to obtain a modified acrylic resin solution.

2. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The weight ratio of graphene oxide, 11-mercaptoundecyltrimethoxysilane and ethanol in step S1 is 0.2-0.4:1.5-2:280-300.

3. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The weight ratio of eugenol, thiolated graphene oxide, benzophenone and dichloromethane in step S2 is 1-2:2.5-4.5:0.01:10-20.

4. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The weight ratio of the modified eugenol, allyl bromide, potassium carbonate and acetone in step S3 is 1.6-2:1.3-1.5:1.3-1.4:20-30.

5. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that In step S4, the weight ratio of methyl methacrylate, hexafluorobutyl methacrylate, butyl acrylate, 2-methoxyethyl acrylate, acryloyloxyethyl trimethylammonium chloride solution, pre-reaction monomer, chain transfer agent MSD, AIBN and BPO is 14-15: 2.5-3:7-8:0.6-1:2-3:1-1.2:0.04-0.06:0.05-0.06:0.01。 6. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The solid content of the modified acrylic resin solution is 45-50%.

7. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The pigment filler is one of organic bentonite, barium sulfate, red iron oxide, zinc oxide and silicon dioxide.

8. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The organic solvent is xylene.

9. The acrylic resin coating for marine engineering according to claim 1, It is characterized in that The dispersant is one of BYK103, BYK104, BYK163 and BYK104S.

10. A method for preparing an acrylic resin coating for marine engineering according to any one of claims 1 to 9, It is characterized in that The following steps are involved: The above raw materials are mixed according to proportions and stirred evenly to obtain acrylic resin coating for marine engineering.

Citation Information

Patent Citations

  • Self-polishing graphene antifouling paint and preparation method thereof

    CN113150628A

  • Self-polishing antifouling paint embedded with crushed Chinese prickly ash and preparation method and application of self-polishing antifouling paint

    CN115216194A

  • Preparation method for in-situ generation of hydrophobic antifouling coating through grafted modified graphene

    CN109536013A

  • Eugenol-based curing agent based on thiol-ene click reaction for epoxy resin as well as preparation method and application of curing agent

    CN110643019A

  • Preparation method of self-polishing, corrosion-resistant, antibacterial, self-repairing and low-surface-energy coating material

    CN117210107A