Paper-plastic product with efficient barrier coating and manufacturing method of paper-plastic product
By introducing wet strength agents, in-pulp sizing agents and stiffeners into pulp molded products, and using silicone coatings to form surface coatings, the problem of poor moisture and oxygen barrier properties of pulp molded products has been solved and achieved Wider application range and higher barrier effect.
Patent Information
- Application Number
- CN202411001406.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-09-24
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to the limitations of its own manufacturing process and raw materials, pulp molded products cannot effectively block moisture and oxygen, resulting in a limited range of use, especially in packaging fluids, pharmaceuticals, cosmetics and other products that require high sealing and barrier properties. The occasion cannot be met.
A method for manufacturing paper and plastic products with high-efficiency barrier coating is adopted. Wet strength agent, in-slurry sizing agent and stiffening agent are introduced into the fiber slurry, and materials such as silicone coating are added during the manufacturing process to form a surface coating. layer, filling the gaps between fibers to improve the sealing and barrier properties of the product.
Significantly improves the barrier properties of paper-plastic products, reduces oxygen permeability and water vapor permeability, expands its application scope, and enables it to meet the packaging needs of fluids, drugs, cosmetics and other products, while maintaining excellent biodegradability and environmental friendliness.
Smart Images

Figure CN118686018A
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pulp molding production, and in particular to a paper-plastic product with a high-efficiency barrier coating and a manufacturing method thereof. Background Art
[0002] Pulp molding products are made of waste paper, bamboo pulp, sugarcane pulp, and wood pulp fibers. After pulping, refining, mixing, vacuum suction filtration, wet embryos are made, and then hot-pressed to form paper-plastic products. No adhesive is required in the production process of the pulp molding products. They are formed only by the interaction of the fibers themselves and the structure of the mold itself. They can be made into various shapes and structures with complex shapes and high dimensional accuracy. The paper-plastic products have excellent biodegradable properties, are environmentally friendly, and can be recycled.
[0003] However, since the main raw materials of pulp molded products are various fiber products, during the manufacturing process, a three-dimensional network space structure is formed by the interweaving of fibers. There are a large number of gaps between the fibers, allowing air and liquid to flow freely between the inside and outside, which is suitable for packaging of electronic products and other products that do not require barrier. For products and fluids that are easy to oxidize and have shelf life requirements, the pulp molded products cannot be used as a suitable packaging carrier to carry these products and fluids due to their own manufacturing and molding process and raw material limitations. In order to expand the scope of use of pulp molded products, especially to apply pulp molded products to the packaging of fluids, drugs, cosmetics and other products that have high requirements for the sealing and barrier properties of packaging containers, it is urgent to develop a pulp molded product with high efficiency barrier effect; at the same time, in order to meet the urgent requirements of environmental protection, the pulp molded product is also required to have excellent biodegradability and environmental friendliness, so that the pulp molded product can be used as a new choice to replace plastic products and be widely used in the packaging of fluids, drugs, cosmetics and other products. In order to meet the above requirements, it is necessary to optimize and upgrade the current manufacturing methods and processes of pulp molding products so that the manufactured paper-molded products can meet the above new requirements.
[0004] As a natural renewable resource, natural fiber has a large number of hydroxyl groups on its surface, and these hydroxyl groups are very easy to combine with water molecules to form a large number of hydrogen bonds, making the fiber surface extremely easy to absorb water and have good hygroscopicity; at the same time, the fibers are interwoven with each other through hydrogen bonds to form a three-dimensional network overall spatial structure, resulting in a large number of gaps between the fibers and excellent air permeability. The pulp molding product itself is a porous structure composed of fibers of long-chain cellulose molecules interwoven through the network. On the one hand, due to the large number of hydroxyl groups in the basic unit of cellulose, cellulose itself has hydrophilicity. On the other hand, due to the porosity of the three-dimensional network formed by the interweaving of fibers, there are many gaps between the fibers. Due to the effect of concentration gradient, gas can pass through the gaps, which leads to high air permeability and moisture permeability of paper and plastic products, thereby limiting the barrier performance of paper and plastic products to moisture and oxygen.
[0005] In order to improve the above-mentioned undesirable problems of pulp molded products, the present invention proposes a paper-molded product with a high-efficiency barrier coating and a method for manufacturing the same, so as to solve the problem in the prior art that pulp molded products have poor barrier properties against moisture and oxygen, resulting in limited use of pulp molded products. Summary of the invention
[0006] The purpose of the present invention is to provide a paper-plastic product with a high-efficiency barrier coating and a method for manufacturing the same, so as to solve the problem in the prior art that pulp molded products have poor barrier properties to moisture and oxygen, resulting in a limited scope of use of pulp molded products.
[0007] The technical solution of the present invention is: a method for manufacturing a paper-plastic product with a high-efficiency barrier coating, the manufacturing steps comprising:
[0008] S1. Weigh fiber slurry and a combination of additives, and prepare the weighed fiber slurry and the combination of additives into a paper-plastic semi-finished product; the fiber slurry includes at least one of wood pulp, sugarcane pulp, and bamboo pulp; the mass ratio of wood pulp, sugarcane pulp, and bamboo pulp in the fiber slurry is (0-10): (0-3.5): (0-6.5); the combination of additives includes a wet strength agent and an internal sizing agent; the wet strength agent is a thermosetting cationic wet strength agent, and the mass percentage of the wet strength agent in the fiber slurry is not less than 3%; the internal sizing agent is a cationic internal sizing agent, and the mass percentage of the internal sizing agent in the fiber slurry is not less than 3%;
[0009] S2. Using an organic solvent as a diluent, preparing a coating material to form a dipping liquid, and placing the dipping liquid in a containing tank; the coating material is one of an organic silicone coating, a high-temperature polyester coating, and a thermoplastic powder coating;
[0010] S3, immersing the paper-plastic semi-finished product prepared in step S1 in the dipping liquid for dipping, wherein the dipping time is controlled within 2-10 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0011] S4, placing the semi-finished paper-plastic product with the surface coated with the dipping liquid into a drying container for drying, and taking it out after drying to obtain a paper-plastic product with a coating on the surface.
[0012] Preferably,
[0013] The organosilicon coating is one of an organosilicon resin coating and a modified organosilicon resin coating;
[0014] The high temperature polyester coating is one of epoxy resin, phenolic resin and polyimide resin;
[0015] The thermoplastic powder coating is one of acrylic polymer, perchlorethylene paint, polyethylene and polyamide coating.
[0016] Preferably, the organic solvent is one of butyl acetate, ethyl cellosolve, methanol, ethanol, isopropanol, and butanol;
[0017] The concentration of the coating material in the dipping solution is 20%-65%.
[0018] Preferably, the concentration of the coating material in the dipping liquid is 25%-45%.
[0019] Preferably, in S2, the receiving groove is a geometric polygonal structure;
[0020] The geometric polygons include triangles, trapezoids, pentagons, and hexagons;
[0021] The receiving tank is placed horizontally or tilted;
[0022] In S3, during dipping, the paper-plastic semi-finished product and the containing tank move relative to each other;
[0023] In the step S4, the drying process is performed at a temperature of 60-110° C. and a drying time of 1-5 min.
[0024] Preferably, the dipping time is 3-5 s; the drying temperature is 80-100° C.; and the drying time is 2-3 min.
[0025] Preferably, the combination of auxiliary agents also includes a bactericide and a stiffening agent;
[0026] The bactericide is a small molecule compound;
[0027] The stiffening agent is preferably a stiffening agent with a positive charge;
[0028] Calculated by the mass percentage of the fiber slurry, the addition ratio of the wet strength agent is 3.5-7%, the addition ratio of the bactericide is 0.1-0.3%, the addition ratio of the stiffening agent is 0.2-1%, and the addition ratio of the internal sizing agent is 3-6%.
[0029] Preferably, the fiber pulp is a combination of wood pulp, sugarcane pulp and bamboo pulp;
[0030] The mass ratio of wood pulp, sugarcane pulp and bamboo pulp in the fiber pulp is (0-6):(2-3.5):(2-6.5).
[0031] Preferably, the fiber pulp is wood pulp;
[0032] The wood pulp is coniferous wood pulp; calculated by the mass percentage of the fiber pulp, the addition ratio of the wet strength agent is 5.5%, the addition ratio of the fungicide is 0.16%, the addition ratio of the stiffener is 8%, and the addition ratio of the internal sizing agent is 5.5%.
[0033] Preferably, the steps of preparing the paper-plastic semi-finished product include:
[0034] a. Add the fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add the fiber slurry to slurry to obtain a first solution;
[0035] b. adding a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0036] c. Add the wet strength agent to the second solution, mix well, then add the sizing agent in the slurry, mix well, and obtain paper-plastic slurry;
[0037] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0038] Preferably, the fungicide needs to be diluted 30-50 times with clean water before addition; the stiffener needs to be diluted 50-80 times with clean water before addition; the wet strength agent needs to be diluted 10-20 times with clean water before addition; and the sizing agent in the slurry needs to be diluted 30-50 times with clean water before addition.
[0039] The present invention also provides a paper-plastic product with a high-efficiency barrier coating, and the paper-plastic product is prepared by the above-mentioned manufacturing method.
[0040] Compared with the prior art, the advantages of the present invention are:
[0041] (1) The present invention provides a paper plastic product with a high-efficiency barrier coating and a manufacturing method thereof. By optimizing the manufacturing process of existing pulp molded products, a surface coating is introduced to fill the gaps between fibers. The fiber is used as a skeleton structure, and a coating material is used as a gap filling auxiliary agent. A layer of coating material is coated on the fiber surface, which not only fills the gap to reduce air permeability, but also improves the sealing and barrier properties of the product, and at the same time improves the physical strength and surface properties of the paper plastic product. The paper plastic product not only has high overall strength, but also has excellent barrier properties, which expands the application range of the paper plastic product and solves the problem that the existing pulp molded product has poor barrier properties to moisture and oxygen, which limits the application range of the pulp molded product.
[0042] (2) The present invention provides a paper-plastic product with a high-efficiency barrier coating and a method for manufacturing the same. In the process of manufacturing the paper-plastic semi-finished product, by selecting and optimizing the fiber slurry and introducing a combination of additives, and by adjusting the addition ratio of the combination of additives and controlling the addition order of the combination of additives, the characteristics of each additive and the superposition of the effects of the combination of additives can be fully utilized, thereby maximizing the effect of the combination of additives in the process of manufacturing the paper-plastic semi-finished product. The combined use of in-slurry sizing agent, wet strength agent and stiffening agent, as well as increasing the addition ratio of wet strength agent and in-slurry sizing agent, can make the paper-plastic semi-finished product have good water resistance. When the paper-plastic semi-finished product is placed in the dipping liquid for dipping, the dipping liquid can be effectively prevented from penetrating into the interior of the paper-plastic semi-finished product, so that the dipping liquid can only stay on the surface of the paper-plastic semi-finished product; at the same time, the good water resistance of the paper-plastic semi-finished product can also effectively prevent the paper-plastic semi-finished product from absorbing water, stretching or deforming during dipping, thereby reducing the defective rate; in addition, the combined use of combined additives also improves the surface hardness index and overall strength performance of the paper-plastic product, thereby expanding the scope of use of the paper-plastic product and reducing the restrictions on the product during use.
[0043] (3) The present invention provides a paper-plastic product with a high-efficiency barrier coating and a method for manufacturing the same. In the process of manufacturing a paper-plastic semi-finished product with a high-efficiency barrier coating through manufacturing processes such as dipping and drying, the coating weight per square meter on the surface of the paper-plastic product can be adjusted by regulating the dipping time, drying temperature and drying time, thereby reducing the oxygen permeability and water vapor permeability of the paper-plastic product and improving the barrier performance of the paper-plastic product.
[0044] (4) The present invention provides a paper-plastic product with a high-efficiency barrier coating and a method for manufacturing the same, wherein the receiving groove used is a geometric polygonal structure, and the receiving groove is placed horizontally or tilted, so that it can not only be used for dipping paper-plastic semi-finished products with different structures or shapes, but also each surface of the paper-plastic semi-finished product can be dipped into the dipping liquid; in addition, when the paper-plastic semi-finished product is immersed in the dipping liquid, it can move relative to the receiving groove, so that the dipping liquid on the surface of the paper-plastic semi-finished product is more evenly distributed; thereby, the surface coating of the manufactured paper-plastic product with a high-efficiency barrier coating has excellent uniformity and flatness. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0046] Figure 1 This is a process principle diagram of the paper-plastic manufacturing process of the present invention;
[0047] Figure 2 It is a process flow chart of the paper-plastic manufacturing process of the present invention; DETAILED DESCRIPTION
[0048] The content of the present invention is further described in detail below in conjunction with specific embodiments, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0049] It should be further explained that the fiber slurry in the embodiment of the present invention is initially in a dry pulp board state, and the "mass ratio, mass parts" in the present invention correspond to the dry weight of the fiber slurry and the initial state of each auxiliary product, and have nothing to do with the amount of water added, the dilution multiple, and the composition of each auxiliary. The dilution multiple of each auxiliary in the present invention includes but is not limited to the dilution multiple in the embodiment, as long as each auxiliary can exert its effect. The concentration of the coating material in the dipping solution in the embodiment of the present invention refers to the mass concentration of the coating material after dilution with the diluent.
[0050] A method for manufacturing a paper-plastic product with a high-efficiency barrier coating, such as Figure 1 As shown, the manufacturing method thereof comprises the following steps:
[0051] S1. Weigh fiber pulp and combined auxiliary agents, and prepare the weighed fiber pulp and combined auxiliary agents into a paper-plastic semi-finished product; the fiber pulp includes at least one of wood pulp, sugarcane pulp and bamboo pulp; the mass ratio of wood pulp, sugarcane pulp and bamboo pulp in the fiber pulp is (0-10): (0-3.5): (0-6.5); the combined auxiliary agents include a wet strength agent and an internal sizing agent; the wet strength agent is a thermosetting cationic wet strength agent, and the mass percentage of the wet strength agent in the fiber pulp is not less than 3%; the internal sizing agent is a cationic internal sizing agent, and the mass percentage of the internal sizing agent in the fiber pulp is not less than 3%.
[0052] S2. Use an organic solvent as a diluent to prepare the coating material to form a dipping liquid, and place it in a holding tank; wherein the coating material is one of silicone coating, high-temperature polyester coating, and thermoplastic powder coating; the silicone coating is one of silicone resin coating and modified silicone resin coating; the high-temperature polyester coating is one of epoxy resin, phenolic resin, and polyimide resin; the thermoplastic powder coating is one of acrylic polymer, perchlorethylene paint (PVDC), polyethylene, polyamide and other coatings; the organic solvent is one of butyl acetate, ethyl cellosolve, methanol, ethanol, isopropanol, and butanol; the concentration of the coating material in the dipping liquid is 20%-65%; the holding tank is a geometric polygonal structure, and the geometric polygons include triangles, trapezoids, pentagons, hexagons, etc., but do not include rectangles and squares, and the holding tank can be placed horizontally or tilted; in addition, the holding tank can be in a static state or in a shaking state, and it is best to use manual or mechanical methods to drive the holding tank to shake regularly.
[0053] S3, immersing the paper-plastic semi-finished product prepared in step S1 in the dipping liquid for dipping, the dipping time is controlled within 2-10s, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface; wherein, during the dipping process, the paper-plastic semi-finished product can be suspended by a hook or the like and then immersed but not moved, or the paper-plastic semi-finished product can be driven to move by the hook, so that when the paper-plastic semi-finished product is immersed in the dipping liquid, it moves relative to the containing tank, so that the dipping liquid on the surface of the paper-plastic semi-finished product is more evenly distributed; thereby obtaining a paper-plastic product with a coating having a uniform and flat surface and high-efficiency barrier performance.
[0054] S4. Put the semi-finished paper-plastic product with the surface coated with the dipping liquid into a drying container for drying at a temperature of 60-110° C. for a drying time of 1-5 min. After drying, take it out to obtain a paper-plastic product with a coating on the surface.
[0055] The preparation steps of the paper-plastic semi-finished product include the following steps:
[0056] a. Dilute the fungicide 30-50 times with clean water and add it to a pulping machine containing papermaking white water, stir and mix evenly, then add fiber slurry to slurry and obtain the first solution; select small molecule compounds as fungicides, and dilute the fungicides and directly dissolve them in papermaking white water; papermaking white water is the water discharged from the forming machine net part in the back-end paper-plastic product forming process, which generally contains fine short fibers and additives in pulp; combine with attached Figure 2 As shown, in the present application, white water is discharged from the rear-end forming machine and supplied to the front-end process for reuse; the fiber pulp includes at least one of wood pulp, sugarcane pulp, and bamboo pulp; because the fiber itself contains polar groups, these groups are ionized in the aqueous solution, so that the fiber surface has a negative charge, and thus the whole is negatively charged.
[0057] b. Dilute the stiffener with clean water by 50-80 times and add it to the first solution. After mixing evenly, perform a pulping process to obtain a second solution. The stiffener is preferably a positively charged stiffener. Since the fiber surface is negatively charged, the stiffener surface is positively charged and can be adsorbed on the fiber surface by the attraction of positive and negative charges.
[0058] c. Dilute the wet strength agent with clean water for 10-20 times and add it to the second solution. After mixing evenly, add the pulp sizing agent diluted with clean water for 30-50 times and mix evenly to obtain paper-plastic pulp. The wet strength agent is preferably a cationic wet strength agent. The fiber surface is negatively charged. After pulping, more free anionic groups are exposed. Since the wet strength agent is positively charged, it is adsorbed on the fiber surface through charge adsorption. The internal sizing agent is preferably a cationic internal sizing agent. After the action of the stiffening agent and the wet strength agent, the fiber surface already has partial positive charge. Then, the internal sizing agent with positive charge is added to further adsorb on the fiber surface. After heating, a network structure with spatial staggered connection is formed.
[0059] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0060] In the actual production process, the production batch is generally large. In order to ensure product quality and production continuity, it is necessary to continuously perform operations such as pulping, refining, mixing, and molding. Therefore, after each step, corresponding containers (such as storage barrels, mixing barrels) are used for mixing or temporary storage to facilitate the continuous implementation of each process; in the process from paper-plastic slurry to the molding machine, it is necessary to dilute it and transfer it through corresponding containers after dilution; using containers for mixing, storage, and transfer are all common technical means and cannot be used as a limitation to the technical solution of the present invention.
[0061] In the process of preparing the paper-plastic semi-finished product, the weighed fiber pulp includes at least one of wood pulp, sugarcane pulp and bamboo pulp; the mass ratio of wood pulp, sugarcane pulp and bamboo pulp in the fiber pulp is (0-10):(0-3.5):(0-6.5); further, when the weighed fiber pulp is a combination of wood pulp, sugarcane pulp and bamboo pulp, the mass ratio of wood pulp, sugarcane pulp and bamboo pulp in the fiber pulp is (0-6):(2-3.5):(2-6.5); when the weighed fiber pulp is a single one of wood pulp, sugarcane pulp and bamboo pulp, wood pulp is preferred.
[0062] The weighed combined auxiliary agents include bactericide, wet strength agent, stiffener, and sizing agent in pulp; and, calculated by the mass percentage of the fiber pulp, the addition ratio of the wet strength agent is 3.5-7%, the addition ratio of the bactericide is 0.1-0.3%, the addition ratio of the stiffener is 0.2-1%, and the addition ratio of the sizing agent in pulp is 3-6%.
[0063] Furthermore, the fiber pulp is preferably wood pulp; wherein the wood pulp is preferably coniferous pulp; calculated by mass percentage of the fiber pulp, the addition ratio of the combined additives is preferably 5.5% for the wet strength agent, 0.16% for the fungicide, 8% for the stiffener, and 5.5% for the in-pulp sizing agent.
[0064] 1. Bamboo pulp: As a material between coniferous wood pulp and broadleaf wood pulp, bamboo pulp can give the product excellent physical strength and surface properties.
[0065] 2. Sugarcane pulp: It is an extract from sugarcane, with shorter fiber length and larger diameter. Shorter fiber length will affect the strength and other physical properties of paper and plastic products. Therefore, sugarcane pulp is generally used in paper and plastic products that do not require high hardness and strength, or used together with bamboo pulp and / or wood pulp to manufacture paper and plastic products with higher requirements for physical strength and surface properties by optimizing the ratio.
[0066] 3. Wood pulp: As an excellent papermaking raw material, the average fiber length is 2-3 microns, which is longer than the 1-2μm bamboo pulp fiber and 0.8-1.5μm sugarcane pulp fiber. As the fiber length increases, the degree of interweaving between the fibers will also increase, which will significantly improve the tensile strength and abrasion tear strength of paper-plastic products. In the manufacturing process of paper-plastic products, as the proportion of wood pulp added increases, the physical strength and surface properties of paper-plastic products will also increase.
[0067] 4. Fungicide: Mainly used to reduce the formation of rotten pulp in the production process, purify the entire white water system, and create a suitable working environment for the combined additives to function. Rotten pulp is a string-like substance produced by the reproduction of microorganisms such as bacteria and molds during the pulping process. Generally, papermaking white water contains bacteria or molds. Because the pulp contains carbohydrates, a small amount of protein, hydrolyzed sugars and other substances, which are all nutrient sources for bacteria or molds and are conducive to the reproduction of bacteria or molds, rotten pulp will be produced in the papermaking white water system. However, as a harmful substance in the system, rotten pulp will adhere to the surface of the pipe during the production process, becoming a white or brown viscous state. Over time, it will fall into the system, resulting in poor process and product contamination. Therefore, it is very necessary to add fungicides during the pulping process.
[0068] 5. Wet strength agent: It is mainly used to be adsorbed on the fiber surface. After heating, a spatial network structure is formed between the fibers, which restrains the movement and water absorption and swelling of the fibers. At the same time, the wet strength agent, as a thermosetting resin, forms a hydrophobic spatial network structure after heating, which reduces the moisture absorption and wetting of the fibers and maintains a higher strength of the product.
[0069] 6. Stiffener: Mainly used to improve the hardness of paper and plastic products. Since the surface of the stiffener contains a large number of active groups such as hydroxyl, amide, and carboxyl, when added to the pulp, it is adsorbed on the fiber surface through the adsorption of electric charge and combines with the hydroxyl groups on the fiber surface to form a large number of hydrogen bonds. During the drying process, a large number of cross-linking bonds are formed to achieve the purpose of improving the stiffness and hardness of the product.
[0070] 7. In-slurry sizing agent: Its surface is cationic starch or cationic etherifying agent, and the inside is coated with AKD wax powder, which is adsorbed on the fiber surface through positive and negative charges; during drying, as the temperature rises, the moisture content decreases, and the lactone ring on AKD reacts with the hydroxyl group on the fiber to form an esterification reaction, forming a covalent bond and fixing it on the fiber, forming a stable film on the fiber surface, and the hydrophobic carbon chain faces outward, changing the fiber from hydrophilic to hydrophobic, thereby making the paper plastic product water-resistant.
[0071] 8. Silicone coating: As a thermosetting film-forming agent, it will cross-link itself into a whole during the heating process, forming a dense organic coating on the surface of the product, which can effectively fill the gaps between the fibers and form a uniform barrier coating on the surface, which has good barrier properties for water vapor and oxygen. In addition, the barrier coating has the characteristics of moderate hardness, good wear resistance, water resistance and high density.
[0072] In the process of preparing the paper-plastic semi-finished product, the present invention can select the following types or functions of instruments:
[0073] 1. Pulp dispersing machine: ZZS1-100 cubic meter produced by Zhucheng Xuridong Machinery Co., Ltd. or D type produced by Qinyang Runfeng Machinery Equipment Co., Ltd.; can be used for fully mixing and stirring high-concentration slurry, water and medicines;
[0074] 2. Refiner: XRD-01 type of Xuridong Machinery Co., Ltd. or 654 type of Shandong Xiuqing Environmental Protection Technology Co., Ltd.; used for continuous refining of pulp in the papermaking industry or even refining of waste paper recycled pulp after decomposition.
[0075] In the process of preparing the paper-plastic semi-finished product, the embodiments of the present invention can use the following types or functions of auxiliary agents:
[0076] 1. Wet strength agent: JH-1201 from Qingzhou Jinhao New Materials Co., Ltd. or FT-S70 from Fengtai Environmental Protection Technology (Shandong) Co., Ltd.;
[0077] 2. Stiffeners, such as D001 from Shandong Gaochao Energy Saving and Environmental Protection Technology Co., Ltd. or HD100 from Hangzhou Lin'an Funeng Resin Co., Ltd.;
[0078] 3. Fungicide: JH-8909B from Qingzhou Jinhao New Materials Co., Ltd. or D0025 from Shanghai Dejian Chemical Co., Ltd.;
[0079] 4. Internal sizing agent: JH-AKD200 of Qingzhou Jinhao New Materials Co., Ltd. or DH110 of Qingzhou Dehai Fine Chemical Co., Ltd.;
[0080] 5. Silicone or acrylic polymer emulsion coatings: HA-8400 from Guangzhou Huigu New Materials Technology Co., Ltd., GJ-306 from Guangzhou Silicon Gold New Materials R&D Co., Ltd., JPA-01 and BW-3005FC from Shenzhen Weixin New Materials Co., Ltd.
[0081] The "portions" in the embodiments of the present invention are portions by mass, and the mass of each portion can be confirmed according to actual needs. For example, in each embodiment, each "portion" can be calibrated as 1Kg, and then 40 portions are 40Kg, 0.1 portion is 0.1Kg, and other portions by mass are the same.
[0082] Example 1
[0083] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0084] a. Add 0.1 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 20 parts of sugarcane pulp, 30 parts of bamboo pulp and 50 parts of wood pulp to pulp and obtain a first solution;
[0085] b. mixing the first solution uniformly and then performing a refining process to obtain a second solution;
[0086] c. Add 4 parts of wet strength agent to the second solution, mix well, then add 3 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0087] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0088] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 25%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0089] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 10 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0090] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 65° C. for a drying time of 4.5 min, and taking it out after drying to obtain a paper-plastic product with a coating on the surface, A1.
[0091] Example 2
[0092] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0093] a. adding 100 parts of wood pulp into a pulping machine containing papermaking white water to perform pulping to obtain a first solution;
[0094] b. mixing the first solution evenly and then performing a refining process to obtain a second solution;
[0095] c. Add 4 parts of wet strength agent to the second solution, mix well, then add 3 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0096] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0097] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 45%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0098] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 5 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0099] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 90° C. for 3.5 min. After drying, taking out the product to obtain a paper-plastic product with a coating on the surface, A2.
[0100] Example 3
[0101] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0102] a. Add 0.2 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0103] b. adding 0.1 parts of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0104] c. Add 5 parts of wet strength agent to the second solution, mix well, then add 4 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0105] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0106] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 37%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0107] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 6 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0108] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying, the drying temperature is 100° C., the drying time is 3 min, and after drying, taking it out to obtain a paper-plastic product with a coating on the surface, A3.
[0109] Example 4
[0110] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0111] a. Add 0.2 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0112] b. adding 0.5 parts of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0113] c. Add 3 parts of wet strength agent to the second solution, mix well, then add 5 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0114] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0115] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 42%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0116] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 4 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0117] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 85° C. for 3 minutes, and taking it out after drying to obtain a paper-plastic product with a coating on the surface, A4.
[0118] Example 5
[0119] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0120] a. Add 0.15 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0121] b. adding 0.7 parts of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0122] c. Add 3 parts of wet strength agent to the second solution, mix well, then add 3 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0123] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0124] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 45%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0125] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 5 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0126] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 80° C. for 3 minutes, and taking it out after drying to obtain a paper-plastic product with a coating on the surface, A5.
[0127] Example 6
[0128] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0129] a. Add 0.2 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0130] b. adding 1.0 part of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0131] c. Add 6 parts of wet strength agent to the second solution, mix well, then add 4 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0132] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0133] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 45%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0134] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 5 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0135] S4. Put the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 90° C. for 2.5 min. Take it out after drying to obtain a paper-plastic product with a coating on the surface, A6.
[0136] Example 7
[0137] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0138] a. Add 0.3 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0139] b. adding 0.8 parts of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0140] c. Add 7 parts of wet strength agent to the second solution, mix well, then add 6 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0141] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0142] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 40%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0143] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 4 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0144] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a drying temperature of 105° C. for 1.5 min. After drying, taking out the paper-plastic product to obtain a paper-plastic product with a coating on the surface, A7.
[0145] Example 8
[0146] S1. Weigh fiber slurry and combined auxiliary agent according to proportion, and prepare the weighed fiber slurry and combined auxiliary agent into a paper-plastic semi-finished product; wherein the preparation steps of the paper-plastic semi-finished product include the following steps:
[0147] a. Add 0.16 parts of fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add 100 parts of wood pulp and pulp to obtain a first solution;
[0148] b. adding 0.8 parts of a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution;
[0149] c. Add 5.5 parts of wet strength agent to the second solution, mix well, then add 5.5 parts of internal sizing agent, mix well, and obtain paper plastic slurry;
[0150] d. The paper plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper plastic semi-finished product.
[0151] S2, preparing an organic silicon coating to form a dipping solution, the concentration of the dipping solution is 40%, and placing the dipping solution in a receiving tank having a side wall and a bottom wall in a geometric polygonal structure;
[0152] S3, immersing the prepared paper-plastic semi-finished product in the dipping liquid for dipping, the dipping time is 3.5 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface;
[0153] S4, putting the paper-plastic product with the coating liquid on the surface into a drying container for drying at a temperature of 90° C. for 2.5 min. After drying, taking out the product to obtain a paper-plastic product with a coating on the surface, A8.
[0154] Comparative Example 1
[0155] a. adding 35 parts of sugarcane pulp and 65 parts of bamboo pulp into a pulping machine filled with papermaking white water to perform pulping to obtain a first solution;
[0156] b. mixing the first solution uniformly and then performing a refining process to obtain a second solution;
[0157] c. Add 4 parts of the internal sizing agent into the second solution and mix well to obtain a paper-plastic slurry;
[0158] d. The paper-plastic slurry is diluted, slurry-fed, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper-plastic semi-finished product, B1.
[0159] Comparative Example 2
[0160] a. adding 20 parts of sugarcane pulp, 30 parts of bamboo pulp and 50 parts of wood pulp into a pulping machine containing papermaking white water to perform pulping to obtain a first solution;
[0161] b. mixing the first solution uniformly and then performing a refining process to obtain a second solution;
[0162] c. Add 5 parts of the internal sizing agent into the second solution and mix well to obtain a paper-plastic slurry;
[0163] d. The paper-plastic slurry is diluted, slurry-fed, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper-plastic semi-finished product, B2.
[0164] Comparative Example 3
[0165] a. adding 100 parts of wood pulp into a pulping machine containing papermaking white water to perform pulping to obtain a first solution;
[0166] b. mixing the first solution uniformly and then performing a refining process to obtain a second solution;
[0167] c. Add 4 parts of the internal sizing agent into the second solution and mix well to obtain a paper-plastic slurry;
[0168] d. The paper-plastic slurry is diluted, supplied with slurry, wet-molded on a molding machine, hot-pressed and shaped, and dried to obtain a paper-plastic semi-finished product, B3.
[0169] The paper plastic products A1-A8 and B1-B3 prepared in the examples of the present invention and the comparative examples were tested for thickness, surface strength, stiffness, oxygen permeability and air permeability. The data are shown in Table 1.
[0170] Table 1: Comparison of test data of paper plastic products A1-A8 and B1-B3 of the present invention
[0171]
[0172]
[0173] As shown in Table 1, compared with the paper-plastic products B1 and B2 prepared in Comparative Examples 1 and 2, the paper-plastic product A1 prepared in Example 1 has significantly increased interlayer bonding force, significantly improved tensile strength and bursting strength, and improved tear resistance. Most importantly, its oxygen permeability and water vapor permeability have been significantly improved. It can be seen that reducing the proportion of bamboo pulp and sugarcane pulp and introducing wood pulp can effectively improve the physical strength and surface properties of paper-plastic products. Coating a layer of surface coating on the surface of the semi-finished paper-plastic product can effectively improve the oxygen and moisture barrier properties of the paper-plastic product. However, the barrier properties of the paper-plastic product A1 prepared in Example 1 still do not meet the requirements for packaging food, medicines, cosmetics and other products, and need to be further improved.
[0174] Compared with the paper plastic product A1 prepared in Example 1, the paper plastic product A2 prepared in Example 2 has significantly lower interlayer bonding force, tensile strength and bursting strength, but significantly higher tear strength and stiffness, and significantly lower oxygen permeability and water vapor permeability, that is, the paper plastic product A2 prepared in Example 2 has higher oxygen and water barrier properties; it can be seen that a single wood pulp can be selected as the fiber pulp to prepare a paper plastic product with a high-efficiency barrier coating on the surface. In addition, compared with the paper plastic product B3 prepared in Comparative Example 3, the paper plastic product A2 prepared in Example 2 has significantly increased interlayer bonding force, and slightly improved tensile strength, bursting strength and tear strength; it can be seen that the introduction of a wet strength agent as an auxiliary agent can maintain a higher physical strength and surface properties of the paper plastic product; at the same time, the wet strength agent can be adsorbed on the fiber surface, and after heating, a spatial network structure with hydrophobicity is formed between the fibers, which restrains the movement of the fibers and the swelling of the fibers by water absorption, and reduces the moisture absorption and wetting of the fibers.
[0175] Compared with the paper plastic product A2 prepared in Example 2, the interlayer bonding force, tensile strength and bursting strength of the paper plastic products A3-A8 prepared in Examples 3-8 can be maintained or improved, and the tear strength and stiffness are significantly increased; thus, it can be seen that the stiffening agent is introduced in the manufacturing process, and the stiffening agent is adsorbed on the fiber surface through the adsorption of electric charge, and combines with the hydroxyl groups on the fiber surface to form a large number of hydrogen bonds. During the drying process, a large number of cross-linking bonds are formed, thereby achieving the purpose of improving the stiffness and hardness of the paper plastic product.
[0176] Comparing the paper plastic products A1-A8 prepared in Examples 1-8 with the paper plastic products B1-B3 prepared in Comparative Examples 1-3, it can be seen that the paper plastic products A3-A8 prepared in Examples 3-8 all have excellent interlayer bonding, tensile strength, bursting strength, stiffness and other properties, and have lower oxygen permeability and water vapor permeability, which can effectively improve the ability of paper plastic products to block oxygen and moisture. Among them, the paper plastic product A8 prepared in Example 8 has the best performance, so the addition amount of fiber slurry and combined auxiliary agent in Example 8 is the optimal ratio.
[0177] In general, Examples 1-8 can make full use of the characteristics of each additive and the superposition of the effects of the combined additives by selecting and optimizing the fiber slurry, introducing the combined additives, adjusting the addition ratio of the combined additives, and controlling the addition order of the combined additives, so as to maximize the effect of the combined additives in the paper-plastic semi-finished product manufacturing process; in the process of manufacturing the paper-plastic semi-finished product with a high-efficiency barrier coating on the surface through manufacturing processes such as dipping and drying, the coating weight per square meter on the surface of the paper-plastic product can be adjusted by regulating the dipping time, drying temperature, and drying time, thereby reducing the oxygen permeability and water vapor permeability of the paper-plastic product and improving the barrier performance of the paper-plastic product. Among them, the superposition of in-slurry sizing agent, wet strength agent and stiffening agent, as well as increasing the addition ratio of wet strength agent and in-slurry sizing agent, can not only effectively improve the physical strength and surface properties of paper plastic products, but also make the paper plastic semi-finished products have good water resistance. When the paper plastic semi-finished products are dipped in the dipping liquid, the dipping liquid can only stay on the surface of the paper plastic semi-finished products, which can effectively prevent the dipping liquid from penetrating into the interior of the paper plastic semi-finished products; at the same time, the good water resistance of the paper plastic semi-finished products can also effectively prevent the paper plastic semi-finished products from absorbing water, swelling or deformation during dipping, thereby reducing the defective rate.
[0178] It should be noted that the bactericide in the present invention includes but is not limited to the bactericide products used in the embodiments of the present invention, and any common small molecule compound bactericides on the market can be used; the wet strength agent in the present invention includes but is not limited to the wet strength agent products used in the embodiments of the present invention, and any common cationic wet strength agent on the market with thermosetting properties can be used; the stiffening agent in the present invention includes but is not limited to the stiffening agent products used in the embodiments of the present invention, and any common cationic stiffening agent on the market can be used; the in-slurry sizing agent in the present invention includes but is not limited to the in-slurry sizing agent products used in the embodiments of the present invention, and any common cationic in-slurry sizing agent on the market can be used.
[0179] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the scope of protection of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description, and it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention.
Claims
1. A method for manufacturing a paper-plastic product with a high-efficiency barrier coating, characterized in that: The manufacturing steps include: S1. Weigh fiber slurry and a combination of additives, and prepare the weighed fiber slurry and the combination of additives into a paper-plastic semi-finished product; the fiber slurry includes at least one of wood pulp, sugarcane pulp, and bamboo pulp; the mass ratio of wood pulp, sugarcane pulp, and bamboo pulp in the fiber slurry is (0-10): (0-3.5): (0-6.5); the combination of additives includes a wet strength agent and an internal sizing agent; the wet strength agent is a thermosetting cationic wet strength agent, and the mass percentage of the wet strength agent in the fiber slurry is not less than 3%; the internal sizing agent is a cationic internal sizing agent, and the mass percentage of the internal sizing agent in the fiber slurry is not less than 3%; S2. Using an organic solvent as a diluent, preparing a coating material to form a dipping liquid, and placing the dipping liquid in a containing tank; the coating material is one of an organic silicone coating, a high-temperature polyester coating, and a thermoplastic powder coating; S3, immersing the paper-plastic semi-finished product prepared in step S1 in the dipping liquid for dipping, wherein the dipping time is controlled within 2-10 seconds, and taking it out after the dipping is completed to obtain the paper-plastic semi-finished product with the dipping liquid on the surface; S4, placing the semi-finished paper-plastic product with the surface coated with the dipping liquid into a drying container for drying, and taking it out after drying to obtain a paper-plastic product with a coating on the surface.
2. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 1, characterized in that: The organosilicon coating is one of an organosilicon resin coating and a modified organosilicon resin coating; The high temperature polyester coating is one of epoxy resin, phenolic resin and polyimide resin; The thermoplastic powder coating is one of acrylic polymer, perchlorethylene paint, polyethylene and polyamide coating.
3. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 2, characterized in that: The organic solvent is one of butyl acetate, ethyl cellosolve, methanol, ethanol, isopropanol and butanol; the concentration of the coating material in the dipping solution is 20%-65%.
4. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 3, characterized in that: In S2, the receiving groove is a geometric polygonal structure; The geometric polygons include triangles, trapezoids, pentagons, and hexagons; The receiving tank is placed horizontally or tilted; In S3, during dipping, the paper-plastic semi-finished product and the containing tank move relative to each other; In the step S4, the drying process is performed at a temperature of 60-110° C. and a drying time of 1-5 min.
5. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 4, characterized in that: The dipping time is 3-5s; the drying temperature is 80-100°C; and the drying time is 2-3min.
6. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 5, characterized in that: The combination of auxiliary agents also includes bactericides and stiffening agents; The bactericide is a small molecule compound; The stiffening agent is preferably a stiffening agent with a positive charge; Calculated by the mass percentage of the fiber slurry, the addition ratio of the wet strength agent is 3.5-7%, the addition ratio of the bactericide is 0.1-0.3%, the addition ratio of the stiffening agent is 0.2-1%, and the addition ratio of the internal sizing agent is 3-6%.
7. A method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 6, characterized in that: The fiber pulp is a combination of wood pulp, sugarcane pulp and bamboo pulp; The mass ratio of wood pulp, sugarcane pulp and bamboo pulp in the fiber pulp is (0-6):(2-3.5):(2-6.5).
8. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 6, characterized in that: The fiber pulp is wood pulp; The wood pulp is coniferous wood pulp; calculated by the mass percentage of the fiber pulp, the addition ratio of the wet strength agent is 5.5%, the addition ratio of the fungicide is 0.16%, the addition ratio of the stiffener is 8%, and the addition ratio of the internal sizing agent is 5.5%.
9. The method for manufacturing a paper-plastic product with a high-efficiency barrier coating according to claim 8, characterized in that: The preparation steps of the paper-plastic semi-finished product include: a. Add the fungicide into a pulping machine containing papermaking white water, stir, and after mixing evenly, add the fiber slurry to slurry to obtain a first solution; b. adding a stiffening agent to the first solution, mixing well and then performing a refining process to obtain a second solution; c. Add the wet strength agent to the second solution, mix well, then add the sizing agent in the slurry, mix well, and obtain paper plastic slurry; d. The paper plastic slurry is diluted, slurry is supplied, wet embryos are formed in a forming machine, hot pressed and shaped, and dried to obtain a paper plastic semi-finished product; Among them, the fungicide needs to be diluted 30-50 times with clean water before adding; the stiffener needs to be diluted 50-80 times with clean water before adding; the wet strength agent needs to be diluted 10-20 times with clean water before adding; the sizing agent in the slurry needs to be diluted 30-50 times with clean water before adding.
10. A paper-plastic product with a high-efficiency barrier coating, characterized in that: The paper plastic product Prepared according to the manufacturing method according to claim 9.