Curled sequin and preparation process thereof
By using a curled sequin design, the problems of heavy weight and environmental unfriendliness of pearlescent decorative particles are solved, achieving a lightweight, environmentally friendly, and durable decorative effect, while the production process is low in energy consumption and pollution.
Patent Information
- Application Number
- CN202411191884.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Existing pearlescent decorative particles are too heavy and environmentally unfriendly, and plastic colored decorative particles have poor strength and are easily broken, affecting the decorative effect.
It uses curled sequins, which are formed by overlapping colored or patterned pearlescent layers, adhesive layers and heat-shrinkable layers to form curled tubular or columnar particles. The shrinkage force of the heat-shrinkable layer makes the pearlescent layer curl, and an aluminum plating layer is added to enhance the reflective effect. A specific adhesive is used to improve water resistance and strength.
It achieves a lightweight and environmentally friendly decorative effect, with good durability, strong resistance to compression and bending, and low energy consumption and low pollution in the production process.
Smart Images

Figure CN118688891B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to environmentally friendly decorative articles, and in particular to a curled sequin and a preparation process thereof. Background Art
[0002] Pearlescent decoration is a common method that fixes reflective colored decorative particles on the surface of fabrics to play a decorative role. It is often used in automotive fabric interiors, clothing, and fabric furniture outer fabrics. In existing pearlescent decorations, glass beads or glass columns with surface color light are used as decorative particles. The density of the glass beads and glass columns used is large, and the weight of the decoration is greatly increased after decoration. In addition, the surface color light treatment process of the glass beads or glass columns requires the use of chromium and nickel-containing reagents or corona and tempering treatments, which is environmentally friendly and energy-intensive.
[0003] In the prior art, there are colored decorative particles made by spraying paint on plastic surfaces to reduce weight. However, the colored decorative particles are small and difficult to recycle. Solid plastic colored decorative particles are not environmentally friendly. Hollow plastic colored decorative particles are weak in strength and are easily crushed by pressure, thus affecting the aesthetic effect of the entire decorative surface.
[0004] Therefore, the inventor of the present application hopes to develop a lightweight, more environmentally friendly curly sequin to replace the original glass beads or glass columns with colored lights on the surface, so as to achieve the same or better decorative effect. Summary of the invention
[0005] In order to solve the problems of existing pearlescent decorative particles being too heavy and unfriendly to the environment, a curled sequin and a preparation process thereof are provided.
[0006] The above first invention objective of the present invention is achieved through the following technical solutions:
[0007] A curled sequin, characterized in that it is in the shape of a curled film sheet, and comprises, from the outside to the inside, a superimposed pearlescent layer with color or pattern, an adhesive layer solidified by an adhesive, and a heat shrinkable layer formed by curling and shrinking a heat shrinkable film, and the thickness of the curled sequin is 0.14-0.4mm.
[0008] By adopting the above technical solution, the curled sequins of the present application are bonded together with the pearlescent layer and the heat shrinkable layer. When the heat shrinkable layer shrinks due to heat, the pearlescent layer is pulled to shrink until the stress of the two is balanced and the curled sequins are curled into tubular or columnar particles. The outermost pearlescent layer has color, which can replace the glass tube and glass column decorative particles. The curled sequins of the present application are lighter and reduce the weight of the decoration. At the same time, when the curled sequins are lightweight, because they are curled to form a tubular or columnar structure, when they are folded in the vertical axis, the curled sequins can be deformed more without being damaged. Therefore, the curled sequins are not easy to be crushed by pressure to affect the overall beauty and coordination of the decorative surface.
[0009] In summary, the curled sequins of the present application can replace the original tubular and columnar decorations while being lighter, more environmentally friendly and more durable.
[0010] Optionally, the bonding layer is obtained by curing a bonding agent, and the bonding agent includes the following raw materials in parts by weight:
[0011] 100 parts of hydroxyl-terminated polyester;
[0012] 60-70 parts of diisocyanate;
[0013] 40~50 parts of diluent;
[0014] 20-30 parts of polyether polyol;
[0015] 18-23 parts of tris(trimethylsilyl) phosphate.
[0016] By adopting the above technical solution, the present application uses a compound of terminal hydroxyl polyester and polyether polyol as the polyol, and the main polyurethane of the adhesive has better basic water resistance;
[0017] Tris(trimethylsilane) phosphate is also added. When the adhesive meets water, its trimethylsilane hydrolyzes and polymerizes with each other, thereby forming a silane cross-linking network, which in turn strengthens the strength of the adhesive, hinders water from continuing to penetrate, and improves the bonding strength. At the same time, the phosphate group reacts with the residual NH of the polyurethane, thereby inhibiting the hydrolysis of -NC=O-, further enhancing the water resistance of the main polyurethane.
[0018] Therefore, after the curled sequins are bonded and formed by the adhesive, they are not easy to come apart at the edges when soaked in hot water or subsequently washed with water, and are not easy to form bubbles due to separation, thereby improving the yield of the curled sequins in the production process and retaining their beautiful appearance after washing.
[0019] Optional: the diluent is ethyl acetate.
[0020] By adopting the above technical solution, ethyl acetate has good solubility as a diluent, the bonding effect of the adhesive is better, and it is environmentally friendly.
[0021] Optionally, the binder also includes 3 to 6 parts of polysulfone, and the polysulfone is soluble in a diluent.
[0022] By adopting the above technical solution, polysulfone is dissolved in the diluent, and the coating of the adhesive is not affected when it is dissolved, and then solidified after coating. By controlling the amount of polysulfone, the curling process of the curled sequins when immersed in hot water is not affected.
[0023] The insolubility and strength of polysulfone in water improve the water resistance of the adhesive, while also enhancing the strength of the adhesive after curing and reducing the irreversible deformation of the curled sequins caused by folding.
[0024] Optionally, there is an aluminum-plated layer between the pearlescent layer and the bonding layer.
[0025] By adopting the above technical solution, an aluminum layer is plated on the side of the pearlescent layer that is relatively exposed, and the pearlescent layer has a stronger reflective effect, so that the curly sequins increase the visual perception of pearlescent reflection and have a better decorative effect.
[0026] Optionally, the aluminum plating layer has a thickness of 5 to 10 μm.
[0027] By adopting the above technical solution, the thickness of the aluminum coating affects the reflective effect on the one hand, and also affects the bending deformation performance of the curled sequins on the other hand. As the aluminum coating thickens, the pearlescent reflection visual effect of the curled sequins becomes better, but the toughness of the curled sequins when compressed and bent decreases. When the thickness of the aluminum coating increases to 5~10μm, the impact of the decrease in toughness of the curled sequins when compressed and bent is minimal, so the thickness of the aluminum coating is preferably 5~10μm.
[0028] Optionally, the pearlescent layer is processed from a PET film.
[0029] Optionally: the heat shrinkable layer is a PET heat shrinkable film.
[0030] By adopting the above technical solution, the pearlescent and heat shrinkable layers made of PET are softer and more resilient than PVC, and the thickness of the curled sequins can be made thinner and have better resistance to compression and folding.
[0031] The above second invention objective of the present invention is achieved through the following technical solutions:
[0032] A process for preparing a curled sequin comprises the following steps:
[0033] S1: Apply adhesive on one side of the heat shrink film and dry until the viscosity of the adhesive increases to 2 to 2.2 times of the original viscosity;
[0034] S2: Lay the pearlescent film on the side of the heat shrinkable film coated with the adhesive, and wait for the adhesive to cure for 48 hours to obtain a sequin film;
[0035] S3: cutting the sequin film to obtain a sequin precursor;
[0036] S4: Soak the sequin precursor in water at 80-90° C. for 5-10 seconds, remove and dry at room temperature to obtain a curly sequin.
[0037] By adopting the above technical solution, the curled sequins of the present application can be curled into shape by simply soaking in hot water. The higher the hot water temperature and the longer the soaking time, the greater the corresponding curling degree. The control is convenient and simple, with low energy consumption and less pollution.
[0038] In summary, this application has at least the following beneficial effects:
[0039] 1. The curled sequins of the present application are formed by bonding a pearlescent layer and a heat shrinkable layer together. When the heat shrinkable layer shrinks due to heat, the pearlescent layer is pulled to shrink until the stress of the two is balanced. The curled sequins are curled into tubular or columnar particles. The outermost pearlescent layer has color. While replacing the original tubular and columnar decorations, it is more lightweight, environmentally friendly and durable.
[0040] 2. The side of the pearlescent layer that is exposed to the outside is coated with an aluminum layer, so that the curled sequins increase the visual perception of pearlescent reflection and have a better decorative effect;
[0041] 3. The pearlescent layer and the heat shrinkable layer are based on PET, so the thickness of the curled sequins can be made thinner and have better anti-compression and folding ability;
[0042] 4. The adhesive used in the adhesive layer of the present application has good water resistance and high bonding strength. After the curled sequins are bonded and formed by the adhesive, they are not easy to be glued at the edges when soaked in hot water and subsequently washed with water, and it is not easy to form bubbles due to separation, which provides the curly sequins with a high yield rate in the production process and retains the beautiful appearance after cleaning;
[0043] 5. The curled sequins of the present application can be curled into shape by simply soaking in hot water. The higher the hot water temperature and the longer the soaking time, the greater the corresponding curling degree. The control is convenient and simple, with low energy consumption and less pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a schematic diagram of the structure of a curly sequin;
[0045] Figure 2 is a schematic diagram of a curled sequin film layer;
[0046] Figure 3 Schematic diagram of the structure of the sequin test product for compression and folding resistance test.
[0047] Figure numerals: 1. pearlescent layer; 2. aluminum-plated layer; 3. adhesive layer; 4. heat shrink layer; 5. plug-in column. DETAILED DESCRIPTION
[0048] raw material:
[0049] Unless otherwise specified, the raw materials in this application are all commercially available products.
[0050] The pearlescent film is prepared by Wenzhou Hongda Laser Imaging Co., Ltd. The pearlescent film here includes not only film sheets with pearlescent color, but also film sheets with other colors and patterns, such as glitter sheet films, laser sheet films, matte sheet films, etc. In this application, the pearlescent film with laser-formed pearlescent pattern is taken as an example.
[0051] The heat shrink film is a PET heat shrink film, which is a commercially available product of Nanyang Jinhebo Plastic Products Co., Ltd.
[0052] Preparation Example 1
[0053] A bonding agent is obtained by mixing hydroxyl-terminated polyester, diisocyanate, diluent, polyether polyol and tris(trimethylsilyl)phosphate. The mass ratio of hydroxyl-terminated polyester, diisocyanate, diluent, polyether polyol, tris(trimethylsilyl)phosphate and polysulfone is 100:68:47:28:21:5.5.
[0054] The hydroxyl-terminated polyester is polycaprolactone diol, and the average relative molecular weight is 500;
[0055] The diisocyanate is 4,4'-diphenylmethane diisocyanate;
[0056] The diluent is ethyl acetate;
[0057] The polyether polyol is polyoxypropylene ether diol, and the average relative molecular weight is 500;
[0058] The polysulfone is polyethersulfone, and its bisphenol A type polysulfone has an average relative molecular weight of 1000.
[0059] Preparation Example 2
[0060] A binder, which is different from Preparation Example 1 in that the mass ratio of terminal hydroxyl polyester, diisocyanate, diluent, polyether polyol, tris(trimethylsilyl)phosphate and polysulfone is 100:60:50:30:23:3.
[0061] Preparation Example 3
[0062] A binder, which is different from Preparation Example 1 in that the mass ratio of terminal hydroxyl polyester, diisocyanate, diluent, polyether polyol, tris(trimethylsilyl)phosphate and polysulfone is 100:70:40:20:18:6.
[0063] Preparation Example 4
[0064] A binder, which is different from Preparation Example 1 in that the mass ratio of terminal hydroxyl polyester, diisocyanate, diluent, polyether polyol and tris(trimethylsilyl)phosphate is 100:68:47:28:21.
[0065] Preparation Example 5
[0066] A binder, which is different from Preparation Example 1 in that the mass ratio of terminal hydroxyl polyester, diisocyanate, diluent and polyether polyol is 100:68:47:28.
[0067] Preparation Example 6
[0068] A binder, which is different from Preparation Example 1 in that the mass ratio of terminal hydroxyl polyester, diisocyanate, diluent, polyether polyol and polysulfone is 100:68:47:28:5.5.
[0069] Preparation Example 7
[0070] A binder, which is different from Preparation Example 1 in that the diluent is propyl acetate.
[0071] Example 1
[0072] As attached Figure 1 and attached Figure 2 As shown, a curled sequin comprises a pearlescent layer 1, an aluminum-plated layer 2, an adhesive layer 3 and a heat shrinkable layer 4 which are stacked in sequence. Both sides of the curled sequin are curled toward the side where the heat shrinkable layer 4 is located.
[0073] The specifications of the curly sequins can be cut according to actual design needs. For example, the curly sequins are circular or elliptical when unfolded, and the lengths of their major and minor axes can be 1 cm and 1 cm, 1.5 cm and 0.8 cm, 0.8 cm and 0.5 cm, etc. Here, it is a circular piece with a diameter of 1 cm.
[0074] The preparation process of the curly sequins is as follows:
[0075] The PET film is laser treated to form a laser pattern to obtain a pearlescent film;
[0076] The side of the pearlescent film that has not been laser treated is coated with an aluminum film with a thickness of 20±1 μm to form an aluminum-plated layer 2, thereby obtaining a second treated film;
[0077] The aluminum-plated layer 2 of the second treated film is coated with clear oil to prevent adhesion and then rolled up to obtain a semi-finished film;
[0078] Apply adhesive evenly on one side of the heat shrink film, with a coating amount of 2.6g / m 2 After the adhesive is dried until the viscosity increases to 2.2 times of the original viscosity, align the side of the heat shrink film coated with the adhesive with the side of the semi-finished film with the aluminum-plated layer 2, and roll-press and laminate them at a pressure of 0.05 MPa. After curing for 48 hours, a sequin film is obtained;
[0079] Cutting the sequin film to obtain a sequin precursor;
[0080] The sequin precursor was immersed in water at 85° C. for 8 seconds, taken out and dried to obtain the curled sequins.
[0081] The thickness of the PET film is 80 μm; the thickness of the heat shrink film is 40 μm, and the thickness of the adhesive layer is controlled to be 10 μm by the gap between rollers during rolling. The adhesive is the adhesive prepared in Preparation Example 1.
[0082] The cut pearlescent film in the curled sequins corresponds to the pearlescent layer 1, the cured adhesive corresponds to the adhesive layer 2, and the shrunk heat shrinkable film corresponds to the heat shrinkable layer 3.
[0083] Pearlescent film and heat shrink film are both based on PET, which is softer and tougher than PVC. On the one hand, the thickness of the curled sequins can be made thinner, and the product specifications can achieve a total thickness of 0.14~0.4mm. At 0.14mm, there is still good folding ability. At 0.4mm, the sequins can still be heated and bend more than 90°.
[0084] The time and temperature of soaking the curled sequins in water affect the curling amount of the curled sequins. The soaking temperature can be 80~90℃ and the soaking time can be 5~10s, which will not affect the adhesion of the heat shrink film. The temperature can be increased and the soaking time can be reduced accordingly.
[0085] The curled sequins of the present application can be curled and formed by simply soaking in hot water, which is convenient and simple to control, with low energy consumption and less pollution. The curled sequins are bonded together by the pearlescent layer 1 and the heat shrinkable layer 4. When the heat shrinkable layer 4 shrinks due to heat, the pearlescent layer 1 is pulled to shrink until the stress of the two is balanced and the curled sequins are curled into tubular or columnar particles. The outermost pearlescent layer 1 has color, which can replace the decorative particles of glass tubes and glass columns. The aluminum-plated layer 2 makes the pearlescent layer 1 have a stronger reflective effect, so that the curled sequins increase the visual sense of pearlescent reflection and have a better decorative effect. In addition, the curled sequins of the present application are lighter, reducing the weight of the decoration. At the same time, when the curled sequins are lightweight, because they are curled to form a structure similar to a tubular or columnar shape, when they are folded in the vertical axis, the curled sequins can be more deformed without being damaged, so the curled sequins are not easy to be crushed by pressure to affect the overall beauty and coordination of the decorative surface.
[0086] In summary, the curly sequins not only replace the original tubular and columnar decorations, but are also lighter, more environmentally friendly and more durable.
[0087] Example 2
[0088] A curly sequin, which differs from Example 1 in that the adhesive is prepared according to Preparation Example 2.
[0089] Example 3
[0090] A curly sequin, which differs from Example 1 in that the adhesive is prepared according to Preparation Example 3.
[0091] Example 4
[0092] A curly sequin, which differs from Example 1 in that the adhesive is prepared according to Preparation Example 4.
[0093] Comparative Example 1
[0094] A curly sequin, which differs from Example 1 in that the adhesive is prepared in Preparation Example 5.
[0095] Comparative Example 2
[0096] A curly sequin, which differs from Example 1 in that the adhesive is prepared according to Preparation Example 6.
[0097] Example 5
[0098] A curly sequin, which differs from Example 1 in that the adhesive is prepared according to Preparation Example 7.
[0099] Example 6
[0100] A curled sequin, which is different from Example 1 in that the thickness of the aluminum plating layer is 2 μm.
[0101] Example 7
[0102] A curled sequin, which is different from Example 1 in that the thickness of the aluminum plating layer is 5 μm.
[0103] Example 8
[0104] A curled sequin, which is different from Example 1 in that the thickness of the aluminum plating layer is 20 μm.
[0105] Detection
[0106] The finished films obtained in Examples 1 to 8 and Comparative Examples 1 to 2 were subjected to a hydrolysis resistance degumming test, and the obtained curved sequins were subjected to a compression resistance test.
[0107] Hydrolysis resistance degumming test:
[0108] Soak the 10cm*10cm finished film in 90℃ water for 72 hours, then gently unfold the finished film and observe from one side of the heat shrink film whether there is edge debonding and separation, or bubbles formed on the film. Record the observations and classify and count the bubble points according to the diameter.
[0109] Compression test
[0110] The finished film of 5 cm*5 cm was immersed in 85° C. water for 8 seconds to obtain a sequin test product.
[0111] As attached Figure 3 As shown, plug posts 5 with a diameter of 1.5 cm and a height of 1 cm are inserted at both ends of the sequin test product, and the side of the plug posts 5 is attached to the inner side of the sequin test product. The overlapping part of the sequin test product is located at the bottom, and the other side is located directly above.
[0112] Install a liftable pressure strip just above the midpoint of the axis of the sequin test product. First, fit the pressure strip to the sequin test product, set the pressure strip position as the initial position, and then lower the pressure strip to press the sequin test product. The descending speed is 0.25cm / s and the descending height is 0.5cm. After standing for 1s, raise the pressure strip to the initial position. This descending and ascending process completes one folding. Repeat the folding 50 times and then gently unfold the finished film. Observe whether the finished film has creases and bubbles formed by separation on the film, record the observation situation, and count the bubble points according to the diameter.
[0113] The test results are shown in Table 1 below.
[0114] Table 1. Test results of Examples 1 to 8 and Comparative Examples 1 to 2
[0115]
[0116] Combined with Table 1, by comparing Example 1 with Comparative Examples 1-2, it can be seen that in the hydrolysis resistance degumming test results, there is no degumming and separation at the edge of Example 1, and the bubble size is less than 0.2 mm and the number is small, while the edges of Comparative Examples 1-2 are degummed and the bubbles are obviously more. The water resistance of the curled sequins of Example 1 is significantly better than that of Comparative Examples 1-2;
[0117] At the same time, in the compression and folding resistance test, Example 1 has no creases and the bubble size is less than 0.2 mm, while Comparative Examples 1~2 not only have creases but also have more and larger bubbles. The compression and folding resistance of the curled sequins in Example 1 is significantly better than that of Comparative Examples 1~2.
[0118] The reason for the above improvement is that the present application uses a compound of terminal hydroxyl polyester and polyether polyol as the polyol, and the basic water resistance of the main polyurethane of the adhesive is better; tri(trimethylsilane) phosphate is also added, and the trimethylsilane of the adhesive is hydrolyzed and polymerized when it meets water, thereby forming a silane cross-linked network, which in turn strengthens the strength of the adhesive, hinders the continued penetration of water, and improves the bonding strength. At the same time, the phosphate group reacts with the residual NH of the polyurethane, thereby inhibiting the hydrolysis of -NC=O-, and further enhancing the water resistance of the main polyurethane; thus, after the curly sequins are bonded and formed by the adhesive, they are not easy to debond at the edges when immersed in hot water and subsequently washed with water, and bubbles are not easy to form due to separation, thereby providing the curly sequins with a high yield rate in the production process and retention of beautiful appearance after cleaning.
[0119] Combined with Examples 2-3, the mass ratio of the terminal hydroxyl polyester, diisocyanate, diluent, polyether polyol, tris(trimethylsilyl) phosphate and polysulfone in the adhesive of the present application is 100:(60-70):(40-50):(20-30):(18-23):(3-6), which can achieve the above-mentioned effects.
[0120] Comparing Example 1 and Example 4, Example 1 adds polysulfone to the adhesive compared with Example 4, and its hydrolysis resistance degumming test results and compression resistance test results are better than those of Example 4. This is because polysulfone is soluble in the diluent, and does not affect the coating of the adhesive when it is dissolved, and then solidifies after coating. By controlling the amount of polysulfone, the curling process of the curly sequins when immersed in hot water will not be affected; and the insolubility and strength characteristics of polysulfone in water improve the water resistance of the adhesive, while enhancing the strength of the adhesive after curing, reducing the irreversible deformation of the curly sequins due to compression.
[0121] By comparing Example 1 and Example 5, it can be seen that different solvents have a certain influence on the bonding effect of the binder. Among them, ethyl acetate has good solubility as a diluent, has a better bonding effect of the binder, and is environmentally friendly.
[0122] By comparing Example 1 with Examples 6 to 8, it can be seen that the thickness of the aluminum coating in the present application affects the reflective effect on the one hand, and also affects the bending deformation performance of the curled sequins on the other hand. As the aluminum coating increases in thickness, the pearlescent reflection visual effect of the curled sequins becomes better, but the toughness of the curled sequins when bent under pressure decreases. When the thickness of the aluminum coating increases to 5 to 10 μm, the impact of the decrease in toughness of the curled sequins when bent under pressure is minimal, so the thickness of the aluminum coating is preferably 5 to 10 μm.
[0123] This specific embodiment is only an explanation of the present invention, and it is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to this embodiment as needed, but as long as it is within the scope of protection required by the present invention, it will be protected by the patent law.
Claims
1. A curly sequin, characterized in that: The curled sequin sheet is in the shape of a curled film, and comprises, from the outside to the inside, a superimposed pearlescent layer (1) with a color or pattern, an adhesive layer (3) cured by an adhesive, and a heat shrinkable layer (4) formed by curling and shrinking a heat shrinkable film, and the thickness of the curled sequin sheet is 0.14-0.4 mm; The bonding layer (3) is obtained by curing a bonding agent, wherein the bonding agent comprises the following raw materials in parts by weight: 100 parts of hydroxyl-terminated polyester; 60-70 parts of diisocyanate; 40~50 parts of diluent; 20-30 parts of polyether polyol; 18-23 parts of tris(trimethylsilyl) phosphate.
2. A curled sequin according to claim 1, characterized in that: The diluent is ethyl acetate.
3. The curled sequin according to claim 2, characterized in that: The binder also includes 3 to 6 parts of polysulfone, and the polysulfone is soluble in a diluent.
4. The curled sequin according to claim 1, characterized in that: An aluminum-plated layer (2) is provided between the pearlescent layer (1) and the bonding layer (3).
5. The curled sequin according to claim 4, characterized in that: The aluminum plating layer (2) has a thickness of 5 to 10 μm.
6. The curled sequin according to claim 1, characterized in that: The pearlescent layer (1) is obtained by processing a PET film.
7. The curled sequin according to claim 1, characterized in that: The heat shrinkable layer (4) is a PET heat shrinkable film.
8. The process for preparing the curled sequins according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: Apply adhesive on one side of the heat shrink film and dry until the viscosity of the adhesive increases to 2 to 2.2 times of the original viscosity; S2: Lay the pearlescent film on the side of the heat shrinkable film coated with the adhesive, and wait for the adhesive to cure for 48 hours to obtain a sequin film; S3: cutting the sequin film to obtain a sequin precursor; S4: Soak the sequin precursor in water at 80-90° C. for 5-10 seconds, remove and dry at room temperature to obtain a curly sequin.