Electrode frame for flow battery and preparation method thereof

By using multi-layer coating technology in the flow battery electrode frame, the problem of unsolid sealing of the electric stack is solved, effective sealing and cost reduction under strong acid conditions is achieved, and the reliability of the system is improved. Security.

CN118693303BActive Publication Date: 2024-11-15SUZHOU TUOJI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411174895.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The sealing method of the stack in existing flow battery systems has a risk of leakage, and the high unit price limits its large-scale commercial use, especially because the ion exchange membrane is not tightly sealed by compaction, making it difficult to maintain sealing under long-term and strong acid conditions. .

Method used

Using a liquid flow battery electrode frame containing substrate and ethylene acrylic maleic anhydride copolymer coating and ethylene-acrylate copolymer coating, the bonding force is enhanced by grinding and multi-layer coating technology, replacing the traditional rubber ring sealing Method to ensure effective sealing of the ion exchange membrane.

Benefits of technology

The liquid flow battery sealing under long-term and strong acid conditions is achieved, the utilization rate of the ion exchange membrane is improved, the cost of VRFB is reduced, the penetration of electrolyte is avoided, and the reliability and safety of the stack is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118693303B_ABST
    Figure CN118693303B_ABST
Patent Text Reader

Abstract

The present invention provides an electrode frame for flow battery and a preparation method thereof. The electrode frame includes a substrate and an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating on the surface of the substrate, wherein the ethylene-propylene-maleic anhydride copolymer coating is located between the substrate and the ethylene-acrylate copolymer coating, and the raw material of the ethylene-propylene-maleic anhydride copolymer coating includes an ethylene-propylene-maleic anhydride copolymer, a first initiator and a first cross-linking agent in a mass ratio of 100:(2-4):(2-8); the raw material of the ethylene-acrylate copolymer coating includes an ethylene-acrylate copolymer, a second initiator, a second cross-linking agent, a coupling agent and an anti-hydrolysis agent in a mass ratio of 100:(2-8):(2-8):(2-8):(1-15). The electrode frame of the present invention can be used to effectively seal the ion exchange membrane to prevent the positive and negative electrolytes from penetrating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of liquid flow battery packaging materials and relates to an electrode frame for a liquid flow battery and a preparation method thereof. Background Art

[0002] Since renewable clean energy such as wind and solar energy are unstable, they need to be equipped with energy storage systems to reduce peak loads and fill valleys to reduce wind and solar power abandonment. Flow batteries, especially all-vanadium flow batteries (VRFB), have the advantages of intrinsic safety, long life, and decoupled design of energy and power, making them an ideal choice for long-term energy storage. However, the current high unit price limits its large-scale commercial use.

[0003] The battery stack is the core component of the liquid flow battery system and is the place where electrochemical reactions occur. The battery stack generally includes end plates, bipolar plates, electrode frames, electrodes, ion exchange membranes and other components. Leakage of the battery stack is a common fault in the liquid flow battery system. Therefore, the sealing of the battery stack is one of the key technologies of the liquid flow battery and is directly related to the reliability and safety of the battery stack.

[0004] At present, a commonly used method for packaging a battery stack is to rely on the compression and sealing of a rubber ring. The rubber ring is placed in the groove of the liquid flow frame, and after all the components are stacked, the end plates are tightened as a whole with bolts to complete the packaging of the battery stack. However, this sealing method not only greatly wastes the ion exchange membrane, but also has the risk of leakage, because the ion exchange membrane is only sealed by compaction.

[0005] Therefore, there is an urgent need for a new material or method that can bond the electrode frame and the ion exchange membrane together and has good acid-resistant bonding. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides an electrode frame for a liquid flow battery and a preparation method thereof. The electrode frame of the present invention can effectively seal the ion exchange membrane, prevent the positive and negative electrolytes from penetrating, and can seal the liquid flow battery under long-term and strong acid conditions.

[0007] Specifically, the first aspect of the present invention provides an electrode frame for a liquid flow battery, wherein the electrode frame for the liquid flow battery comprises a substrate and an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating located on the surface of the substrate, wherein the ethylene-propylene-maleic anhydride copolymer coating is located between the substrate and the ethylene-acrylate copolymer coating, and the raw materials of the ethylene-propylene-maleic anhydride copolymer coating comprise an ethylene-propylene-maleic anhydride copolymer, a first initiator, and a first co-crosslinking agent in a mass ratio of 100:(2-4):(2-8); the raw materials of the ethylene-acrylate copolymer coating comprise an ethylene-acrylate copolymer, a second initiator, a second co-crosslinking agent, a coupling agent, and an anti-hydrolysis agent in a mass ratio of 100:(2-8):(2-8):(2-8):(1-15).

[0008] In one or more embodiments, the material of the substrate is selected from one or more of PP, PEN, PPS and PET.

[0009] In one or more embodiments, the substrate surface is roughened.

[0010] In one or more embodiments, the single-side thickness of the ethylene propylene maleic anhydride copolymer coating is 5-20 μm.

[0011] In one or more embodiments, the single-side thickness of the ethylene-acrylate copolymer coating is 10-25 μm.

[0012] In one or more embodiments, the ethylene propylene maleic anhydride copolymer is a copolymer of ethylene, propylene and maleic anhydride monomer or a copolymer of ethylene, propylene, maleic anhydride monomer and a functional monomer; preferably, the functional monomer contains one or more groups selected from epoxy, anhydride and carbonyl groups; preferably, in the ethylene propylene maleic anhydride copolymer, the mass fraction of the ethylene structural unit is 30%-54%, the mass fraction of the propylene structural unit is 45%-69%, the mass fraction of the maleic anhydride monomer structural unit is 1%-3%, and the mass fraction of the functional monomer structural unit is 0-1%.

[0013] In one or more embodiments, the first initiator and the second initiator are each independently selected from one or more of a peroxide initiator and an azo initiator.

[0014] In one or more embodiments, the first co-crosslinking agent and the second co-crosslinking agent contain two or more carbon-carbon double bonds; preferably, the first co-crosslinking agent and the second co-crosslinking agent are each independently selected from one or more of triallyl isocyanurate, triallyl cyanurate, terminal hydroxyl polybutadiene and trimethylolpropane trimethacrylate.

[0015] In one or more embodiments, the ethylene-acrylate copolymer is a copolymer of ethylene and an acrylate monomer; preferably, the acrylate monomer is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate and butyl methacrylate; preferably, in the ethylene-acrylate copolymer, the mass fraction of the ethylene structural unit is 50%-80%, and the mass fraction of the acrylate monomer structural unit is 20%-50%.

[0016] In one or more embodiments, the coupling agent is a silane coupling agent; preferably, the coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane, γ-aminopropyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.

[0017] In one or more embodiments, the anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent.

[0018] A second aspect of the present invention provides a method for preparing an electrode frame for a flow battery as described in any embodiment of the present invention, the method comprising the following steps:

[0019] (1) uniformly dispersing the raw material of the ethylene-propylene-maleic anhydride copolymer coating in a solvent, filtering and degassing to obtain an ethylene-propylene-maleic anhydride copolymer coating solution;

[0020] The surface of the substrate of the electrode frame for the flow battery is polished, and then the ethylene propylene maleic anhydride copolymer coating solution is applied to the polished surface of the substrate, and dried to obtain the ethylene propylene maleic anhydride copolymer coating;

[0021] (2) uniformly dispersing the raw material of the ethylene-acrylate copolymer coating in a solvent, filtering and degassing to obtain an ethylene-acrylate copolymer coating solution;

[0022] The ethylene-acrylate copolymer coating solution is coated on the surface of the ethylene-propylene-maleic anhydride copolymer coating and dried to obtain the ethylene-acrylate copolymer coating.

[0023] In one or more embodiments, the solvent is selected from one or more of xylene, toluene, cyclohexane, methyl ethyl ketone, and tetrahydrofuran.

[0024] In one or more embodiments, in step (1), the solid content of the ethylene-propylene-maleic anhydride copolymer coating solution is 5 wt%-30 wt%.

[0025] In one or more embodiments, in step (1), the grinding mesh size is 800-1200 mesh.

[0026] In one or more embodiments, in step (1), the drying temperature is 140-180°C.

[0027] In one or more embodiments, in step (2), the solid content of the ethylene-acrylate copolymer coating solution is 5 wt%-30 wt%.

[0028] In one or more embodiments, in step (2), the drying temperature is 140-180°C.

[0029] A third aspect of the present invention provides a liquid flow battery, which comprises an electrode frame for a liquid flow battery as described in any embodiment of the present invention or an electrode frame for a liquid flow battery prepared by a method as described in any embodiment of the present invention.

[0030] In one or more embodiments, the flow battery is an all-vanadium flow battery.

[0031] In one or more embodiments, the preparation of the liquid flow battery includes placing an ion exchange membrane between two electrode frames for liquid flow batteries as described in any embodiment of the present invention, and then performing a bonding and curing step.

[0032] The present invention has the following beneficial effects: the electrode frame for the liquid flow battery of the present invention can replace the rubber ring used to seal the battery stack in the liquid flow battery, effectively seal the ion exchange membrane, prevent the penetration of positive and negative electrode electrolytes, and can seal the liquid flow battery under long-term and strong acid conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of a flow battery stack in some embodiments of the present invention.

[0034] Figure 1 In the figure, 1 is an end plate, 2 is a bipolar plate, 3 is an electrode frame, 4 is an electrode, and 5 is an ion exchange membrane. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.

[0036] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0037] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0038] In this document, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values ​​within the range (including integers and fractions).

[0039] Herein, the sum of the percentages of the various components of the composition is 100%.

[0040] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0041] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0042] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0043] The object of the present invention is to provide a new electrode frame for a liquid flow battery (especially a vanadium battery) and a preparation method thereof. The electrode frame of the present invention can effectively seal the ion exchange membrane to prevent the positive and negative electrolytes from penetrating. The electrode frame of the present invention has a strong bonding force with the ion membrane and is resistant to strong acid corrosion. It can seal the liquid flow battery under long-term strong acid conditions without leakage for a long time, thereby greatly improving the utilization rate of the ion membrane and reducing the cost of VRFB.

[0044] In some embodiments, such as Figure 1As shown, the flow battery stack includes an end plate, a bipolar plate, an electrode frame of the present invention, an electrode and an ion exchange membrane, wherein the electrode frame is arranged on both sides of the positive and negative electrodes, and the two electrode frames of the present invention both with the above coating are bonded and cured, and the ion exchange membrane and the positive and negative electrodes are sandwiched in between, so as to achieve sealing of the ion exchange membrane. The battery stack of the present invention does not need to use a frame membrane.

[0045] The electrode frame of the present invention comprises a substrate and an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating sequentially disposed on the surface of the substrate.

[0046] In the electrode frame of the present invention, the thickness of the substrate can be 0.5-2 mm. In some embodiments, the surface of the substrate is roughened by using 800-1200 mesh sandpaper to a level that is noticeably abrasive.

[0047] In the electrode frame of the present invention, the single-side thickness of the ethylene-propylene-maleic-anhydride copolymer coating may be 5-20 μm, such as 10 μm or 15 μm.

[0048] In the electrode frame of the present invention, the single-side thickness of the ethylene-acrylate copolymer coating may be 10-25 μm, such as 15 μm or 20 μm.

[0049] In the present invention, the raw material of the ethylene propylene maleic anhydride copolymer coating comprises ethylene propylene maleic anhydride copolymer, a first initiator and a first co-crosslinking agent. In some embodiments, the raw material of the ethylene propylene maleic anhydride copolymer coating consists of ethylene propylene maleic anhydride copolymer, a first initiator and a first co-crosslinking agent.

[0050] In the present invention, the raw materials of the ethylene-acrylate copolymer coating include ethylene-acrylate copolymer, a second initiator, a second co-crosslinking agent, a coupling agent and an anti-hydrolysis agent. In some embodiments, the raw materials of the ethylene-acrylate copolymer coating consist of ethylene-acrylate copolymer, a second initiator, a second co-crosslinking agent, a coupling agent and an anti-hydrolysis agent.

[0051] The ethylene propylene maleic anhydride copolymer suitable for the present invention can be a copolymer of ethylene, propylene and maleic anhydride monomers, or a copolymer of ethylene, propylene, maleic anhydride monomers and functional monomers. In other words, the functional monomer structural unit is optionally present in the ethylene propylene maleic anhydride copolymer.

[0052] In the ethylene-propylene-maleic anhydride copolymer, the mass fraction of the ethylene structural unit can be 30%-54%, for example, 35%, 40%, 45%, 50%; the mass fraction of the propylene structural unit can be 45%-69%, for example, 50%, 55%, 60%, 65%; the mass fraction of the maleic anhydride monomer structural unit can be 1%-3%, for example, 2%; the mass fraction of the functional monomer structural unit is 0-1%.

[0053] The ethylene-acrylate copolymer suitable for the present invention can be a binary copolymer of ethylene and acrylate monomers, or a ternary or higher copolymer of ethylene, acrylate monomers and functional monomers. In other words, the functional monomer structural unit is optionally present in the ethylene-acrylate copolymer.

[0054] In the ethylene-acrylate copolymer, the mass fraction of the ethylene structural unit can be 50%-80%, for example, 55%, 60%, 65%, 70%, 75%; the mass fraction of the acrylate monomer structural unit can be 20%-50%, for example, 25%, 30%, 35%, 40%, 45%; the mass fraction of the functional monomer structural unit is 0-1%.

[0055] In the present invention, acrylate monomers include acrylates (e.g., alkyl acrylates) and methacrylates (e.g., alkyl methacrylates). Acrylate monomers suitable for use in the present invention include, but are not limited to, one or more selected from methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, etc. In some embodiments, the acrylate monomer is butyl acrylate.

[0056] In some embodiments, the ethylene-acrylate copolymer is a copolymer of ethylene and butyl acrylate.

[0057] The initiators (first initiator and second initiator) suitable for the present invention may be peroxide initiators, azo initiators or a combination thereof. Examples of available peroxide initiators include dibenzoyl peroxide, tert-butyl perbenzoate, lauroyl peroxide, di-tert-butyl peroxide, tert-butyl peroxide 2-ethylhexanoate, etc. Examples of available azo initiators include azobisisobutyronitrile, dimethyl azobisisobutyrate, 2,2'-azobis(2,4-dimethylvaleronitrile), etc. In some embodiments, the first initiator is tert-butyl perbenzoate. The mass ratio of the first initiator to the ethylene-propylene-maleic anhydride copolymer may be (2-8):100, for example, 3:100, 4:100, 5:100, 8:100.

[0058] In some embodiments, the second initiator is dibenzoyl peroxide. The mass ratio of the second initiator to the ethylene-acrylate copolymer can be (2-8):100, such as 2:100, 4:100, 5:100, 8:100.

[0059] The cross-linking aid (the first cross-linking aid and the second cross-linking aid) suitable for the present invention contains two or more carbon-carbon double bonds. Examples of available cross-linking aids include triallyl isocyanurate, triallyl cyanurate, hydroxyl-terminated polybutadiene, trimethylolpropane trimethacrylate, etc. In some embodiments, the first cross-linking aid is triallyl isocyanurate and / or hydroxyl-terminated polybutadiene. The mass ratio of the first cross-linking aid to the ethylene-propylene maleic anhydride copolymer can be (2-8):100, such as 2:100, 4:100, 5:100, 6:100. In some embodiments, the first cross-linking aid is triallyl isocyanurate and hydroxyl-terminated polybutadiene, and the mass ratio of triallyl isocyanurate to hydroxyl-terminated polybutadiene is preferably 1:(2-3), such as 1:2.5, which is conducive to improving the bonding force. In some embodiments, the second cross-linking aid is triallyl cyanurate. The mass ratio of the second auxiliary cross-linking agent to the ethylene-acrylate copolymer can be (2-8):100, for example, 2:100, 4:100, 5:100, 6:100.

[0060] The coupling agent suitable for the present invention may be a silane coupling agent. Examples of available silane coupling agents include γ-aminopropyl triethoxysilane, vinyl trimethoxysilane, γ-aminopropyl trimethoxysilane, vinyl triethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, etc. In some embodiments, the coupling agent is composed of γ-aminopropyl triethoxysilane and one or two selected from vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane, and the mass ratio of γ-aminopropyl triethoxysilane and one or two selected from vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane can be 1:2 to 2:1, such as 3:2. The mass ratio of the coupling agent to the ethylene-acrylate copolymer can be (2-8):100, such as 1:100, 2:100, 3:100, 4:100, 5:100.

[0061] The anti-hydrolysis agent suitable for the present invention can be a carbodiimide anti-hydrolysis agent. Carbodiimide is a class of organic compounds containing a -C=N=C- structural unit. Examples of available carbodiimide anti-hydrolysis agents include Stabaxol I, Stabaxol P, Stabaxol P200, Stabaxol P400, etc. In some embodiments, the anti-hydrolysis agent is a polycarbodiimide anti-hydrolysis agent, such as Stabaxol I. The mass ratio of the anti-hydrolysis agent to the ethylene acrylate copolymer can be (1-15):100, such as 2:100, 3:100, 4:100, 5:100, 6:100, 8:100, 10:100.

[0062] The electrode frame of the present invention can be prepared by dissolving the raw materials of ethylene propylene maleic anhydride copolymer coating and the raw materials of ethylene-acrylate copolymer coating in solvents to obtain coating solutions, then coating the ethylene propylene maleic anhydride copolymer coating solution on a substrate of the electrode frame, drying to obtain an ethylene propylene maleic anhydride copolymer coating, and then coating the ethylene-acrylate copolymer coating solution on the ethylene propylene maleic anhydride copolymer coating, and drying.

[0063] In some embodiments, the method of preparing the electrode frame of the present invention comprises the following steps:

[0064] (1) uniformly dispersing the raw material of ethylene propylene maleic anhydride copolymer coating in a solvent, filtering and degassing to obtain an ethylene propylene maleic anhydride copolymer coating solution;

[0065] The surface of the substrate of the electrode frame for the flow battery is polished, and then the ethylene propylene maleic anhydride copolymer coating solution is applied to the polished surface of the substrate, and dried to obtain the ethylene propylene maleic anhydride copolymer coating;

[0066] (2) uniformly dispersing the raw material of the ethylene-acrylate copolymer coating in a solvent, filtering and degassing to obtain an ethylene-acrylate copolymer coating solution;

[0067] The ethylene-acrylate copolymer coating solution is coated on the surface of the ethylene-propylene-maleic anhydride copolymer coating and dried to obtain the ethylene-acrylate copolymer coating.

[0068] In step (1), the solvent may be one or more selected from the group consisting of xylene, toluene, cyclohexane, methyl ethyl ketone and tetrahydrofuran. In some embodiments, the solvent is xylene.

[0069] The solid content of the ethylene propylene maleic anhydride copolymer coating solution may be 5wt%-30wt%, preferably 15wt%-25wt%, for example 18wt%, 20wt%, 22wt%.

[0070] In step (1), the surface of the substrate is polished, and then the ethylene propylene maleic anhydride copolymer coating solution is applied to the polished surface of the substrate. The polishing mesh size can be 800-1200 meshes.

[0071] In some embodiments, in step (1), the ethylene propylene maleic anhydride copolymer can be dissolved in a solvent (e.g., xylene) at high temperature in a dissolving kettle to obtain an ethylene propylene maleic anhydride copolymer solution with a suitable solid content, which is then cooled to room temperature for use, and then the first initiator and the first auxiliary cross-linking agent are mixed with the prepared ethylene propylene maleic anhydride copolymer solution at a certain ratio at high speed to form a uniform solution, the solution in the kettle is filtered through a filter, and the filtered solution is placed in a vacuum degassing kettle to evacuate the solution to remove bubbles in the solution, and then allowed to stand for use.

[0072] In step (1), the coating thickness of the coating solution on the substrate surface can be adjusted according to the target thickness of the ethylene-propylene-maleic anhydride copolymer coating.

[0073] In step (2), the solvent may be one or more selected from xylene, toluene, cyclohexane, methyl ethyl ketone, tetrahydrofuran, etc. In some embodiments, the solvent is xylene.

[0074] The solid content of the coating solution may be 5wt%-30wt%, preferably 15wt%-25wt%, for example 18wt%, 20wt%, 22wt%.

[0075] In some embodiments, in step (1), the ethylene-acrylate copolymer can be dissolved in a solvent (such as xylene) at high temperature in a dissolving kettle to obtain an ethylene-acrylate copolymer solution with a suitable solid content, which is then cooled to room temperature for use. Then, an initiator, a co-crosslinking agent, a coupling agent and an anti-hydrolysis agent are mixed with the prepared ethylene-acrylate copolymer solution in a certain proportion at high speed to form a uniform solution. The solution in the kettle is filtered through a filter, and the filtered solution is placed in a vacuum degassing kettle to evacuate the solution to remove bubbles in the solution, and the solution is allowed to stand for use.

[0076] In step (2), the coating thickness of the ethylene-acrylate copolymer coating solution on the ethylene-propylene-maleic anhydride copolymer coating surface can be adjusted according to the target thickness of the ethylene-acrylate copolymer coating.

[0077] In some embodiments, in step (1) and / or (2), the prepared coating solution can be delivered to the coating head by a delivery pump, the coating machine is started, and the coating is performed by the coating head, which can be in the form of a micro-dimple, a comma scraper, a slit, etc. The thickness of the coating can be controlled by controlling the pump delivery speed, the scraper height, and the casting speed, and then the electrode frame coated with the coating is sent to an oven for drying to evaporate the solvent. The drying temperature can be 140-180°C.

[0078] The present invention also includes a liquid flow battery, which includes the liquid flow battery electrode frame of the present invention. The liquid flow battery electrode frame of the present invention can replace the rubber ring used to seal the battery stack in the liquid flow battery. The liquid flow battery of the present invention is preferably an all-vanadium liquid flow battery.

[0079] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.

[0080] The ethylene propylene maleic anhydride copolymer used in the examples and comparative examples was purchased from ARLANXEO with the brand name Keltan® 1519R, the mass fraction of the ethylene structural unit was 49%, the mass fraction of the propylene structural unit was 49.1%, and the mass fraction of the maleic anhydride structural unit was 1.9%.

[0081] The hydroxy-terminated polybutadiene used in the examples and comparative examples was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.

[0082] The ethylene-acrylate copolymer used in the examples and comparative examples was purchased from SK, with the brand name Lotryl® 35BA40. The mass fraction of the ethylene structural unit is 65%, and the mass fraction of the acrylate structural unit is 35%. LOTRYL® 35BA40 is a random copolymer of ethylene and butyl acrylate produced by a high-pressure free radical polymerization process.

[0083] The electrode frame substrate for the polymer flow battery used in the examples and comparative examples was purchased from Dongguan Yixinda Plastic Material Co., Ltd. and the brand was 30% fiber-reinforced black PP board.

[0084] Example 1

[0085] Preparation of ethylene propylene maleic anhydride copolymer coating:

[0086] 1) Dissolve ethylene propylene maleic anhydride copolymer (EPDM)

[0087] Ethylene propylene maleic anhydride copolymer was dissolved in xylene, wherein the mass ratio of ethylene propylene maleic anhydride copolymer to xylene was 15:85, so that its solid content was 15%; the dissolution was carried out at a stirring speed of 300 r / min and a temperature of 100°C. After stirring for 30 minutes, when the solid particles were completely dissolved and the solution became translucent, the stirring was stopped.

[0088] 2) Add additives and mix well

[0089] The xylene solution of EPDM, initiator benzoyl peroxide, co-crosslinking agent triallyl isocyanurate (TAIC), and terminal hydroxyl polybutadiene were added into the reactor in a mass ratio of 100:3:2:5, and stirred for 30 minutes to mix evenly.

[0090] 3) Coating

[0091] First, the polypropylene (PP) flow battery electrode frame is roughened with 1000-mesh sandpaper, and then the solution obtained in step 2) is filtered, allowed to stand for defoaming, and applied on the flow battery electrode frame with a scraper, and dried at 160° C. to obtain a flow battery electrode frame containing an ethylene-propylene-maleic anhydride copolymer coating with a thickness of 10 μm.

[0092] Preparation of ethylene-acrylate copolymer coating:

[0093] 4) Dissolved ethylene-acrylate copolymer

[0094] Dissolve ethylene-acrylate copolymer in xylene, wherein the mass ratio of ethylene-acrylate copolymer to xylene is 20:80, so that its solid content is 20%; dissolve at a stirring speed of 600 r / min and a temperature of 80°C. After stirring for 30 minutes, when the solid particles are completely dissolved and the solution becomes translucent, stop stirring.

[0095] 5) Add additives and mix evenly

[0096] After the solution cooled to room temperature, the xylene solution of ethylene-acrylate copolymer, dibenzoyl peroxide (BPO), co-crosslinking agent triallyl isocyanurate (TAIC), coupling agent γ-aminopropyltriethoxysilane (KH550), coupling agent vinyltrimethoxysilane (KH171), and polycarbodiimide anti-hydrolysis agent (Stabaxol P200) were added into the reactor at a mass ratio of 100:3:3:2:2:5 and mixed evenly.

[0097] 6) Coating

[0098] The solution obtained in step 5 is filtered, allowed to stand to defoam, and coated on the electrode frame for the liquid flow battery in step 3 by a scraper coating method, and dried at 160°C to obtain an electrode frame for the liquid flow battery containing an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating, wherein the total thickness of the coating is 25 μm.

[0099] 7) Fit

[0100] Two electrode frames for liquid flow batteries, both with the above coating, are bonded and cured at 140°C, and an ion exchange membrane is sandwiched in between for bonding. The size of the ion exchange membrane can be slightly smaller than that of the electrode frame for the liquid flow battery, thereby increasing the utilization rate of the ion exchange membrane.

[0101] Example 2

[0102] Preparation of ethylene propylene maleic anhydride copolymer coating:

[0103] 1) Dissolve ethylene propylene maleic anhydride copolymer (EPDM)

[0104] Ethylene propylene maleic anhydride copolymer was dissolved in xylene, wherein the mass ratio of ethylene propylene maleic anhydride copolymer to xylene was 15:85, so that its solid content was 15%; the dissolution was carried out at a stirring speed of 300 r / min and a temperature of 100°C. After stirring for 30 minutes, when the solid particles were completely dissolved and the solution became translucent, the stirring was stopped.

[0105] 2) Add additives and mix well

[0106] Add the xylene solution of EPDM, initiator tert-butyl peroxydibenzoate, co-crosslinking agent triallyl isocyanurate (TAIC), and terminal hydroxyl polybutadiene into the reactor in a ratio of 100:3:2:5, and stir for 30 minutes to mix evenly.

[0107] 3) Coating

[0108] First, the polypropylene (PP) flow battery electrode frame was roughened with 1000-mesh sandpaper, and then the solution obtained in step 1 was filtered and allowed to stand for defoaming. The solution was coated on the flow battery electrode frame with a suitable thickness using a scraper, and the solvent was dried at 160°C to obtain a flow battery electrode frame with a dry glue thickness of 10 μm.

[0109] Preparation of ethylene-acrylate copolymer coating:

[0110] 4) Dissolved ethylene-acrylate copolymer

[0111] Dissolve ethylene-acrylate copolymer in xylene at a ratio of 20:80 to make a solid content of 20%. Dissolve at a stirring speed of 600 r / min and a temperature of 80°C. After stirring for 30 minutes, when the solid particles are completely dissolved and the solution becomes translucent, stop stirring.

[0112] 5) Add additives and mix evenly

[0113] After the solution temperature dropped to room temperature, the xylene solution of ethylene-acrylate copolymer, tert-butyl perbenzoate, co-crosslinking agent triallyl cyanurate, γ-aminopropyltriethoxysilane (KH550), vinyltrimethoxysilane (KH171), and polycarbodiimide anti-hydrolysis agent (Stabaxol 1) were added into the reactor in a ratio of 100:4:2:3:2:6 and mixed evenly.

[0114] 6) Coating

[0115] The solution obtained in step 5 is filtered, allowed to stand to defoam, and coated on the flow battery electrode frame in step 3 with a suitable thickness using a scraper. The solvent is dried at 160° C. to obtain a flow battery electrode frame with a dry glue thickness of 25 μm.

[0116] 7) Fit

[0117] Two electrode frames for liquid flow batteries, both with the above coating, are bonded and cured at 140°C, and an ion exchange membrane is sandwiched in between for bonding. The size of the ion exchange membrane can be slightly smaller than that of the electrode frame for the liquid flow battery, thereby increasing the utilization rate of the ion exchange membrane.

[0118] Comparative Example 1

[0119] The process is the same as in Example 1 except that the drying temperature in step 3 is changed to 80°C.

[0120] Comparative Example 2

[0121] Except that the PP plate in Example 1 is not polished with 1000-mesh sandpaper, the rest is the same as Example 1.

[0122] Comparative Example 3

[0123] Preparation of ethylene-acrylate copolymer coating:

[0124] 1) Dissolved ethylene-acrylate copolymer

[0125] Dissolve ethylene-acrylate copolymer in xylene at a mass ratio of 20:80 to make a solid content of 20%. Dissolve at a stirring speed of 600 r / min and a temperature of 80°C. After stirring for 30 minutes, when the solid particles are completely dissolved and the solution becomes translucent, stop stirring.

[0126] 2) Add additives and mix evenly

[0127] After the solution cooled to room temperature, the xylene solution of ethylene-acrylate copolymer, dibenzoyl peroxide (BPO), co-crosslinking agent triallyl isocyanurate (TAIC), γ-aminopropyltriethoxysilane (KH550), vinyltrimethoxysilane (KH171), and polycarbodiimide anti-hydrolysis agent (Stabaxol P200) were added into the reactor at a mass ratio of 100:3:3:2:2:5 and mixed evenly.

[0128] 3) Coating

[0129] The solution obtained in step 2) is filtered, allowed to stand for defoaming, and applied on a flow battery electrode frame polished with 800-mesh sandpaper using a scraper, and dried at 160° C. to obtain a flow battery electrode frame having an ethylene-acrylate copolymer coating with a thickness of 25 μm.

[0130] 4) Fit

[0131] Two electrode frames for liquid flow batteries, both with ethylene-acrylate copolymer coatings, are bonded and cured at 140°C, and an ion exchange membrane is sandwiched in between for bonding. The size of the ion exchange membrane can be slightly smaller than that of the electrode frame for the liquid flow battery, thereby increasing the utilization rate of the ion exchange membrane.

[0132] Comparative Example 4

[0133] Preparation of ethylene propylene maleic anhydride copolymer coating:

[0134] 1) Dissolve ethylene propylene maleic anhydride copolymer (EPDM)

[0135] Ethylene propylene maleic anhydride copolymer was dissolved in xylene, wherein the mass ratio of ethylene propylene maleic anhydride copolymer to xylene was 15:85, so that its solid content was 15%; the dissolution was carried out at a stirring speed of 300 r / min and a temperature of 100°C. After stirring for 30 minutes, when the solid particles were completely dissolved and the solution became translucent, the stirring was stopped.

[0136] 2) Add additives and mix well

[0137] The xylene solution of EPDM, initiator benzoyl peroxide, co-crosslinking agent triallyl isocyanurate (TAIC), and terminal hydroxyl polybutadiene were added into the reactor in a mass ratio of 100:3:2:5, and stirred for 30 minutes to mix evenly.

[0138] 3) Coating

[0139] First, the polypropylene (PP) flow battery electrode frame is roughened with 1000-mesh sandpaper, and then the solution obtained in step 2) is filtered, allowed to stand for defoaming, and applied on the flow battery electrode frame with a scraper, and dried at 160° C. to obtain a flow battery electrode frame containing an ethylene-propylene-maleic anhydride copolymer coating with a thickness of 10 μm.

[0140] 4) Fit

[0141] Two flow battery electrode frames, both coated with ethylene propylene maleic anhydride copolymer, are bonded and cured at 140°C, and an ion exchange membrane is sandwiched in between for bonding. The size of the ion exchange membrane can be slightly smaller than that of the flow battery electrode frame, thereby increasing the utilization rate of the ion exchange membrane.

[0142] Test Example 1

[0143] 1. Shear strength test method of coating adhesion: The electrode frames for flow batteries of Examples 1-2 and Comparative Examples 1-4 were cured at 140°C and subjected to shear tests on a tensile machine. The substrate of the electrode frame for flow batteries was 2 cm wide, and the contact area of ​​the coating was 2 cm long and 2 cm wide. The results are shown in Table 1.

[0144] 2. Test method for peeling strength of coating on ion exchange membrane: The electrode frame for flow battery of Examples 1-2 and Comparative Examples 1-4 was glued with 2 cm wide and 10 cm long ion exchange membrane at the coating, and after curing at 140°C, a 180° peeling test was performed on a tensile machine. The substrate of the electrode frame for flow battery was 2 cm wide. The results are shown in Table 1.

[0145] 3. Acid resistance test method: The electrode frames for flow batteries of Examples 1-2 and Comparative Examples 1-4 were placed in an all-vanadium flow battery electrolyte (vanadium ion concentration is 1.7 mol / L) and immersed at 50°C for 0-1000 hours. The shear strength and 180° peel strength were tested according to GB / T2790 standard. The results are shown in Table 2.

[0146] Table 1: Shear strength and peel strength test results

[0147]

[0148] Table 2: Acid resistance test results

[0149]

[0150] From the test results of Examples 1-2 in Tables 1 and 2, it can be seen that the electrode frame for the liquid flow battery of the present invention has very high shear strength and peel strength, can effectively seal the ion exchange membrane, and prevent the penetration of positive and negative electrode electrolytes; the electrode frame for the liquid flow battery of the present invention still has very high shear strength and peel strength after being immersed in the electrolyte for a long time, and can seal the liquid flow battery under long-term and strong acid conditions.

[0151] It can be seen from Table 1 and Table 2 that in Comparative Example 1, since the drying temperature in step 3 is too low, the shear strength and peel strength of the electrode frame obtained are 0, and the ion exchange membrane cannot be sealed; the substrate of Comparative Example 2 is not polished, and the shear strength of the obtained electrode frame is low; the difference between Example 1 and Comparative Examples 3-4 is that the electrode frame of Example 1 contains an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating, the electrode frame of Comparative Example 3 contains only an ethylene-acrylate copolymer coating, and the electrode frame of Comparative Example 4 contains only an ethylene-propylene-maleic anhydride copolymer coating. The results show that the shear strength of Comparative Example 3 is not as good as that of Example 1, and the peel strength of Comparative Example 4 is not as good as that of Example 1, indicating that the electrode frame for the liquid flow battery of the present invention has excellent shear strength and peel strength, and can effectively seal the ion exchange membrane.

[0152] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. An electrode frame for a liquid flow battery, characterized in that: The electrode frame for the flow battery comprises a substrate and an ethylene-propylene-maleic anhydride copolymer coating and an ethylene-acrylate copolymer coating located on the surface of the substrate, wherein the ethylene-propylene-maleic anhydride copolymer coating is located between the substrate and the ethylene-acrylate copolymer coating, and the raw materials of the ethylene-propylene-maleic anhydride copolymer coating comprise an ethylene-propylene-maleic anhydride copolymer, a first initiator, and a first auxiliary cross-linking agent in a mass ratio of 100:(2-4):(2-8); the raw materials of the ethylene-acrylate copolymer coating comprise an ethylene-acrylate copolymer, a second initiator, a second auxiliary cross-linking agent, a coupling agent, and an anti-hydrolysis agent in a mass ratio of 100:(2-8):(2-8):(2-8):(1-15); The ethylene-propylene-maleic anhydride copolymer is a copolymer of ethylene, propylene and maleic anhydride monomers or a copolymer of ethylene, propylene, maleic anhydride monomers and functional monomers; in the ethylene-propylene-maleic anhydride copolymer, the mass fraction of the ethylene structural unit is 30%-54%, the mass fraction of the propylene structural unit is 45%-69%, and the mass fraction of the maleic anhydride monomer structural unit is 1%-3%; The first auxiliary cross-linking agent and the second auxiliary cross-linking agent are each independently selected from one or more of triallyl isocyanurate, triallyl cyanurate, hydroxyl-terminated polybutadiene and trimethylolpropane trimethacrylate; The ethylene-acrylate copolymer is a copolymer of ethylene and acrylate monomers; in the ethylene-acrylate copolymer, the mass fraction of the ethylene structural unit is 50%-80%, and the mass fraction of the acrylate monomer structural unit is 20%-50%; The coupling agent is a silane coupling agent; The anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent.

2. The electrode frame for a flow battery according to claim 1, wherein: The material of the substrate is selected from one or more of PP, PEN, PPS and PET; and / or The surface of the substrate is roughened.

3. The electrode frame for a flow battery according to claim 1, wherein: The single-side thickness of the ethylene-propylene-maleic-anhydride copolymer coating is 5-20 μm; and / or The single-side thickness of the ethylene-acrylate copolymer coating is 10-25 μm.

4. The electrode frame for a flow battery according to claim 1, wherein: The functional monomer contains one or more groups selected from epoxy, anhydride and carbonyl groups; in the ethylene-propylene-maleic anhydride copolymer, the mass fraction of the functional monomer structural unit is 0-1%; The first initiator and the second initiator are each independently selected from one or more of a peroxide initiator and an azo initiator; The acrylic acid ester monomer is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate and butyl methacrylate; The coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane, γ-aminopropyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.

5. A method for preparing an electrode frame for a flow battery according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) uniformly dispersing the raw material of the ethylene-propylene-maleic anhydride copolymer coating in a solvent, filtering and degassing to obtain an ethylene-propylene-maleic anhydride copolymer coating solution; The surface of the substrate of the electrode frame for the flow battery is polished, and then the ethylene propylene maleic anhydride copolymer coating solution is applied to the polished surface of the substrate, and dried to obtain the ethylene propylene maleic anhydride copolymer coating; (2) uniformly dispersing the raw material of the ethylene-acrylate copolymer coating in a solvent, filtering and degassing to obtain an ethylene-acrylate copolymer coating solution; The ethylene-acrylate copolymer coating solution is coated on the surface of the ethylene-propylene-maleic anhydride copolymer coating and dried to obtain the ethylene-acrylate copolymer coating.

6. The method according to claim 5, characterized in that The solvent is selected from one or more of xylene, toluene, cyclohexane, methyl ethyl ketone and tetrahydrofuran.

7. The method according to claim 5, characterized in that In step (1), the solid content of the ethylene-propylene-maleic anhydride copolymer coating solution is 5wt%-30wt%.

8. The method according to claim 5, characterized in that In step (1), the grinding mesh size is 800-1200 mesh; and / or In step (1), the drying temperature is 140-180°C.

9. The method according to claim 5, characterized in that In step (2), the solid content of the ethylene-acrylate copolymer coating solution is 5wt%-30wt%; and / or In step (2), the drying temperature is 140-180°C.

10. A liquid flow battery, characterized in that: The liquid flow battery comprises the liquid flow battery electrode frame according to any one of claims 1 to 4 or comprises the liquid flow battery electrode frame prepared by the method according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • Gas diffusion layer incorporating a gasket

    CN101563803A

  • Fuel cell subassemblies incorporating subgasketed thrifted membranes

    CN102687323A

  • Solar cell sealing film and solar cell utilizing same

    CN103392238A

  • Membrane seal assembly

    CN116057739A

  • Coating slurry and preparation method thereof as well as frame film and product thereof

    CN117551374A