A texturing method for recycling texturing agent
By recycling the texturing agent and controlling its circulation speed, the problems of poor stability of the silicon wafer pyramid texture and short service life of the texturing agent are solved. The stability and reflectivity of the pyramid texture are improved, and the texturing agent is extended. The service life is long and the cost of texturing is reduced.
Patent Information
- Application Number
- CN202411172541.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
In the continuous kettle reaction of the existing texturing equipment, the microscopic size differences and uneven appearance of the silicon wafer pyramid texture lead to high texturing costs and a short service life of the texturing agent.
The method of recycling the texturing agent is adopted. By controlling the circulation speed of the texturing agent solution in the main tank, a staged circulation method is adopted to adjust the reaction efficiency between the silicon wafer and the texturing agent, avoid the accumulation of by-products, keep the viscosity of the solution stable, and ensure Pyramid suede microscopic dimensional consistency.
It achieves the improvement of the stability and reflectivity of the pyramid texture, extends the service life of the texturing agent, reduces the cost of texturing, and ensures the photoelectric conversion efficiency and light absorption effect of the silicon wafer.
Smart Images

Figure CN118693188B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor equipment, and in particular to a texturing method for recycling a texturing agent. Background Art
[0002] Silicon wafers are treated with texturing to form a pyramid textured surface structure, which reduces reflectivity. Texturing mainly uses texturing additives. By combining texturing additives with crystal surfaces, the various corrosion properties of single-crystal silicon wafers in alkaline solutions are improved to form a pyramid structure. Since texturing equipment is generally a continuous kettle reactor, the solution system is maintained by continuously adding reactants (texturing additives) and the silicon wafers are texturing treated in the system.
[0003] However, in actual use, it was found that although the reactants were continuously added to the system, over time, even under the same processing parameters, the microscopic size of the pyramid velvet surface of the silicon wafer would be different, and even uneven appearance, raindrop marks and other poor velvet appearance would appear, affecting the stability of the pyramid structure of the silicon wafer. The treatment method for this is usually to replace all the velvet additives in the reactor after about 50 batches, which undoubtedly leads to high velvet production costs. Summary of the invention
[0004] The purpose of the present application is to provide a texturing method for recycling a texturing agent, which can solve the problems of poor stability and abnormal appearance of silicon wafer pyramids and the short service life and high cost of the texturing agent.
[0005] To solve the above problems, the technical solution adopted by the present invention is:
[0006] The present application provides a texturing method for recycling a texturing agent, comprising the following steps:
[0007] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, take out each batch of silicon wafers after texturing treatment in the main tank, there is no basket bubbling during texturing, and the overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling;
[0008] In the process of texturing 1 to 100 batches of silicon wafers, the circulation rate of the texturing agent added to the main tank is 78 to 82 L / min;
[0009] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 85 to 90 L / min;
[0010] During the texturing process of batches 201 to 250 of silicon wafers, the circulation rate of the texturing agent added into the main tank was 92 to 98 L / min.
[0011] In some embodiments of the present application, each batch of silicon wafers is subjected to texturing treatment by being placed in a main tank, subjected to texturing treatment at a temperature of 80 to 85° C. for 400 to 450 seconds, and then taken out.
[0012] In some embodiments of the present application, the texturing agent comprises the following raw materials in parts by volume: 7-8 parts of sodium hydroxide, 2.5-3 parts of ADD and 650-700 parts of deionized water.
[0013] In some embodiments of the present application, during the texturing process of 1 to 250 batches of silicon wafers, the texturing agent raw materials are added to the main tank when each batch of silicon wafers is processed.
[0014] In some embodiments of the present application, in the process of texturing 1 to 100 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.2 to 0.23 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0015] In some embodiments of the present application, in the process of texturing 101 to 200 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0016] In some embodiments of the present application, in the process of texturing 201 to 250 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0017] In some embodiments of the present application, in the above-mentioned process of texturing 1 to 250 batches of silicon wafers, the liquid is drained for 70 to 90 seconds after each batch of silicon wafers is processed.
[0018] In some embodiments of the present application, after the main tank is drained, the volume of the solution in the main tank is maintained at 690-710 L.
[0019] In some embodiments of the present application, the volume of the main tank is 720-750L.
[0020] Compared with the prior art, the invention of this application has at least the following advantages or beneficial effects:
[0021] The present application controls the circulation speed of the texturing agent solution in the main tank and adopts a staged circulation method to maintain a stable reaction efficiency between the texturing agent and the silicon wafer, so that the microscopic size of the pyramid velvet surface is stable and the appearance of uneven velvet surface defects is avoided. The inventor believes that this may be due to the fact that by-products (silicates) are generated after the texturing agent reacts with the silicon wafer, and after multiple batches of cyclic texturing, the by-products will accumulate, resulting in different solution viscosities in the early, middle and final stages of the reaction system. By controlling the circulation speed in stages, the contact between the texturing agent and the silicon wafer can be improved, thereby improving the stability of the pyramid velvet surface.
[0022] Specifically, in the early stage, the circulation speed is slow. Due to the sufficient concentration of the texturing agent, the low concentration of silicate, and the small viscosity of the solution, the slow circulation speed will promote chemical reactions, and the number of pyramid nucleations will be large, forming a larger pyramid structure with a larger specific surface area. Gradually in the later stage, the circulation speed will accelerate, which will promote chemical reactions. Even if the silicate concentration and solution viscosity increase with the increase in batches, it can promote the nucleation of the pyramid to a certain extent, obtain a certain pyramid height, and form a larger specific surface area. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is a pyramid data comparison diagram of Example 1 of the present application and Comparative Example 1;
[0025] Figure 2 This is a comparison chart of the reflectivity of Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.
[0028] The present application provides a texturing method for recycling a texturing agent, comprising the following steps:
[0029] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, take out each batch of silicon wafers after texturing treatment in the main tank, there is no basket bubbling during texturing, and the overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling;
[0030] In the process of texturing 1 to 100 batches of silicon wafers, the circulation rate of the texturing agent added to the main tank is 78 to 82 L / min;
[0031] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 85 to 90 L / min;
[0032] During the texturing process of batches 201 to 250 of silicon wafers, the circulation rate of the texturing agent added into the main tank was 92 to 98 L / min.
[0033] Preferably, the basket-free bubbling is specifically performed when there is no flower basket in the tank, and the bubbling is stopped after the flower basket is put into the tank.
[0034] The present application controls the circulation speed of the texturing agent solution in the main tank and adopts a staged circulation method to maintain a stable reaction efficiency between the texturing agent and the silicon wafer, so that the microscopic size of the pyramid velvet surface is stable and the appearance of uneven velvet surface defects is avoided. The inventor believes that this may be due to the fact that by-products (silicates) are generated after the texturing agent reacts with the silicon wafer, and after multiple batches of cyclic texturing, the by-products will accumulate, resulting in different solution viscosities in the early, middle and final stages of the reaction system. By controlling the circulation speed in stages, the contact between the texturing agent and the silicon wafer can be improved, thereby improving the stability of the pyramid velvet surface.
[0035] In some embodiments of the present application, each batch of silicon wafers is subjected to texturing treatment by being placed in a main tank, subjected to texturing treatment at a temperature of 80 to 85° C. for 400 to 450 seconds, and then taken out.
[0036] The texturing process under this condition can stabilize the pyramid texture, increase the light absorption of the silicon wafer, and improve the photoelectric conversion efficiency.
[0037] In some embodiments of the present application, the texturing agent comprises the following raw materials in parts by volume: 7-8 parts of sodium hydroxide, 2.5-3 parts of ADD and 650-700 parts of deionized water.
[0038] Under this ratio, the damaged layer on the silicon surface can be effectively removed, and under this ratio, the desired pyramid velvet structure can be obtained after the initial liquid preparation, and a lower reflectivity can be obtained.
[0039] In some embodiments of the present application, during the texturing process of 1 to 250 batches of silicon wafers, the texturing agent raw materials are added to the main tank when each batch of silicon wafers is processed.
[0040] After multiple batches of reactions, more by-products will accumulate in the solution system, which will affect the concentration of the texturing agent. By adding the texturing agent raw materials and adjusting the concentration of the texturing agent in the solution, the texturing effect of the silicon wafer can be improved and stabilized.
[0041] In some embodiments of the present application, in the process of texturing 1 to 100 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.2 to 0.23 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0042] Preferably, the ADD is a texturing additive, comprising the following raw materials in weight percentage: 0.1-3% sodium hydroxide, 2-10% isopropanol, 0.01-2% additive, and the balance is water.
[0043] The above-mentioned additives include sodium lactate or sodium citrate, propylene glycol, sodium silicate, sodium carbonate and / or sodium bicarbonate.
[0044] In some embodiments of the present application, in the process of texturing 101 to 200 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0045] In some embodiments of the present application, in the process of texturing 201 to 250 batches of silicon wafers, the following raw materials in parts by weight are added to the main tank during the processing of each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of ADD and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80 to 85°C.
[0046] In some embodiments of the present application, in the above-mentioned process of texturing 1 to 250 batches of silicon wafers, the liquid is drained for 70 to 90 seconds after each batch of silicon wafers is processed.
[0047] Since the reaction will produce by-products (such as sodium silicate), and sodium silicate is flocculent, it will affect the viscosity and reaction rate of the solution. After the above treatment, the by-products can be discharged to increase the reaction rate and reduce the viscosity.
[0048] In some embodiments of the present application, after the main tank is drained, the volume of the solution in the main tank is maintained at 690-710 L.
[0049] In some embodiments of the present application, the volume of the main tank is 720-750L.
[0050] In some embodiments of the present application, the main groove is made of PP material.
[0051] In some embodiments of the present application, the replenishment liquid in the auxiliary tank is circulated into the main tank through a circulation pump.
[0052] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0053] Example 1
[0054] A texturing method for recycling a texturing agent comprises the following steps:
[0055] The main tank has a capacity of 730 L, and the raw materials of the texturing agent are: 7.5 L of sodium hydroxide, 2.8 L of ADD and 680 L of deionized water.
[0056] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, put each batch of silicon wafers in the main tank for texturing at 82℃ for 420s and then take them out. During the texturing process, there is no bubbling and overflowing. The overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling.
[0057] During the texturing process of batches 1 to 100 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 80 L / min, and the following raw materials were added: 0.715 L of sodium hydroxide, 0.21 L of ADD, and 1.8 L of deionized water, and the temperature of the deionized water was 83°C;
[0058] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 88 L / min, and the following raw materials were added: 0.715 L of sodium hydroxide, 0.2 L of ADD, and 1.8 L of deionized water, and the temperature of the deionized water was 83°C;
[0059] During the texturing process of batches 201 to 304 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 95 L / min, and the following raw materials were added: 0.715 L of sodium hydroxide, 0.2 L of ADD and 1.8 L of deionized water, and the temperature of the deionized water was 83°C.
[0060] Example 2
[0061] A texturing method for recycling a texturing agent comprises the following steps:
[0062] The volume of the main tank is 730L, and the raw materials of the texturing agent are: 7L of sodium hydroxide, 2.5L of ADD and 700L of deionized water.
[0063] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, and put each batch of silicon wafers into the main tank for texturing at 80℃ for 450s before taking them out. During the texturing process, there is no bubbling and the overflowing texturing agent flows into the auxiliary tank, and then replenishes it into the main tank for recycling.
[0064] During the texturing process of batches 1 to 100 of silicon wafers, the texturing agent was added to the main tank at a circulation rate of 78 L / min, and the following raw materials were added: 0.7 L of sodium hydroxide, 0.2 L of ADD, and 1.9 L of deionized water, and the temperature of the deionized water was 85°C;
[0065] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 85 L / min, and the following raw materials were added: 0.7 L of sodium hydroxide, 0.19 L of ADD, and 1.9 L of deionized water, and the temperature of the deionized water was 85°C;
[0066] During the texturing process of batches 201 to 304 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 92 L / min, and the following raw materials were added: 0.7 L of sodium hydroxide, 0.19 L of ADD and 1.9 L of deionized water, and the temperature of the deionized water was 85°C.
[0067] Example 3
[0068] A texturing method for recycling a texturing agent comprises the following steps:
[0069] The volume of the main tank is 730L, and the raw materials of the texturing agent are: 8L of sodium hydroxide, 3L of ADD and 650L of deionized water.
[0070] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, put each batch of silicon wafers in the main tank for texturing at 85℃ for 400s and then take them out. During the texturing process, there is no bubbling and overflowing. The overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling.
[0071] During the texturing process of batches 1 to 100 of silicon wafers, the texturing agent was added to the main tank at a circulation rate of 82 L / min, and the following raw materials were added: 0.73 L of sodium hydroxide, 0.23 L of ADD, and 1.7 L of deionized water, and the temperature of the deionized water was 80°C;
[0072] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 90 L / min, and the following raw materials were added: 0.73 L of sodium hydroxide, 0.21 L of ADD, and 1.7 L of deionized water, and the temperature of the deionized water was 80°C;
[0073] During the texturing process of batches 201 to 304 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 98 L / min, and the following raw materials were added: 0.73 L of sodium hydroxide, 0.21 L of ADD and 1.7 L of deionized water, and the temperature of the deionized water was 80°C.
[0074] Example 4
[0075] A texturing method for recycling a texturing agent comprises the following steps:
[0076] The volume of the main tank is 730L, and the raw materials of the texturing agent are: 7-8L of sodium hydroxide, 2.5-3L of ADD and 650-700L of deionized water.
[0077] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, and put each batch of silicon wafers into the main tank for texturing treatment at 80-85℃ for 400-450s before taking them out. During the texturing process, there is no bubbling and the overflowing texturing agent flows into the auxiliary tank, and then replenishes into the main tank from the auxiliary tank for recycling;
[0078] In the process of texturing 1 to 100 batches of silicon wafers, the circulation rate of the texturing agent added to the main tank is 78 to 82 L / min, and the following raw materials are added: 0.7 to 0.73 L of sodium hydroxide, 0.2 to 0.23 L of ADD and 1.7 to 1.9 L of deionized water, and the temperature of the deionized water is 80 to 85 °C;
[0079] During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 85 to 90 L / min, and the following raw materials were added: 0.7 to 0.73 L of sodium hydroxide, 0.19 to 0.21 L of ADD, and 1.7 to 1.9 L of deionized water. The temperature of the deionized water was 80 to 85 °C.
[0080] During the texturing process of batches 201 to 304 of silicon wafers, the circulation rate of the texturing agent added into the main tank was 92 to 98 L / min, and the following raw materials were added: 0.7 to 0.73 L of sodium hydroxide, 0.19 to 0.21 L of ADD and 1.7 to 1.9 L of deionized water, and the temperature of the deionized water was 80 to 85°C.
[0081] Comparative Example 1
[0082] This comparative example is basically the same as Example 1, except that only 250 batches were made, and the circulation speed of batches 1 to 250 was 90 L / min.
[0083] A texturing method for recycling a texturing agent comprises the following steps:
[0084] The volume of the main tank is 730L, and the raw materials of the texturing agent are: 7.5L of sodium hydroxide, 2.8L of ADD and 680L of deionized water.
[0085] Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, put each batch of silicon wafers in the main tank for texturing at 82℃ for 420s and then take them out. During the texturing process, there is no bubbling and overflowing. The overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling.
[0086] During the texturing process of batches 1 to 100 of silicon wafers, the following raw materials were added: 0.715 L of sodium hydroxide, 0.21 L of ADD, and 1.8 L of deionized water, with the temperature of the deionized water being 83°C;
[0087] During the texturing process of batches 101 to 200 of silicon wafers, the following raw materials were added: 0.715 L of sodium hydroxide, 0.2 L of ADD, and 1.8 L of deionized water, with the temperature of the deionized water being 83°C;
[0088] During the texturing process of batches 201 to 250 of silicon wafers, the following raw materials were added: 0.715 L of sodium hydroxide, 0.2 L of ADD and 1.8 L of deionized water, and the temperature of the deionized water was 83°C.
[0089] Example
[0090] Each batch of silicon wafers after texturing in Example 1 and Comparative Example 1 were inspected using a Zeta 3D microscope at 100 times magnification. The results are as follows: Figures 1-2 shown.
[0091] Figure 1 This is a comparison chart of pyramid data after silicon wafer texturing. The horizontal axis is the number of silicon wafer cycle processing batches, the vertical axis on the left is size and height, and the vertical axis on the right is ratio. Figure 1 The SY group is the sample of Example 1, and the BL group is the sample of Comparative Example 1; Size is the size of the pyramid, height is the height of the pyramid, and ratio is the specific surface area of the pyramid. Figure 1 The size average curve represents the size of the pyramid base. By comparing SY-size and BL-size, it can be seen that the size of the SY group (Example 1) can be effectively stabilized at about 1.75 μm throughout the life cycle of the system, and can be stably achieved for 300 batches; while the size of the BL (Comparative Example 1) shows an obvious downward trend throughout the life cycle of the system.
[0092] Reference Figure 1 The height curve represents the average height of the pyramid. By comparing SY-height and BL-height, it can be seen that the height of the SY group (Example 1) can be stabilized at 1.1 μm throughout the life cycle of the system, and can be stably achieved for 300 batches; while the height of the BL group (Comparative Example 1) shows an obvious downward trend throughout the life cycle of the system.
[0093] Reference Figure 1The radio curve represents the average specific surface area of the pyramid. By comparing SY-radio and BL-ratio, it can be seen that the specific surface area of the SY group (Example 1) can be stabilized at 1.3μm throughout the life cycle of the system, and can be stably achieved for 300 batches; while the specific surface area of the BL group (Comparative Example 1) has an obvious downward trend starting from the 200th batch.
[0094] This shows that the SY group (Example 1) can significantly improve the stability of silicon wafer texturing through staged cycles, can control the pyramid to be at a stable level throughout the cycle, can adjust the liquid replenishment to achieve the expected pyramid structure, and expand the process adjustment window. And the solution life is increased by 20% and still has a stable pyramid structure.
[0095] Figure 2 This is a comparison chart of the reflectivity of silicon wafers after texturing. The horizontal axis is the number of silicon wafer cycle batches, and the vertical axis is the reflectivity.
[0096] Figure 2 The reflectivity characterizes the light absorption effect of the velvet surface. The higher the reflectivity, the lower the light absorption, and the lower the reflectivity, the higher the light absorption. It can be seen from the figure that SY (Example 1) can control the reflectivity to be in a relatively stable state throughout the life cycle, and has a lower reflectivity when the system life is 300 batches. The reflectivity of BL (Comparative Example 1) fluctuates greatly throughout the life cycle of the system, and at the end (250 batches), the reflectivity is significantly higher than that of SY. Conclusion: SY (Example 1) can control the reflectivity at a relatively stable level, improve the light absorption effect of silicon wafers, and extend the life of the solution system by 20%, so that the velvet making agent can be used more times compared to non-stage circulation.
[0097] In summary, the embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
Claims
1. A texturing method for recycling a texturing agent, characterized in that: The steps include: Put the texturing agent into the main tank of the reactor, put the silicon wafers into the main tank, take out each batch of silicon wafers after texturing treatment in the main tank, there is no basket bubbling during texturing, and the overflowing texturing agent flows into the auxiliary tank, and then replenishes from the auxiliary tank into the main tank for recycling; In the process of texturing 1 to 100 batches of silicon wafers, the circulation rate of the texturing agent added to the main tank is 78L / min to 82L / min; During the texturing process of batches 101 to 200 of silicon wafers, the circulation rate of the texturing agent added to the main tank was 85L / min to 90L / min; During the texturing process of batches 201 to 250 of silicon wafers, the circulation rate of the texturing agent added into the main tank was 92L / min to 98L / min.
2. A texturing method for recycling a texturing agent according to claim 1, characterized in that: Each batch of silicon wafers is specifically placed in the main tank for texturing treatment at a temperature of 80° C. to 85° C. for 400 seconds to 450 seconds and then taken out.
3. The texturing method of recycling the texturing agent according to claim 1, characterized in that: The texturing agent comprises the following raw materials in parts by volume: 7 to 8 parts of sodium hydroxide, 2.5 to 3 parts of a texturing additive and 650 to 700 parts of deionized water.
4. A texturing method for recycling a texturing agent according to claim 3, characterized in that: During the texturing process of batches 1 to 100, batches 101 to 200 and batches 201 to 250 of silicon wafers, texturing agent raw materials are added to the main tank when processing each batch of silicon wafers.
5. A texturing method for recycling a texturing agent according to claim 3 or 4, characterized in that: During the texturing process of 1 to 100 batches of silicon wafers, the following raw materials in parts by weight are added into the main tank for each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.2 to 0.23 parts of texturing additives and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80°C to 85°C.
6. A texturing method for recycling a texturing agent according to claim 3 or 4, characterized in that: During the texturing process of 101 to 200 batches of silicon wafers, the following raw materials in parts by weight are added into the main tank for each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of texturing additives and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80°C to 85°C.
7. A texturing method for recycling a texturing agent according to claim 3 or 4, characterized in that: During the texturing process of batches 201 to 250 of silicon wafers, the following raw materials in parts by weight are added into the main tank for each batch of silicon wafers: 0.7 to 0.73 parts of sodium hydroxide, 0.19 to 0.21 parts of texturing additives and 1.7 to 1.9 parts of deionized water, and the temperature of the deionized water is 80°C to 85°C.
8. The texturing method of recycling the texturing agent according to claim 4, characterized in that: During the texturing process of batches 1 to 100, batches 101 to 200 and batches 201 to 250 of silicon wafers, the liquid is drained for 70s to 90s after each batch of silicon wafers is processed.
9. A texturing method for recycling a texturing agent according to claim 8, characterized in that: After the main tank is drained, the volume of the solution in the main tank is maintained at 690L to 710L.
10. The texturing method of recycling the texturing agent according to claim 8, characterized in that: The main tank has a capacity of 720L to 750L.
Citation Information
Patent Citations
Silicon wafer texturing and cleaning process, solar cell and preparation method of solar cell
CN115312628A
Thin silicon heterojunction solar cell textured surface preparation method and heterojunction cell
CN117457799A