Polypropylene pipe and preparation method thereof

By using modified nanomaterials and crosslinked rubber particles in polypropylene pipelines and combining with beta nucleating agents to modify, the antibacterial, hydrophobic and toughness problems of the pipeline are solved, and excellent hydrophobic, antibacterial and toughening properties are achieved to prevent scale. and bacteria breed, improving the durability of the pipe.

CN118702996BActive Publication Date: 2024-11-19ERA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411204147.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Polypropylene pipelines are prone to breed bacteria and scale when transporting drinking water, and are brittlely damaged at low temperatures. The existing antibacterial and hydrophobic structure is not long-lasting and does not solve the problem of the pipeline toughness.

Method used

The double-layer polypropylene pipeline was prepared by extrusion granulation process. Modified nanotitanium dioxide-carrying silver, nanotitanium-doped zinc oxide and nanosilicon dioxide were introduced into the inner layer material, and mixed with EPDM master glue, high molecular weight silicone and cross-section The auxiliary agent forms fine cross-linked rubber particles, improves impact resistance and hydrophobic effect, and adds β nucleating agent to the outer layer material to improve toughness.

Benefits of technology

The excellent hydrophobic, antibacterial and toughening properties of the pipe are achieved, preventing scale formation and bacterial growth, and improving the durability of the pipe and reducing fluid resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702996B_ABST
    Figure CN118702996B_ABST
Patent Text Reader

Abstract

The invention discloses a polypropylene pipe and a preparation method thereof, and relates to the technical field of pipes. By optimizing the inner layer material used to prepare the inner layer of the pipe, an EPDM masterbatch is first prepared and then mixed with polypropylene to prepare the inner layer material. In the preparation process of the EPDM masterbatch, modified nano titanium dioxide silver, modified nano titanium-doped zinc oxide, and modified nano silicon dioxide modified by a silane coupling agent are introduced, and EPDM grafted maleic anhydride is also introduced. In the process of preparing the inner layer material, high molecular weight silicone, polypropylene grafted maleic anhydride and a crosslinking aid are introduced while mixing polypropylene and the EPDM masterbatch, and the crosslinking aid includes N-cyclohexyl-2-benzothiazole sulfonamide, stearic acid, 2,4-di-tert-butyl peroxide isopropylbenzene and triallyl isocyanurate. The inner layer of the pipe prepared by the preparation method provided by the invention has excellent hydrophobic, antibacterial and toughening properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipelines, and in particular to a polypropylene pipeline and a preparation method thereof. Background Art

[0002] Polyolefin pipes are widely used in building water supply pipes, industrial pipes, irrigation and heating. When transporting drinking water, especially when the water flow stops, bacteria will inevitably grow. Bacteria will produce biofilms that affect water quality and also cause scaling in pipes. At the same time, due to the problem of water hardness, the presence of calcium ions and magnesium ions will produce precipitates, leading to scale. Scale not only affects water quality, but also reduces the pipe diameter, increases the roughness of the pipe wall surface, and affects flow.

[0003] In addition, the temperature in winter is close to the glass transition temperature of polypropylene, which makes polypropylene brittle at low temperatures and prone to brittle failure during transportation and installation. To address this problem, co-extrusion is often used to add antibacterial masterbatch and hydrophobic masterbatch to the inner layer. However, after long-term use of the pipeline, the antibacterial and hydrophobic structure is not durable, and the toughness problem of the pipeline is not solved.

[0004] Therefore, there is an urgent need to provide polypropylene pipes that have excellent hydrophobic, antibacterial and toughening properties.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a polypropylene pipe and a preparation method thereof, aiming to provide a polypropylene pipe with excellent hydrophobic, antibacterial and toughening properties.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a method for preparing a polypropylene pipe, comprising preparing an outer layer material and an inner layer material by an extrusion granulation process respectively, and then performing double-layer extrusion using the outer layer material and the inner layer material;

[0009] The preparation process of the inner layer material includes:

[0010] The nano-titanium dioxide loaded with silver, the nano-titanium-doped zinc oxide and the nano-silicon dioxide are modified by using a silane coupling agent to obtain modified nano-titanium dioxide loaded with silver, modified nano-titanium-doped zinc oxide and modified nano-silicon dioxide respectively;

[0011] The modified nano-titanium dioxide loaded with silver, the modified nano-titanium-doped zinc oxide, the modified nano-silicon dioxide, the EPDM grafted maleic anhydride and the EPDM are mixed and extruded to obtain the EPDM masterbatch;

[0012] The inner layer material is obtained by blending and extruding polypropylene, EPDM masterbatch, alkane oil, high molecular weight silicone, polypropylene grafted maleic anhydride and a cross-linking aid; wherein the number average molecular weight of the high molecular weight silicone is 500,000-1.5 million, and the cross-linking aid includes N-cyclohexyl-2-benzothiazole sulfonamide, stearic acid, 2,4-di-tert-butyl peroxide isopropylbenzene and triallyl isocyanurate.

[0013] In an optional embodiment, the raw materials for preparing the inner layer material include, by mass: 100 parts of polypropylene, 20-50 parts of EPDM masterbatch, 4-10 parts of alkane oil, 1-5 parts of high molecular weight silicone, and 1-5 parts of polypropylene grafted maleic anhydride (PP-g-MAH); the cross-linking aids include 0.1~0.5 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.1~0.5 parts of stearic acid (SA), 0.2~1 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP) and 0.2~1 parts of triallyl isocyanurate (TAIC).

[0014] In an optional embodiment, when the inner layer material is prepared from the EPDM masterbatch, a twin-screw extrusion process is adopted, and the twin-screw extruder is provided with an end feeding port and a middle feeding port, and the end feeding port is provided near the inlet end of the twin-screw extruder;

[0015] Polypropylene, EPDM masterbatch, alkane oil, high molecular weight silicone and polypropylene grafted maleic anhydride are added from the end feed port, and the crosslinking aid is added from the middle feed port;

[0016] Preferably, the temperature between the inlet end and the middle feed port of the twin-screw extruder is controlled to be 100°C-180°C, and the temperature from the middle feed port to the end of the twin-screw extruder is controlled to be 160°C-220°C. After extrusion, the strips are formed through a porous die, and then crushed by a crusher and sieved by a screen to prepare 2mm-6mm EPDM masterbatch particles.

[0017] In an optional embodiment, the twin-screw extruder includes a first heating zone to a tenth heating zone arranged in sequence, the temperature of the first heating zone to the fifth heating zone is 100°C-180°C, and the temperature of the sixth heating zone to the tenth heating zone is 160°C-220°C; the speed of the twin-screw extruder is 300rpm-600rpm;

[0018] Preferably, the end feed port is located in the first heating zone, the middle feed port is located in the fifth to seventh heating zones, the temperature of the sixth to seventh heating zones is 160°C-180°C, and the temperature of the eighth to tenth heating zones is 180°C-220°C.

[0019] In an optional embodiment, the raw materials for preparing the EPDM masterbatch include, by weight: 100 parts of EPDM, 0.5-5.0 parts of modified nano-titanium dioxide loaded with silver, 0.5-5 parts of modified nano-titanium-doped zinc oxide, 10-40 parts of modified nano-silicon dioxide, 30-80 parts of alkane oil, 0.5-10 parts of EPDM grafted maleic anhydride, and 1-4 parts of antioxidant;

[0020] Preferably, the antioxidant is selected from at least one of antioxidant 1010 and antioxidant 1076;

[0021] More preferably, the antioxidant comprises 0.5-2 parts of antioxidant 1010 and 0.5-2 parts of antioxidant 1076;

[0022] Preferably, the particle sizes of the modified nano-titanium dioxide loaded with silver, the modified nano-titanium-doped zinc oxide and the modified nano-silicon dioxide are less than or equal to 100 nm.

[0023] In an optional embodiment, the process of preparing the EPDM masterbatch includes: mixing the raw materials for preparing the EPDM masterbatch, double-roll extruding and cooling to form a sheet, and then crushing by a crusher and screening by a sieve to prepare EPDM masterbatch particles with a particle size of 2 mm-6 mm;

[0024] Preferably, the process of mixing the raw materials for preparing the EPDM masterbatch includes: mixing for 10 min to 30 min at 150° C. to 170° C. and 30 rpm to 60 rpm using an internal mixer.

[0025] In an optional embodiment, the process of preparing modified nano titanium dioxide loaded with silver, modified nano titanium-doped zinc oxide and modified nano silicon dioxide comprises:

[0026] Soak nano-titanium dioxide loaded with silver, nano-titanium-doped zinc oxide and nano-silicon dioxide in a silane coupling agent solution for 10-60 minutes respectively, and then dry;

[0027] Preferably, the concentration of the silane coupling agent solution is 0.5%-5%;

[0028] Preferably, the solvents used to prepare the silane coupling agent solution are water and ethanol, and the volume ratio of water to ethanol is (1.5-3.0):1.

[0029] In an optional embodiment, the outer layer material is prepared by: mixing polypropylene particles and a β-nucleating agent, followed by extrusion granulation;

[0030] Preferably, the raw materials for preparing the outer layer material include, by weight: 100 parts of polypropylene particles and 0.05-1.00 parts of β-nucleating agent; the β-nucleating agent is selected from at least one of carboxylates, rare earth compounds and amide compounds.

[0031] In an optional embodiment, during the double-layer extrusion using the outer layer material and the inner layer material, the extrusion temperature is controlled to be 160° C.-220° C. and the torque is 60%-85%;

[0032] Preferably, the outer diameter of the polypropylene pipe is 20 mm-30 mm, the outer layer wall thickness is 3.5 mm-5.0 mm, and the inner layer thickness is 0.4 mm-0.6 mm.

[0033] In a second aspect, the present invention provides a polypropylene pipe prepared by the preparation method of any one of the aforementioned embodiments.

[0034] The present invention has the following beneficial effects: by optimizing the inner layer material used for preparing the inner layer of the pipeline, the EPDM masterbatch is first prepared and then mixed with polypropylene to prepare the inner layer material, specifically:

[0035] In the preparation process of EPDM masterbatch, modified nano-titanium dioxide loaded with silver, modified nano-titanium-doped zinc oxide, and modified nano-silicon dioxide modified by silane coupling agent are introduced. EPDM grafted maleic anhydride is also introduced. EPDM grafted maleic anhydride will attract the polar groups in the silane coupling agent, allowing the compatibilizer (EPDM grafted maleic anhydride) to be enriched around the silane-modified particles. At the same time, the maleic anhydride group forms chemical bonds with the silane-modified nano-titanium dioxide loaded with silver, nano-titanium-doped zinc oxide, nano-silicon oxide, etc., which improves the compatibility of the particles and enhances the adhesion of the particles in the EPDM matrix.

[0036] In the process of preparing the inner layer material, high molecular weight silicone, polypropylene grafted maleic anhydride and crosslinking aids are introduced while mixing polypropylene and EPDM masterbatch. The crosslinking aids include N-cyclohexyl-2-benzothiazole sulfonamide, stearic acid, 2,4-di-tert-butyl peroxide isopropylbenzene and triallyl isocyanurate. Under the action of high-speed shear, the EPDM masterbatch gradually crosslinks and undergoes a phase transition in the PP matrix to form fine crosslinked rubber particles. These particles are wrapped with nano-titanium dioxide silver, nano-titanium-doped zinc oxide, and nano-silicon dioxide. The crosslinking effect can fix the shape of the rubber particles and allow the particles to exist stably in the rubber phase. These rubber particles greatly improve the impact resistance in the polypropylene matrix and form micron-level protrusions on the surface of the material. By blending high molecular weight silicone with maleic anhydride grafted polypropylene (PP-g-MAH), PP-g-MAH has good compatibility with PP resin. Since the grafted maleic anhydride group also has good compatibility with EPDM-g-MAH, adding PP-g-MAH as a compatibilizer can improve the combination of EPDM rubber particles and PP. High molecular weight silicone and nano-silica treated with silane coupling agent are dispersed in the polypropylene matrix, and together with EPDM rubber particles, nano-scale and micron-scale protrusions are constructed on the inner surface of the pipe to form a rough surface.

[0037] The inner layer of the pipeline prepared by the preparation method provided by the present invention has excellent hydrophobic, antibacterial and toughening properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0039] Figure 1 A schematic structural diagram of a twin-screw extruder provided in an embodiment of the present invention;

[0040] Figure 2 This is the DSC graph of the outer layer of β-modified PPR.

[0041] Icons: 100-twin-screw extruder; 101-first heating zone; 102-second heating zone; 103-third heating zone; 104-fourth heating zone; 105-fifth heating zone; 106-sixth heating zone; 107-seventh heating zone; 108-eighth heating zone; 109-ninth heating zone; 110-tenth heating zone; 111-end feed port; 112-middle feed port; 113-exhaust port; 114-vacuum evacuator. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0043] The embodiment of the present invention provides a method for preparing a polypropylene pipe, comprising preparing an outer layer material and an inner layer material by an extrusion granulation process, and then performing double-layer extrusion using the outer layer material and the inner layer material. By adding modified cross-linked functional particles to the material and modifying it with a compatibilizer, the adhesion of the particles is improved to achieve hydrophobic, antibacterial, and toughening effects. By modifying the inner layer material to form fine functional rubber particles in the plastic, the antibacterial, anti-scaling, and toughening effects of the inner wall of the pipe are achieved.

[0044] Specifically, the following steps are included:

[0045] S1. Preparation of outer layer materials

[0046] The preparation process of the outer layer material includes: mixing polypropylene particles and a beta nucleating agent, and then extruding and granulating to obtain the outer layer material with a particle size of 2 to 6 mm.

[0047] In some embodiments, the raw materials for preparing the outer layer material include, by weight fraction: 100 parts of polypropylene particles and 0.05-1.00 parts of β-nucleating agent. On the premise that the amount of polypropylene particles is 100 parts, the amount of β-nucleating agent can be 0.05 parts, 0.10 parts, 0.30 parts, 0.50 parts, 0.80 parts, 1.00 parts, etc. In the actual operation process, 100 parts of polypropylene particles and 0.05-1.00 parts of β-nucleating agent can be added to a mixer and mixed for 10 minutes to 50 minutes, and then granulated by twin-screw extrusion to prepare the outer layer material.

[0048] Furthermore, the β-nucleating agent is selected from at least one of carboxylates, rare earth compounds and amide compounds. The β-nucleating agent can be any one or more of the above, for example, WBG-2, nμ-100, TMB-5, etc.

[0049] It should be noted that the outer layer is the pressure-bearing layer of the pipeline. The polypropylene material used is pipeline-grade material through β-crystal modification. Carboxylates, rare earth compounds, and amide compounds are added as β-crystal nucleating agents to change its crystal form and increase the number of tie molecules between crystals. This can effectively improve the toughness of the pipeline, improve the creep resistance of the pipeline, and ensure long-term hydrostatic performance.

[0050] Specifically, the overall thickness of the pipeline pressure-bearing layer must meet the pipeline design requirements and ensure that the pipeline's pressure-bearing capacity meets the standard requirements when supplying hot and cold water. The pressure-bearing layer may also include functional layers such as oxygen barrier layers and thermal insulation layers on the premise of meeting the pressure-bearing requirements. The raw materials used for the part of the pipeline responsible for the pressure-bearing function must be certified pipeline-grade raw materials.

[0051] S2. Preparation of inner layer material

[0052] The inner layer is an antibacterial, hydrophobic and toughened modified layer. The inner layer is also based on pipeline-grade polypropylene raw materials and has been subjected to antibacterial, anti-fouling and toughening modification. The preparation process of the inner layer material includes:

[0053] (1) Preparation of silane-modified particles

[0054] Nano-titanium dioxide loaded with silver, nano-titanium-doped zinc oxide and nano-silicon dioxide are modified by silane coupling agent to obtain modified nano-titanium dioxide loaded with silver, modified nano-titanium-doped zinc oxide and modified nano-silicon dioxide. Through the modification of silane coupling agent, silicon-oxygen chemical bonds are formed with the powder, so that the functional powder changes from the original hydrophilic and oleophobic to oleophilic and hydrophobic.

[0055] It should be noted that the bactericidal and antibacterial mechanisms of nano-titanium dioxide-loaded silver and nano-titanium-doped zinc oxide are as follows:

[0056] The sterilization principle of nano-titanium dioxide loaded with silver: nano-titanium dioxide forms peroxide free radicals and hydroxide particles under the catalytic action of ultraviolet light, which can react with most organic matter and kill bacteria. Nano-titanium dioxide can permanently sterilize. The silver ions released by silver nanoparticles have a strong antibacterial effect, and silver ions improve the photocatalytic effect of nano-titanium dioxide.

[0057] The antibacterial mechanism of titanium-doped nano zinc oxide (Ti-doped ZnO) is similar to that of ordinary nano zinc oxide, but the presence of titanium can enhance its antibacterial properties. The following are the main antibacterial mechanisms of titanium-doped nano zinc oxide:

[0058] (a) Reactive oxygen species (ROS) generation

[0059] Titanium-doped nano-zinc oxide can generate more reactive oxygen species (ROS) under light conditions, such as hydroxyl radicals (•OH), superoxide anions (O2⁻•) and hydrogen peroxide (H2O2). These reactive oxygen species are highly oxidizing and can destroy bacterial cell membranes, proteins and DNA, leading to bacterial death. Titanium-doped enhancement effect: After the addition of titanium, the band gap width of nano-zinc oxide and the separation efficiency of photogenerated electron-hole pairs are increased, thereby generating more ROS and improving the antibacterial efficiency.

[0060] (b) Direct contact sterilization

[0061] Nano zinc oxide particles can directly attach to the surface of bacterial cells, destroy the cell membrane structure through physical and chemical effects, causing the cell contents to leak out, thereby killing bacteria. Titanium-doped enhancement effect: The incorporation of titanium may change the surface properties of nanoparticles, making their interaction with bacterial cell membranes stronger, thereby enhancing the direct contact sterilization effect.

[0062] (c) Ion release

[0063] Nano zinc oxide can release zinc ions (Zn²⁺) in aqueous solution, which can bind to proteins on bacterial cell walls and cell membranes, disrupting bacterial metabolic processes and inhibiting their growth and reproduction. Titanium-doped enhancement effect: Titanium-doped particles may affect the solubility of ZnO particles and the release rate of Zn²⁺, thereby enhancing the antibacterial effect.

[0064] (d) Photocatalytic effect

[0065] Under ultraviolet or visible light irradiation, nano-ZnO exhibits strong photocatalytic activity, and the generated electron-hole pairs can further enhance the generation of ROS, thereby enhancing the antibacterial activity.

[0066] Titanium-doping enhancement effect: Titanium doping can broaden the light absorption range of ZnO, especially in the visible light region, and improve its antibacterial effect under natural light.

[0067] (e) Changes in membrane permeability

[0068] Titanium-doped nano-zinc oxide particles can change the permeability of bacterial cell membranes, leading to changes in cell membrane potential and osmotic pressure imbalance, ultimately leading to bacterial cell death.

[0069] In some embodiments, the process of preparing modified nano-titanium dioxide loaded with silver, modified nano-titanium-doped zinc oxide, and modified nano-silicon dioxide comprises: soaking nano-titanium dioxide loaded with silver, nano-titanium-doped zinc oxide, and nano-silicon dioxide in a silane coupling agent solution for 10 min-60 min (e.g., 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc.), respectively, and then drying. The soaking process can be combined with ultrasonic oscillation, and the drying method is not limited, and can be dried at room temperature, such as drying at room temperature for 20 h-30 h.

[0070] Furthermore, the concentration of the silane coupling agent solution is 0.5%-5%, at which the modification effect is better and the hydrophobic effect can be further improved. The concentration of the silane coupling agent solution refers to the mass fraction of the silane coupling agent in the solution, which can be 0.5%, 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, etc.

[0071] Furthermore, the solvents used in preparing the silane coupling agent solution are water and ethanol, and the volume ratio of water to ethanol is (1.5-3.0):1, such as 1.5:1, 2.0:1, 2.5:1, 3.0:1, etc. By adjusting the amount of the mixed solvent, the concentration of the prepared silane coupling agent solution meets the requirements.

[0072] Specifically, nano-titanium dioxide loaded with silver, nano-titanium-doped zinc oxide and nano-silicon dioxide can be commercially available raw materials, and preferably have a particle size of less than or equal to 100 nm.

[0073] (2) Preparation of EPDM masterbatch

[0074] EPDM masterbatch is obtained by mixing and extruding modified nano-titanium dioxide loaded silver, modified nano-titanium-doped zinc oxide, modified nano-silicon dioxide, EPDM grafted maleic anhydride (compatibilizer, EPDM-g-MAH) and EPDM. Due to the polar effect, the maleic anhydride group of EPDM-g-MAH will attract the polar group in the silane coupling agent, allowing the compatibilizer to be enriched around the silane-modified particles. At the same time, the maleic anhydride group forms chemical bonds with the silane-modified nano-titanium dioxide loaded silver, nano-titanium-doped zinc oxide, nano-silicon oxide, etc., which improves the compatibility of the particles and increases the adhesion of the particles in the EPDM matrix.

[0075] Specifically, EPDM grafted maleic anhydride can be a commercially available material, such as VA1801 from ExxonMobil, or can be prepared independently using conventional methods. EPDM is a terpolymer obtained by copolymerization of ethylene, propylene and non-conjugated dienes, also known as ethylene propylene diene monomer rubber. EPDM can be a commercially available material, such as 3072EM and 3092M from Mitsui Chemicals.

[0076] In some embodiments, the raw materials for preparing EPDM masterbatch include, by weight: 100 parts of EPDM, 0.5-5.0 parts of modified nano-titanium dioxide loaded with silver, 0.5-5 parts of modified nano-titanium-doped zinc oxide, 10-40 parts of modified nano-silicon dioxide, 30-80 parts of alkane oil, 0.5-10 parts of EPDM grafted maleic anhydride and 1-4 parts of antioxidant. The amount of each component used within the above range can improve the compatibility of the modified particles in the EPDM matrix and improve the adhesion of the particles in the EPDM matrix.

[0077] Specifically, under the premise that the amount of EPDM is 100 parts, the amount of modified nano-titanium dioxide loaded with silver can be 0.5 parts, 1.0 parts, 2.0 parts, 3.0 parts, 4.0 parts, 5.0 parts, etc., the amount of modified nano-titanium-doped zinc oxide can be 0.5 parts, 1.0 parts, 2.0 parts, 3.0 parts, 4.0 parts, 5.0 parts, etc., the amount of modified nano-silicon dioxide can be 10 parts, 20 parts, 30 parts, 40 parts, etc., the amount of alkane oil can be 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, etc., the amount of EPDM grafted maleic anhydride can be 0.5, 1.0 parts, 3.0 parts, 5.0 parts, 8.0 parts, 10.0 parts, etc., and the amount of antioxidant can be 1 part, 2 parts, 3 parts, 4 parts, etc. The particle sizes of the modified nano-titanium dioxide loaded with silver, the modified nano-titanium-doped zinc oxide and the modified nano-silicon dioxide are less than or equal to 100 nm.

[0078] Further, the antioxidant is selected from at least one of antioxidant 1010 and antioxidant 1076, and the antioxidant can be any one or more of the above. In a preferred embodiment, under the premise that the amount of EPDM is 100 parts, the antioxidant includes 0.5-2 parts of antioxidant 1010 and 0.5-2 parts of antioxidant 1076, the amount of antioxidant 1010 can be 0.5 parts, 1.0 parts, 2.0 parts, etc., and the amount of antioxidant 1076 can be 0.5 parts, 1.0 parts, 2.0 parts, etc. Antioxidant 1010 and antioxidant 1076 can both be commercially available raw materials.

[0079] In some embodiments, the process of preparing EPDM masterbatch includes: mixing the raw materials for preparing EPDM masterbatch, extruding with cooled double rollers to cool and form flakes, and then crushing with a crusher and screening with a screen to prepare 2mm-6mm EPDM masterbatch particles. The raw materials can be mixed in any manner, and a mixer can be used to mix the materials to improve the uniformity of the mixing.

[0080] In the actual operation process, an internal mixer is used to mix at 150℃-170℃, 30rpm-60rpm for 10min-30min. Specifically, the temperature of the internal mixer can be set to 150℃-170℃, and the speed can be set to 30rpm-60rpm. The lower temperature ensures that EPDM does not decompose. First, add EPDM to the internal mixer. After the torque reaches a balance, add alkane oil, nano-titanium dioxide-loaded silver, nano-titanium-doped zinc oxide, and nano-silicon dioxide, and keep it for 10-30min.

[0081] (3) Co-extrusion with polypropylene to prepare inner layer material

[0082] The inner layer material is obtained by blending and extruding polypropylene (PP), EPDM masterbatch, alkane oil, high molecular weight silicone, polypropylene grafted maleic anhydride and a cross-linking aid; wherein the number average molecular weight of the high molecular weight silicone is 500,000-1.5 million, and the cross-linking aid includes N-cyclohexyl-2-benzothiazole sulfonamide, stearic acid, 2,4-di-tert-butyl peroxide isopropylbenzene and triallyl isocyanurate.

[0083] It should be noted that when EPDM masterbatch is blended with PP, PP or EPDM will form a dispersed phase, and a cross-linking system is added. Under the action of high-speed shear, the EPDM masterbatch is gradually cross-linked, and a phase transition occurs in the PP matrix to form fine cross-linked rubber particles. These particles are coated with nano-titanium dioxide-loaded silver, nano-titanium-doped zinc oxide, and nano-silicon dioxide. The cross-linking effect can fix the morphology of the rubber particles and allow the particles to exist stably in the rubber phase. These rubber particles greatly improve the impact resistance in the polypropylene matrix, and at the same time form a micron-level protrusion structure on the surface of the material. In addition, high molecular weight silicone is blended with maleic anhydride grafted polypropylene (PP-g-MAH). PP-g-MAH has good compatibility with PP resin. Since the grafted maleic anhydride group also has good compatibility with EPDM-g-MAH, adding PP-g-MAH as a compatibilizer can improve the bonding between EPDM rubber particles and PP. Nano-silica treated with high molecular weight silicone and silane coupling agent dispersed in the polypropylene matrix can form nano-scale and micron-scale protrusions on the inner surface of the pipe together with EPDM rubber particles to form a rough surface, thereby achieving a hydrophobic effect.

[0084] Specifically, rough surface hydrophobicity is a bionic principle of lotus leaves, which can reduce fluid resistance and prevent scale adsorption. The present invention can form a rough surface in the pipe by optimizing the preparation process of the inner layer material, which is conducive to improving the hydrophobic effect.

[0085] In some embodiments, the raw materials for preparing the inner layer material include, by weight: 100 parts of polypropylene, 20-50 parts of EPDM masterbatch, 4-10 parts of alkane oil, 1-5 parts of high molecular weight silicone, 1-5 parts of polypropylene grafted maleic anhydride (PP-g-MAH); crosslinking aids include 0.1-0.5 parts of N-cyclohexyl-2-benzothiazole sulfenamide (CZ), 0.1-0.5 parts of stearic acid (SA), 0.2-1 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP) and 0.2-1 parts of triallyl isocyanurate (TAIC). By adjusting the amount of each component, the hydrophobic effect of the inner layer can be further improved, so that the inner layer of the pipeline has excellent hydrophobic, antibacterial and toughening properties.

[0086] Specifically, under the premise that the amount of polypropylene is 100 parts, the amount of EPDM masterbatch can be 20 parts, 30 parts, 40 parts, 50 parts, etc., the amount of alkane oil can be 4 parts, 6 parts, 8 parts, 10 parts, etc., the amount of high molecular weight silicone can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc., the amount of polypropylene grafted maleic anhydride can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc., the amount of N-cyclohexyl-2-benzothiazole sulfonamide can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc. The amount of iodine can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, etc., the amount of stearic acid can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, etc., the amount of 2,4-di-tert-butyl peroxide isopropylbenzene can be 0.2 part, 0.4 part, 0.6 part, 0.8 part, 1.0 part, etc., the amount of triallyl isocyanurate can be 0.2 part, 0.4 part, 0.6 part, 0.8 part, 1.0 part, etc.

[0087] In some embodiments, when the inner layer material is prepared from EPDM masterbatch, a twin-screw extrusion process is used. Figure 1 The twin-screw extruder 100 shown is used for extrusion. The twin-screw extruder 100 is provided with an end feed port 111 and a middle feed port 112. The end feed port 111 is provided close to the inlet end of the twin-screw extruder. Polypropylene, EPDM masterbatch, alkane oil, high molecular weight silicone and polypropylene grafted maleic anhydride are added from the end feed port 111, and a cross-linking aid is added from the middle feed port 112. The other raw materials are first heated and melted and then mixed with the cross-linking aid for cross-linking.

[0088] In some embodiments, the temperature between the inlet end of the twin-screw extruder and the middle feeding port 112 is controlled to be 100°C-180°C (such as 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc.), and the temperature from the middle feeding port 112 to the end of the twin-screw extruder is 160°C-220°C (such as 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc.), and the cross-linking reaction is promoted by further controlling the temperature of each section.

[0089] In some embodiments, the twin-screw extruder 100 includes a first heating zone 101 to a tenth heating zone 110 arranged in sequence, as shown in the figure, including a first heating zone 101, a second heating zone 102, a third heating zone 103, a fourth heating zone 104, a fifth heating zone 105, a sixth heating zone 106, a seventh heating zone 107, an eighth heating zone 108, a ninth heating zone 109 and a tenth heating zone 110, and the temperature is controlled in intervals. The temperature of the first heating zone to the fifth heating zone is 100°C-180°C, the temperature of the sixth heating zone to the tenth heating zone is 160°C-220°C, the end feed port 111 is located in the first heating zone 101, and the middle feed port 112 is located in the fifth heating zone 105 to the seventh heating zone 107, such as being located in the sixth heating zone 106.

[0090] Specifically, the end feeding port 111 is fed by a screw, and PP, EPDM masterbatch, and PP-g-MAH are added to make PP and EPDM reach a molten state and fully mixed. The cross-linking aid is added at the middle feeding port 112 through screw feeding metering.

[0091] Furthermore, the twin-screw extruder 100 is also provided with an exhaust port 113 for exhausting the gas generated during the extrusion process, and may also be provided with a vacuum pump 114, which can be turned on when vacuum extrusion is required.

[0092] Furthermore, the speed of the twin-screw extruder is 300rpm-600rpm, and the temperature of the sixth heating zone to the seventh heating zone is 160℃-180℃, which can reduce the crosslinking rate and allow the crosslinking agent to be fully dispersed. The main engine speed is increased to enhance the shearing effect, so that the rubber and PP can undergo phase inversion and form fine rubber particles in the PP matrix. The temperature of the eighth heating zone to the tenth heating zone is 180℃-220℃. The temperature of the eighth heating zone to the tenth heating zone is increased to accelerate the crosslinking reaction. Under high speed, the residence time of the material in the screw barrel is shortened, and the crosslinking reaction requirements can still be met, while avoiding degradation. The maximum temperature should be controlled within 220℃.

[0093] After extrusion by a twin-screw extruder, it passes through a porous die to form strips, and then is cooled and pelletized to obtain a length of 2~6mm EPDM masterbatch particles after crushing by a crusher and sieving by a sieve.

[0094] It should be noted that the hydrophobic working principle of the solution of the embodiment of the present invention is as follows:

[0095] (a) The material has low surface energy

[0096] Silane modification can give nano-titanium dioxide silver, nano-zinc oxide, and nano-silicon dioxide low surface energy, making them hydrophobic and oleophilic. In addition to improving processing, the addition of alkane oil to EPDM rubber can also reduce the surface energy of the material.

[0097] (b) Micron-nano protrusion structure

[0098] Silane-modified nano-silicon dioxide, titanium dioxide-loaded silver, and nano-zinc dioxide reduce the surface energy of the material. The combination of EPDM and nanoparticles creates a rough surface that combines micrometers and nanometers. The micro-rough surface achieved by the stacking of micrometer- and nanometer-level particles reduces the contact angle of the surface from a physical level. It can reduce the contact of water flow and prevent scale from staying. Therefore, the formation of scale is prevented through two principles.

[0099] S3, double layer extrusion

[0100] The outer layer material and the inner layer material are used to pass through the polyolefin double-host single screw production line for double-layer co-extrusion to produce a double-layer pipe. The production process and flow are consistent with the conventional double-layer co-extrusion pipe. In this process, the extrusion temperature is controlled at 160℃-220℃ and the torque is 60%-85%.

[0101] In some embodiments, the outer diameter of the polypropylene pipe is 20mm-30mm, such as 20mm, 23mm, 25mm, 28mm, 30mm, etc.; the outer wall thickness is 3.5mm-5.0mm, such as 3.5mm, 4.0mm, 4.5mm, 5.0mm, etc.; the inner layer thickness is 0.4mm-0.6mm, such as 0.4mm, 0.5mm, 0.6mm, etc.

[0102] An embodiment of the present invention provides a polypropylene pipe, which is prepared by the preparation method provided by the embodiment of the present invention. The inner layer of the pipe has excellent hydrophobic, antibacterial and toughening properties.

[0103] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0104] Example 1

[0105] This embodiment provides a method for preparing a polypropylene pipe, comprising the following steps:

[0106] (1) Outer material production

[0107] 0.5 parts of β-crystal nucleating agent (nμ-100, purchased from New Japan Chemical Co., Ltd., model nμ-100) were added to every 100 parts of polypropylene, mixed in a mixer for 20 minutes, and granulated by single-screw extrusion. The temperature of the granulator was controlled at 160~200℃ to obtain an outer layer material with a particle size of 2~6mm.

[0108] (2) Treat nano-titanium dioxide loaded with silver, titanium-doped nano-zinc oxide, and nano-silicon dioxide with a silane coupling agent. The specific operation is to treat nano-titanium dioxide loaded with silver, nano-silicon dioxide, and titanium-doped nano-zinc oxide with a water / ethanol solution of a silane coupling agent under ultrasonic oscillation conditions, soak for 30 minutes, the concentration of the silane coupling agent is 2%, and the volume ratio of water to ethanol is 7:3, and then dry at room temperature for 24 hours. The particle sizes of nano-titanium dioxide loaded with silver (VKT07 of Xuancheng Jingrui New Materials Co., Ltd.), titanium-doped nano-zinc oxide (CYJH05 of Hangzhou Jiupeng New Materials Co., Ltd.), and nano-silicon dioxide (AM-SiO2-021-1 of Zhejiang Yamei Nanotechnology Co., Ltd.) are 30±10nm, 15±10nm, and 20±10nm, respectively, and the silane coupling agent is γ-aminopropyltriethoxysilane.

[0109] (3) 100 parts of EPDM were added to the mixer, and the mixer temperature was controlled at 160°C and the speed was controlled at 50 rpm. During this process, antioxidants 1010 and 1076 were added, each in an amount of 1 part to alleviate polymer degradation. After the torque reached equilibrium, 60 parts of alkane oil (Southco paraffin oil 2280), 2 parts of modified nano-titanium dioxide loaded with silver, 5 parts of modified nano-titanium-doped zinc oxide, 35 parts of modified nano-silicon dioxide, and 5 parts of EPDM grafted maleic anhydride (EPDM-g-MAH) were added and mixed for 20 minutes. After extrusion by a twin-screw extruder, it was formed into strips through a porous die, and then cooled and pelletized to obtain EPDM masterbatch particles with a length of 2~6 mm, which were crushed by a crusher and sieved by a sieve.

[0110] (4) Twin-screw extrusion granulation of inner layer material:

[0111] Main engine speed: 500rpm

[0112] The temperature settings are as follows (unit: °C, the same below):

[0113] Table 1 Temperature of each zone in Example 1

[0114]

[0115] Feed the materials in sequence and use the screw for metering. Add 100 parts of PP, 20 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil and 2 parts of high molecular weight silicone (number average molecular weight of 900,000 to 1,000,000, purchased from Chengdu Silike Technology Co., Ltd., model LYSI-406, the same below) to the first feeding port.

[0116] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0117] Through water cooling and pelletizing, the inner layer material with a particle size of 2~6mm is prepared.

[0118] (5) Double-layer co-extrusion of polypropylene pipes

[0119] The inner layer material and the outer layer material are extruded by a 70-33 / 60-36 dual-host polyolefin extruder to prepare a double-layer pipe. The outer layer material is prepared by step (1) to prepare polypropylene β-crystal modified pellets, and the inner layer material is prepared by step (4) to prepare functional modified masterbatch. The extrusion temperature is controlled at 200°C and the torque is 70%.

[0120] The outer diameter is 25.1±0.1mm, the outer wall thickness is 3.5~4.0mm, and the inner layer thickness is 0.5±0.1mm. The outer layer thickness of the pipe meets the wall thickness requirements of GB / T 18742.2-2018 S3.2.

[0121] Example 2

[0122] Compared with Example 1, the only difference is the following conditions, and other conditions refer to Example 1:

[0123] Step (4) Add materials in order and use a screw to measure. Add 100 parts of PP, 30 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil, and 2 parts of high molecular weight silicone (number average molecular weight of 900,000 to 1,000,000, purchased from Chengdu Silike Technology Co., Ltd., model LYSI-406, the same below) to the first feeding port.

[0124] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0125] Example 3

[0126] Compared with Example 1, the only difference is the following conditions, and other conditions refer to Example 1:

[0127] Step (4) Add materials in order and use a screw to measure. Add 100 parts of PP, 40 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil, and 2 parts of high molecular weight silicone (number average molecular weight of 900,000 to 1,000,000, purchased from Chengdu Silike Technology Co., Ltd., model LYSI-406, the same below) to the first feeding port.

[0128] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0129] Example 4

[0130] Compared with Example 1, the only difference is the following conditions, and other conditions refer to Example 1:

[0131] Step (4) Twin-screw extrusion granulation of inner layer material:

[0132] Main engine speed: 200rpm

[0133] The temperature settings are as follows:

[0134] Table 2 Temperature of each zone in Example 4

[0135]

[0136] Feed the materials in sequence and use the screw for metering. At the first feeding port, add 100 parts of PP, 20 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil, and 2 parts of high molecular weight silicone (number average molecular weight of 900,000 to 1,000,000, purchased from Chengdu Silike Technology Co., Ltd., model LYSI-406, the same below).

[0137] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0138] The inner layer functional material is prepared by water cooling and pelletizing.

[0139] Example 5

[0140] Compared with Example 1, the only difference is that no β-crystal nucleating agent is added in step (1), that is, pipeline-grade unmodified polypropylene is used.

[0141] Example 6

[0142] Compared with Example 1, the only difference is the following conditions, and other conditions refer to Example 1:

[0143] Step (4) Twin-screw extrusion granulation of inner layer material:

[0144] Main engine speed: 500rpm

[0145] The temperature settings are as follows:

[0146] Table 3 Temperature of each zone in Example 6

[0147]

[0148] Feed the materials in sequence and use the screw for metering. Add 100 parts of PP, 20 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil and 2 parts of high molecular weight silicone into the first feeding port.

[0149] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0150] The inner layer functional material is prepared by water cooling and pelletizing.

[0151] Example 7

[0152] Compared with Example 1, the only difference is the following conditions, and other conditions refer to Example 1:

[0153] Step (4) Twin-screw extrusion granulation of inner layer material:

[0154] Main engine speed: 500rpm;

[0155] The temperature settings are as follows:

[0156] Table 4 Temperature of each zone in Example 7

[0157]

[0158] The materials were added in sequence and measured by a screw. 100 parts of PP, 20 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil, and 0 parts of high molecular weight silicone were added to the first feeding port (no high molecular weight silicone was added in Example 7).

[0159] The second feeding port uses a screw to measure and add 0.2 parts of N-cyclohexyl-2-benzothiazole sulfonamide (CZ), 0.2 parts of stearic acid (SA), 0.6 parts of 2,4-di-tert-butyl peroxide isopropylbenzene (BIBP), and 0.5 parts of triallyl isocyanurate (TAIC).

[0160] The inner layer functional material is prepared by water cooling and pelletizing.

[0161] Example 8

[0162] The only difference from Example 1 is that no vulcanization is performed. The specific steps are as follows:

[0163] (1) Same as step (1) of Example 1.

[0164] (2) Same as step (2) of Example 1.

[0165] (3) Same as step (3) of Example 1.

[0166] (4) The main difference from step (4) of Example 1 is that no cross-linking aid is added.

[0167] Inner layer material twin screw extrusion granulation:

[0168] Main engine speed: 500rpm;

[0169] The temperature setting of each zone refers to Example 1.

[0170] Feed the materials in sequence and use the screw for metering. Add 100 parts of PP, 20 parts of EPDM masterbatch, 3 parts of PP-g-MAH, 5 parts of alkane oil and 2 parts of high molecular weight silicone into the first feeding port.

[0171] The inner layer functional material is prepared by water cooling and pelletizing.

[0172] (5) Same as step (5) in Example 1.

[0173] Example 9

[0174] The only difference from Example 1 is that step (2) is not performed, that is, the silver-loaded nano-titanium dioxide, titanium-doped nano-zinc oxide, and nano-silicon dioxide are not modified with silane.

[0175] Example 10

[0176] The only difference from Example 1 is that the type of crosslinking aid in step (4) is different, specifically as follows: the second feeding port is metered by a screw to feed 0.2 parts of stearic acid (SA), 0.15 parts of tetramethylthiuram disulfide (TMTD), 0.1 parts of 2-mercaptobenzothiazole (M), and 0.3 parts of sublimated sulfur (S).

[0177] Test Example 1

[0178] The performance of the double-layer pipe was tested in each embodiment, and the results are shown in Table 5.

[0179] Performance testing method:

[0180] Yield strength test: GB / T 8804.3-2003, punch dumbbell-shaped specimens from the tube, tensile rate 50mm / min;

[0181] Simply supported beam notched impact (-20℃) ISO 179: Cut 80mm*10mm specimens from the length of the pipe and make A-type notch for testing.

[0182] Contact angle test GB / T 24368-2009;

[0183] Antibacterial test ISO 22196 2007;

[0184] Scrub resistance: First, mold the inner pipe material to make a 400mm*150mm flat plate, fix the flat plate on the scrub resistance tester, add 2ml of tap water, fix the brush on the scrub resistance tester, the total weight of the brush and the fixture is 450±10g, and reciprocate at a frequency of 35 times per minute for 24 hours. After scrubbing, conduct contact angle and antibacterial tests.

[0185] Table 5 Performance test results of double-layer pipes obtained in various embodiments

[0186] project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Yield strength MPa 23 22.2 21.6 21.8 23.8 21.3 23.5 19.8 20.4 24 <![CDATA[Notched Izod impact strength (-20 °C) KJ / m 2 > 5.2 6 6.5 4.9 4 4.8 5.0 5.0 4.3 4.7 Contact angle° 126 129 125 121 127 119 113 115 112 127 Anti-glucose bacterium activity rate% 99.8 99.8 99.9 96.6 98.4 95.6 99.5 97.9 95.7 99.6% Contact angle after scrubbing resistance° 120 / / / / / / 102 107 / Activity rate against golden glucose bacteria after scrubbing % 98.2% / / / / / / 93.6 93.2 /

[0187] Comparing Example 1 and Example 4, it can be seen that when the main engine speed is reduced from 500RPM to 200RPM, the shear weakening affects the phase conversion process, resulting in a decrease in yield strength and simply supported beam impact strength. The inability to fully form fine rubber particles affects the construction of the hydrophobic structure and the dispersion of the antibacterial particles, resulting in a decrease in the contact angle and the activity rate against golden glucose bacteria.

[0188] Comparing Example 1 with Example 2 and Example 3, it can be seen that increasing the amount of EPDM masterbatch can improve the notched impact strength, but the yield strength is significantly reduced. Since the amount of crosslinking agent is not increased accordingly, the degree of vulcanization is insufficient, and the rubber particles cannot be well formed and dispersed, resulting in the inability to form an optimal hydrophobic surface. In Example 3, the contact angle is reduced compared with Example 1.

[0189] Comparing Example 1 with Example 5, without adding the β-nucleating agent, the simply supported beam impact strength is significantly reduced.

[0190] Comparing Example 1 with Example 6, increasing the extrusion temperature will accelerate the vulcanization reaction when the vulcanizing agent is not fully dispersed, thereby affecting the uniformity of the rubber particle size, resulting in a decrease in yield strength, a decrease in simply supported beam notched impact strength, a decrease in contact angle, and a decrease in antibacterial properties.

[0191] Comparing Example 1 with Example 7, not adding high molecular weight silicone affects the hydrophobic surface composition and reduces the hydrophobic angle.

[0192] Comparing Example 1 with Example 8, vulcanization without adding a vulcanizing agent cannot form uniform rubber particles, resulting in a decrease in yield strength. After scrubbing, the contact angle and antibacterial property are significantly reduced.

[0193] Comparing Example 1 with Example 9, the inorganic particles were not modified by the silane coupling agent and agglomerated, which significantly reduced the contact angle. After scrubbing, the contact angle and antibacterial property did not decrease significantly.

[0194] Comparing Example 1 with Example 10, the yield strength of the sulfur vulcanization system is higher than that of the BIBP vulcanization system, and the simply supported beam impact strength is slightly reduced.

[0195] Test Example 2

[0196] The DSC graph of the outer layer pipe prepared in Test Example 1 is as follows: Figure 2 shown.

[0197] It can be seen that two melting peaks can be clearly seen through the DSC graph, among which the β-crystal melting peak is more significant than the α-crystal melting peak, indicating that the β-nucleating agent has a significant crystal transformation effect.

[0198] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a polypropylene pipe, characterized in that: The method comprises preparing an outer layer material and an inner layer material respectively by an extrusion granulation process, and then performing double-layer extrusion using the outer layer material and the inner layer material; Wherein, the preparation process of the inner layer material includes: The nano-titanium dioxide loaded with silver, the nano-titanium-doped zinc oxide and the nano-silicon dioxide are modified by using a silane coupling agent to obtain modified nano-titanium dioxide loaded with silver, modified nano-titanium-doped zinc oxide and modified nano-silicon dioxide respectively; The modified nano titanium dioxide loaded with silver, the modified nano titanium-doped zinc oxide, the modified nano silicon dioxide, EPDM grafted maleic anhydride and EPDM are mixed and extruded to obtain an EPDM masterbatch; The inner layer material is obtained by blending and extruding polypropylene, the EPDM masterbatch, alkane oil, high molecular weight silicone, polypropylene grafted maleic anhydride and a crosslinking aid; wherein the number average molecular weight of the high molecular weight silicone is 500,000-1.5 million, and the crosslinking aid includes N-cyclohexyl-2-benzothiazole sulfonamide, stearic acid, 2,4-di-tert-butyl peroxide isopropylbenzene and triallyl isocyanurate; When the inner layer material is prepared from the EPDM masterbatch, a twin-screw extrusion process is adopted, and the twin-screw extruder is provided with an end feeding port and a middle feeding port, and the end feeding port is arranged close to the inlet end of the twin-screw extruder; the polypropylene, the EPDM masterbatch, the alkane oil, the high molecular weight silicone and the polypropylene grafted maleic anhydride are added from the end feeding port, and the cross-linking aid is added from the middle feeding port; The temperature between the inlet end of the twin-screw extruder and the middle feeding port is controlled to be 100° C.-180° C., and the temperature from the middle feeding port to the end of the twin-screw extruder is controlled to be 160° C.-220° C. After extrusion, the extruder is formed into strips through a porous die, and then crushed by a crusher and sieved by a screen to prepare 2mm-6mm EPDM masterbatch particles; The twin-screw extruder comprises a first heating zone to a tenth heating zone arranged in sequence, the temperature of the first heating zone to the fifth heating zone is 100°C-180°C, and the rotation speed of the twin-screw extruder is 300rpm-600rpm; the end feed port is located in the first heating zone, the middle feed port is located in the fifth heating zone to the seventh heating zone, the temperature of the sixth heating zone to the seventh heating zone is 160°C-180°C, and the temperature of the eighth heating zone to the tenth heating zone is 180°C-220°C; The preparation process of the outer layer material comprises: mixing polypropylene particles and a β-nucleating agent, and then extruding and granulating; The raw materials for preparing the outer layer material include, by weight, 100 parts of polypropylene particles and 0.05-1.00 parts of a beta nucleating agent; the beta nucleating agent is selected from at least one of carboxylates, rare earth compounds and amide compounds.

2. The preparation method according to claim 1, characterized in that: Calculated by weight, the raw materials for preparing the inner layer material include: 100 parts of polypropylene, 20-50 parts of EPDM masterbatch, 4-10 parts of alkane oil, 1-5 parts of high molecular weight silicone, and 1-5 parts of polypropylene grafted maleic anhydride; the cross-linking aids include 0.1-0.5 parts of N-cyclohexyl-2-benzothiazole sulfonamide, 0.1-0.5 parts of stearic acid, 0.2-1 parts of 2,4-di-tert-butyl peroxide isopropylbenzene and 0.2-1 parts of triallyl isocyanurate.

3. The preparation method according to claim 1, characterized in that: The raw materials for preparing the EPDM masterbatch include, by weight: 100 parts of EPDM, 0.5-5.0 parts of modified nano titanium dioxide loaded with silver, 0.5-5 parts of modified nano titanium-doped zinc oxide, 10-40 parts of modified nano silicon dioxide, 30-80 parts of alkane oil, 0.5-10 parts of EPDM grafted maleic anhydride and 1-4 parts of antioxidant.

4. The preparation method according to claim 3, characterized in that: The antioxidant is selected from at least one of the antioxidant 1010 and the antioxidant 1076.

5. The preparation method according to claim 4, characterized in that: The antioxidants include 0.5-2 parts of antioxidant 1010 and 0.5-2 parts of antioxidant 1076.

6. The preparation method according to claim 3, characterized in that: The particle sizes of the modified nano titanium dioxide loaded with silver, the modified nano titanium-doped zinc oxide and the modified nano silicon dioxide are less than or equal to 100 nm.

7. The preparation method according to claim 3, characterized in that: The process of preparing the EPDM masterbatch includes: mixing the raw materials for preparing the EPDM masterbatch, double-roller extrusion and cooling to form sheets, and then crushing by a crusher and screening by a screen to prepare EPDM masterbatch particles with a particle size of 2mm-6mm.

8. The preparation method according to claim 7, characterized in that: The process of mixing the raw materials for preparing the EPDM masterbatch includes: mixing for 10 minutes to 30 minutes at 150° C. to 170° C. and 30 rpm to 60 rpm using an internal mixer.

9. The preparation method according to claim 1, characterized in that: The process of preparing the modified nano titanium dioxide loaded with silver, the modified nano titanium-doped zinc oxide and the modified nano silicon dioxide comprises: The nano-titanium dioxide loaded with silver, the nano-titanium-doped zinc oxide and the nano-silicon dioxide are respectively soaked in the silane coupling agent solution for 10 minutes to 60 minutes, and then dried.

10. The preparation method according to claim 9, characterized in that: The concentration of the silane coupling agent solution is 0.5%-5%.

11. The preparation method according to claim 10, characterized in that: The solvents used in preparing the silane coupling agent solution are water and ethanol, and the volume ratio of water to ethanol is (1.5-3.0):

1.

12. The preparation method according to claim 1, characterized in that: During the double-layer extrusion process using the outer layer material and the inner layer material, the extrusion temperature is controlled to be 160° C.-220° C. and the torque is controlled to be 60%-85%.

13. The preparation method according to claim 12, characterized in that: The outer diameter of the polypropylene pipe is 20mm-30mm, the outer wall thickness is 3.5mm-5.0mm, and the inner layer thickness is 0.4mm-0.6mm.

14. A polypropylene pipe, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 13.