A method for smelting tungsten without ammonia by ion exchange

Through dynamic adsorption and acid precipitation purification steps, combined with ammonia-free desorption, the problem of ammonia nitrogen pollution in tungsten smelting is solved, the preparation of high-purity tungsten oxide is realized, the treatment cost and environmental impact are reduced, and the green development of tungsten smelting is supported.

CN118703801BActive Publication Date: 2024-11-22GANNAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210204.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The introduction of ammonia nitrogen pollutants during tungsten smelting has led to challenges in environmental protection and sustainable development, and the existing governance methods have high costs and no pollution has been solved from the source.

Method used

Using dynamic adsorption, ammonia-free desorption and acid precipitation purification steps, 201×7U strong alkaline anion exchange resin and inorganic acid are used to prepare high-purity tungstenic acid through dynamic adsorption and acid precipitation purification, and finally obtain tungsten oxide powder through oxidation and roasting to avoid The occurrence of ammonia nitrogen pollution.

Benefits of technology

The ammonia-free process has been realized, which reduces the difficulty and cost of controlling ammonia nitrogen pollutants, supports the green transformation of the tungsten smelting industry, and improves the sustainability of the production process through resource recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118703801B_ABST
    Figure CN118703801B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of tungsten smelting, and provides a method for tungsten ion exchange ammonia-free smelting, comprising the following steps: S1, dynamic adsorption; S2, ammonia-free desorption; S3, acid precipitation purification; S4, oxidative roasting. Through dynamic adsorption, WO4 in a low-concentration sodium tungstate solution is converted into tungstate WO4 by using 201×7U strong alkaline anion exchange resin. 2‑ The impurity elements are removed by transferring from the solution to the solid resin, and then sodium chloride and sodium hydroxide are used as ammonia-free desorbents to obtain a high-concentration sodium tungstate solution. Relying on inorganic acid precipitation purification and washing, high-purity tungstic acid is prepared, and finally tungsten oxide powder is prepared by oxidative roasting. This method does not require the preparation of tungsten oxide through the intermediate ATP, realizes an ammonia-free production process, fundamentally eliminates the generation of ammonia nitrogen pollutants, effectively avoids the diffusion of ammonia nitrogen in the smelting process, significantly reduces the difficulty and cost of treating ammonia nitrogen pollutants, and provides strong support for the green transformation of the tungsten smelting industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tungsten smelting, and in particular to an ion exchange ammonia-free smelting method of tungsten. Background Art

[0002] APT (ammonium paratungstate) is a key intermediate product in the tungsten smelting process. Its production methods are diverse, mainly including the following routes: First, ion exchange is carried out after decomposition by sodium hydroxide, followed by molybdenum removal with copper salt, and finally the product is obtained by evaporation and crystallization. Another method is to purify and remove impurities after decomposition of sodium carbonate, and then remove molybdenum by sulfidic acid precipitation method, and evaporation and crystallization is also the final step. The third route involves the decomposition of sodium carbonate, followed by alkaline extraction, combined with copper salt or resin adsorption technology to remove molybdenum, and finally ends with evaporation and crystallization. In addition, there is acid decomposition, alkaline dissolution, and then ion exchange, acid extraction or alkaline extraction to remove impurities, and finally APT is obtained by evaporation and crystallization. However, these preparation processes inevitably require the introduction of ammonia water or ammonium salts, resulting in the generation of ammonia nitrogen pollutants. Especially in wastewater and waste gas, the presence of ammonia increases the difficulty of resource utilization and brings higher governance costs. These problems seriously restrict the development of the tungsten smelting industry in a more environmentally friendly and sustainable direction.

[0003] In order to solve the problem of ammonia nitrogen pollution control in tungsten smelting, researchers have developed a variety of processes and achieved significant progress, but there are still some shortcomings. Among them, the wastewater distillation deammoniation method first adjusts the pH value of ammonia-containing wastewater to ≥13 using sodium hydroxide or calcium oxide, calcium hydroxide, etc., and then uses steam heating to convert the ammonia in the wastewater into gaseous ammonia first, so as to achieve separation from the wastewater, and finally converts the ammonia into ammonia water through condensation to achieve the recycling of ammonia. This process has obvious advantages when treating high-concentration ammonia nitrogen wastewater, but has the disadvantages of high energy consumption and large alkali consumption when treating low-concentration ammonia nitrogen wastewater. The MAP precipitation method uses phosphates (trisodium phosphate, sodium hydrogen phosphate, etc.) and magnesium salts (magnesium chloride, magnesium sulfate, etc.) to form ammonium phosphate magnesium salt precipitation with ammonia in the wastewater to achieve ammonia removal. This process introduces phosphates, which not only removes ammonia, but also brings new pollution problems. In addition, the consumption of ammonia precipitation agent is large, which makes the cost high. The sodium hypochlorite / sodium perchlorate / calcium perchlorate oxidation method is suitable for treating low-concentration ammonia nitrogen wastewater, but it will introduce chlorate ions, making the on-site environment poor and prone to chlorine poisoning. The ammonia-containing waste gas condensation-absorption method uses a heat exchanger to condense the ammonia-containing waste gas first to prepare low-concentration ammonia water (low-concentration ammonia water can be returned for distillation to prepare high-concentration ammonia water), and then uses water elution-acid elution to remove ammonia nitrogen from the waste gas. This process has a good deammoniation effect, but there are problems such as large amount of elution liquid and high alkali consumption.

[0004] In summary, tungsten smelting introduces ammonium salts or ammonia water through the preparation of APT and then tungsten oxide, which causes the problem of ammonia nitrogen pollutant diffusion in the smelting process. Although significant control effects have been achieved through continuous technical breakthroughs, there are still problems such as high control costs and failure to solve the risk of ammonia nitrogen pollutant escape from the source. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide an ion exchange ammonia-free smelting method for tungsten, comprising the following steps:

[0006] S1. Dynamic adsorption: Place 201×7U strong alkaline anion exchange resin in a simulated exchange column, soak the 201×7U strong alkaline anion exchange resin in pure water for 24 hours, then soak it in 0.5mol / L hydrochloric acid solution for 24 hours, wash it with clean water after soaking, then place a low concentration sodium tungstate solution in the simulated exchange column for dynamic adsorption, and finally wash it with pure water to obtain washing water I. After washing, the adsorption-saturated 201×7U strong alkaline anion exchange resin enters the next step, and washing water I is collected and processed;

[0007] S2, ammonia-free desorption: the saturated 201×7U strong alkaline anion exchange resin in step S1 is dynamically desorbed, the desorbent is a mixed solution of sodium chloride and sodium hydroxide, the desorbed liquid is collected to obtain a high-concentration sodium tungstate solution, and enters the next step. The desorbed 201×7U strong alkaline anion exchange resin is washed with pure water and enters the next dynamic adsorption cycle for recycling to obtain washing water II, which is collected and processed;

[0008] S3, acid precipitation purification: the high concentration sodium tungstate solution obtained in step S2 is neutralized and purified by acid precipitation with inorganic acid. After the neutralization and purification of the acid precipitation, it is filtered and washed to obtain filtrate I and filter residue I. The filtrate I is collected and processed. The filter residue I is stirred and washed three times to obtain filter residue IV. The filter residue IV is dissolved at room temperature with hydrogen peroxide. After the dissolution is completed, the dissolved solution is heated to 60°C to 80°C, and then sulfuric acid is added to stir the acid precipitation. The stirring speed is 40r / min to 60r / min. The end point of the stirring acid precipitation is that the sulfuric acid concentration in the solution is 1mol / L to 2mol / L. After the stirring acid precipitation is completed, it is filtered and washed with hot pure water. After washing, tungstic acid and washing water III are obtained. The tungstic acid is dried and enters the next link. The acid precipitation mother liquor and washing water III after the acid precipitation purification are collected and processed;

[0009] S4, oxidative calcination: oxidative calcination is performed on the tungstic acid obtained in step S3, the calcination temperature is 650° C. to 750° C., the calcination time is 2 h to 5 h, and tungsten oxide powder is obtained after the calcination.

[0010] Furthermore, in step S1, the simulated exchange column is made of organic glass and has a size of φ4 cm×60 cm.

[0011] Furthermore, in step S1, when the 201×7U strong alkaline anion exchange resin is soaked in pure water, the pure water level exceeds the resin layer by 2 cm, and the soaked 201×7U strong alkaline anion exchange resin is washed with clean water until the pH value of the simulated exchange column outlet water is 5-7, and the end point of dynamic adsorption is that the WO3 concentration in the simulated exchange column outlet water is ≥0.5 g / L.

[0012] Furthermore, in step S2, the concentration of sodium chloride in the desorbent is 180 g / L to 220 g / L, and the concentration of sodium hydroxide is 0.5 g / L to 5 g / L.

[0013] Further, in step S2, the desorption liquid is collected three times according to the order of the desorption liquid outflow. The first time, the desorption liquid equivalent to 18% to 22% of the resin volume that flows out first is collected. At this time, the concentration of sodium tungstate in the desorption liquid is low. After collection, it returns to the dynamic adsorption in step S1. The second time, the desorption liquid equivalent to 59% to 61% of the resin volume that flows out thereafter is collected. At this time, the collected desorption liquid is a high-concentration sodium tungstate solution and enters the next link. The third time, the desorption liquid equivalent to 19% to 21% of the resin volume that flows out last is collected. At this time, the concentration of sodium tungstate in the desorption liquid is also low. After collection, it is used to prepare the desorbent of the next cycle.

[0014] Furthermore, during the neutralization acid precipitation purification process in step S3, stirring is performed at room temperature for 2 h to 3 h, and the neutralization acid precipitation purification endpoint is when the inorganic acid concentration in the solution is 2 mol / L to 4 mol / L.

[0015] Further, in step S3, the process of stirring and washing the filter residue I three times is as follows: in the first stirring and washing, inorganic acid is used as a detergent, the acid concentration is 1mol / L~2mol / L, the washing liquid-solid mass ratio is 1:1, the stirring and washing time is 1h, and after the stirring and washing is completed, filtration is performed to obtain filtrate II and filter residue II, filtrate II is collected and processed, and filter residue II is stirred and washed for the second time. Inorganic acid is still used as a detergent for this stirring and washing, the acid concentration is 1mol / L~2mol / L, the washing liquid-solid mass ratio is 1:1, and the stirring and washing time is 1h. After the stirring and washing is completed, filtration is performed to obtain filtrate III and filter residue III, filtrate III is collected and processed, and filter residue III is stirred and washed for the third time. Hot pure water is used as a detergent for this stirring and washing, the washing liquid-solid mass ratio is 3:1~5:1, stirring and washing for 1h, and after the stirring and washing is completed, filtration is performed to obtain filtrate IV and filter residue IV, filtrate IV is collected and processed, and the stirring speed of the three times is 40r / min~60r / min.

[0016] Furthermore, in step S3, when the filter residue IV is dissolved at room temperature with hydrogen peroxide, the liquid-solid mass ratio is 1:1 to 3:1, and the dissolution time is 1h to 3h.

[0017] Furthermore, in step S3, the inorganic acid is hydrochloric acid, sulfuric acid or nitric acid.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Through dynamic adsorption, 201×7U strong alkaline anion exchange resin is used to convert WO4 2- The impurity elements are removed by transferring from the solution to the solid resin, and then sodium chloride and sodium hydroxide are used as ammonia-free desorbents to obtain a high-concentration sodium tungstate solution. Relying on inorganic acid precipitation purification and washing, high-purity tungstic acid is prepared, and finally tungsten oxide powder is prepared by oxidative roasting. This method uses an ammonia-free process and does not need to prepare the intermediate APT to obtain tungsten oxide. It fundamentally eliminates the generation of ammonia nitrogen pollutants, effectively avoids the diffusion of ammonia nitrogen in the smelting process, and significantly reduces the difficulty and cost of controlling ammonia nitrogen pollutants, providing strong support for the green transformation of the tungsten smelting industry.

[0020] 2. In the ammonia-free desorption process, the desorption liquid is collected three times. The desorption liquid with high concentration of sodium tungstate collected in the second time is used to enter the next process, while the desorption liquid with low sodium tungstate concentration collected in the first and third times is used to return to the previous step and used to prepare the desorbent for the next cycle. This method significantly reduces the consumption of raw materials and production costs. This resource recycling strategy not only improves the sustainability of the production process, but also reduces the impact on the environment. At the same time, the acid precipitation mother liquor after the acid precipitation purification stage can be adjusted to pH by sodium hydroxide, and can also be used to prepare the desorbent for the next cycle, realizing the design concept of green chemistry and circular economy as a whole. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation of the present invention or the technical solution in the prior art, the drawings required for describing the specific implementation or the prior art will be briefly introduced below. Obviously, the drawings described below are only one implementation of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is a flow chart of the ion exchange ammonia-free smelting method of tungsten according to an embodiment of the present invention. DETAILED DESCRIPTION

[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the technical scheme in the specific implementation mode of the present invention is clearly and completely described below to further illustrate the present invention. Obviously, the specific implementation mode described is only a part of the implementation mode of the present invention, rather than all styles.

[0024] Embodiment 1: Figure 1 As shown, the ion exchange ammonia-free smelting method of tungsten in this embodiment includes the following steps:

[0025] S1. Dynamic adsorption: Measure 280 ml of 201×7U strong alkaline anion exchange resin and load it into a simulated exchange column (the simulated exchange column is made of organic glass, with a size of φ4cm×60cm and a resin layer height of 40cm). Soak the resin in pure water for 24 hours. During the soaking, the liquid level exceeds the resin layer by 2cm. Then soak it in 0.5mol / L hydrochloric acid solution for 24 hours. After soaking, wash it with 2000ml of clean water until the pH value of the water out of the exchange column is 5.0. The prepared low-concentration sodium tungstate solution (WO3 21.31g / L, NaOH 5.76g / L) was pumped into the simulated exchange column by a peristaltic pump for dynamic adsorption. The flow rate was controlled at 3ml / min. When the WO3 concentration of the simulated exchange column was ≥0.5g / L, the adsorption was stopped. At this time, the volume of the low-concentration sodium tungstate solution pumped into the simulated exchange column was 2200ml, and the dynamic adsorption was completed. Then, the washing process was entered, and 2000ml of pure water was used for washing. The washing water flow rate was 5ml / min. After the washing was completed, washing water I was obtained. After the dynamic adsorption effluent and washing water I were mixed, the volume was measured to be 4125ml. The WO3 concentration was measured by sampling to be 0.11g / L, and the total adsorbed WO3 was 46.43g, and the adsorption rate was 99.04%. The adsorption-saturated 201×7U strong alkaline anion exchange resin entered the next link.

[0026] S2, ammonia-free desorption: the saturated 201×7U strong basic anion exchange resin in step S1 is subjected to dynamic desorption, the desorbent is a mixed solution of sodium chloride and sodium hydroxide, wherein the concentration of sodium chloride is 195.71 g / L, the concentration of sodium hydroxide is 4.5 g / L, the flow rate of the desorbent pumped in is controlled to be 2 ml / min, the total volume of the desorbent added is 180 ml, the desorbent is collected three times in the order of the desorbent discharge, the first collection volume is 50 ml, the WO3 concentration is 3.20 g / L, the WO3 concentration is low, and the collected desorbent is returned to the reactor. Dynamic adsorption, the second collection volume is 170ml, WO3 concentration is 245.13g / L, WO3 concentration is high, it is a high concentration of sodium tungstate solution, and enters the acid precipitation purification link. The third collection volume is 50ml, WO3 concentration is 3.45g / L, WO3 concentration is relatively low, and it is used to prepare the desorbent for the next cycle after collection. The total desorption rate is 90.47%. The 201×7U strong alkaline anion exchange resin after desorption is washed with pure water and enters the next dynamic adsorption cycle for recycling to obtain washing water II, which is collected and treated.

[0027] S3, acid precipitation purification: The high-concentration sodium tungstate solution (second-stage desorption liquid) obtained in step S2 is neutralized and purified by acid precipitation with hydrochloric acid. The end point of acid precipitation with hydrochloric acid is 4 mol / L, and stirring is carried out at room temperature for 2 hours. After the acid precipitation is completed, filtration and washing are carried out to obtain filtrate I and filter residue I. The acid precipitation filtrate I is collected and processed, and the filter residue I is stirred and washed three times. In the first washing, hydrochloric acid solution is used as a detergent, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate II and filter residue II. Filtrate II is collected and processed, and filter residue II is washed for the second time. Hydrochloric acid is used as a detergent for this washing, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate III and filter residue III. Filtrate III is collected and processed, and filter residue III is washed for the third time. This washing is washed with hot pure water, and the washing liquid-to-solid mass ratio is 1:1. The ratio is 5:1, stirring and washing for 1h, filtering after washing to obtain filtrate IV and residue IV, filtrate IV is collected and processed, residue IV is dissolved with hydrogen peroxide at room temperature, the liquid-to-solid mass ratio is 3:1, the dissolution time is 3h, after the dissolution is completed, the dissolved solution is heated to 80°C, and then sulfuric acid is added and stirred for acid precipitation. The end point of acid precipitation is that the concentration of sulfuric acid in the solution reaches 2mol / L. After the acid precipitation is completed, filtering is carried out, and then washing with hot pure water. After washing, tungstic acid and washing water III are obtained, and then the tungstic acid is dried and enters the next link. The acid precipitation mother liquor and washing water III after the acid precipitation purification are collected and processed.

[0028] S4, oxidative roasting: the tungstic acid obtained in step S3 is oxidatively roasted at a temperature of 750°C for 5 hours to obtain tungsten oxide powder. The tungsten oxide powder is sampled and then analyzed by direct reading spectrometer for the content of each impurity element in the tungsten oxide powder. The results are as follows: Na 8.0 ppm, K 7.0 ppm, Mg 0.62 ppm, Al 4.47 ppm, Si 0.58 ppm, Ca 5.12 ppm, Ti 4.26 ppm, V 2.42 ppm, Mn 0.27 ppm, Fe 3.69 ppm, Co 0.19 ppm, Ni0.93 ppm, Cu 1.0 ppm, As 3.85 ppm, Mo 6.0 ppm, Cd 1.07 ppm, Cr 5.79 ppm, Sn 2.1ppm, Sb 1.90 ppm, Pb 0.2 ppm, Bi 0.47 ppm, P 4.0 ppm, and the total content of impurity elements is less than 50 ppm, which means that the quality of the tungsten oxide powder obtained in this embodiment exceeds the quality requirements of the national standard.

[0029] Embodiment 2: The process of the ion exchange ammonia-free smelting method of tungsten in this embodiment is the same as that of embodiment 1, and the specific process parameters are:

[0030] S1. Dynamic adsorption: Measure 280 ml of 201×7U strong alkaline anion exchange resin and load it into a simulated exchange column (the simulated exchange column is made of organic glass, with a size of φ4cm×60cm and a resin layer height of 40cm). Soak the resin in pure water for 24 hours. During the soaking, the liquid level exceeds the resin layer by 2cm. Then soak it in 0.5mol / L hydrochloric acid solution for 24 hours. After soaking, wash it with 2000ml of clean water until the pH value of the water out of the exchange column is 5.0. The prepared low-concentration sodium tungstate solution (WO3 15.24g / L, NaOH 5.06g / L) was pumped into the simulated exchange column by a peristaltic pump for dynamic adsorption. The flow rate was controlled at 3ml / min. When the WO3 concentration of the simulated exchange column was ≥0.5g / L, the adsorption was stopped. At this time, the volume of the low-concentration sodium tungstate solution pumped into the simulated exchange column was 3000ml, and the dynamic adsorption was completed. Then, the washing process was entered, and 2000ml of pure water was used for washing. The washing water flow rate was 5ml / min. After the washing was completed, washing water I was obtained. After the dynamic adsorption effluent and washing water I were mixed, the volume was measured to be 4910ml. The WO3 concentration was measured by sampling to be 0.10g / L, and the total adsorbed WO3 was 45.23g, and the adsorption rate was 98.93%. The adsorption-saturated 201×7U strong alkaline anion exchange resin entered the next link.

[0031] S2, ammonia-free desorption: the saturated 201×7U strong basic anion exchange resin in step S1 is subjected to dynamic desorption, the desorbent is a mixed solution of sodium chloride and sodium hydroxide, wherein the concentration of sodium chloride is 211.32 g / L, the concentration of sodium hydroxide is 5.0 g / L, the flow rate of the desorbent pumped in is controlled to be 2 ml / min, the total volume of the desorbent is 180 ml, the desorbent is collected three times in the order of the desorbent discharge, the first collection volume is 50 ml, the WO3 concentration is 2.30 g / L, the WO3 concentration is low, and the desorbent is returned to the dynamic desorption system after collection. The second collection volume is 170ml, the WO3 concentration is 262.11g / L, the WO3 concentration is high, it is a high concentration sodium tungstate solution, and it enters the acid precipitation purification link. The third collection volume is 50ml, the WO3 concentration is 2.87g / L, and the WO3 concentration is relatively low. After collection, it is used to prepare the desorbent for the next cycle. The total desorption rate is 99.09%. The 201×7U strong alkaline anion exchange resin after desorption is washed with pure water and enters the next dynamic adsorption cycle for recycling to obtain washing water II, which is collected and treated.

[0032] S3, acid precipitation purification: The high-concentration sodium tungstate solution (second-stage desorption liquid) obtained in step S2 is neutralized with hydrochloric acid for acid precipitation purification. Nitric acid is added to the acid precipitation end point to an acid concentration of 3 mol / L. Stir at room temperature for 3 hours. After the acid precipitation is completed, filter and wash to obtain filtrate I and filter residue I. The acid precipitation filtrate I is collected and processed, and the filter residue I is stirred and washed three times. In the first washing, nitric acid solution is used as a detergent, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate II and filter residue II. Filtrate II is collected and processed, and filter residue II is washed for the second time. Nitric acid is used as a detergent for this washing, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate III and filter residue III. Filtrate III is collected and processed, and filter residue III is washed for the third time. This washing is washed with hot pure water, and the washing liquid-to-solid mass ratio is 1:1. The ratio is 4:1, stirring and washing for 1h, filtering after washing to obtain filtrate IV and filter residue IV, filtrate IV is collected and processed, filter residue IV is dissolved with hydrogen peroxide at room temperature, the liquid-to-solid mass ratio is 4:1, the dissolution time is 3h, after the dissolution is completed, the dissolved solution is heated to 70°C, and then sulfuric acid is added and stirred for acid precipitation. The end point of acid precipitation is that the concentration of sulfuric acid in the solution reaches 2mol / L. After the acid precipitation is completed, it is filtered and washed with hot pure water. After washing, tungstic acid and washing water III are obtained, and then the tungstic acid is dried and enters the next link. The acid precipitation mother liquor and washing water III after the acid precipitation purification are collected and processed.

[0033] S4, oxidative calcination: oxidative calcination of the tungstic acid obtained in step S3, the calcination temperature is 700 ° C, the calcination time is 5h, and tungsten oxide powder is obtained after calcination. The tungsten oxide powder is sampled and then analyzed by direct reading spectrometer for the content of each impurity element in the tungsten oxide powder. The results are: Na 9.0 ppm, K 8.0 ppm, Mg 0.85 ppm, Al 4.86 ppm, Si 1.32ppm, Ca 5.89 ppm, Ti 4.11 ppm, V 4.62 ppm, Mn 0.68 ppm, Fe 5.06 ppm, Co 0.43 ppm, Ni0.77 ppm, Cu 3.5 ppm, As 3.10 ppm, Mo 9.0 ppm, Cd 1.57 ppm, Cr 4.69 ppm, Sn 3.91ppm, Sb 1.87 ppm, Pb The total content of impurity elements is less than 50 ppm, which indicates that the quality of the tungsten oxide powder obtained in this embodiment exceeds the quality requirements of the national standard.

[0034] Embodiment 3: The process of the ion exchange ammonia-free smelting method of tungsten in this embodiment is the same as that of the embodiment 1, and the specific process parameters are:

[0035] S1. Dynamic adsorption: Measure 280 ml of 201×7U strong alkaline anion exchange resin and load it into a simulated exchange column (the simulated exchange column is made of organic glass, with a size of φ4cm×60cm and a resin layer height of 40cm). Soak the resin in pure water for 24 hours. During the soaking, the liquid level exceeds the resin layer by 2cm. Then soak it in 0.5mol / L hydrochloric acid solution for 24 hours. After soaking, wash it with 2000ml of clean water until the pH value of the water out of the exchange column is 5.0. The prepared low-concentration sodium tungstate solution (WO3 18.01g / L, NaOH 3.26g / L) was pumped into the simulated exchange column by a peristaltic pump for dynamic adsorption. The flow rate was controlled at 2ml / min. When the WO3 concentration of the simulated exchange column was ≥0.5g / L, the adsorption was stopped. At this time, the volume of the low-concentration sodium tungstate solution pumped into the simulated exchange column was 2550ml, and the dynamic adsorption was completed. Then the washing process was entered, and 2000ml of pure water was used for washing. The washing water flow rate was 5ml / min. After the washing was completed, washing water I was obtained. After the dynamic adsorption effluent and washing water I were mixed, the volume was measured to be 4460ml. The WO3 concentration was measured by sampling to be 0.08g / L, and the total adsorbed WO3 was 45.57g, and the adsorption rate was 99.23%. The adsorption-saturated 201×7U strong alkaline anion exchange resin entered the next link.

[0036] S2, ammonia-free desorption: the saturated 201×7U strong basic anion exchange resin in step S1 is subjected to dynamic desorption, the desorbent is a mixed solution of sodium chloride and sodium hydroxide, wherein the concentration of sodium chloride is 218.67 g / L, the concentration of sodium hydroxide is 4.69 g / L, the flow rate of the desorbent pumped in is controlled to be 2 ml / min, the total volume of the desorbent is 180 ml, and the desorbent is collected three times in the order of the desorbent discharge, the first collection volume is 50 ml, the WO3 concentration is 3.05 g / L, the WO3 concentration is low, and the desorbent is returned to the dynamic desorption system after collection. The second collection volume is 170ml, the WO3 concentration is 264.79g / L, the WO3 concentration is high, it is a high concentration sodium tungstate solution, and it enters the acid precipitation purification link. The third collection volume is 50ml, the WO3 concentration is 2.65g / L, and the WO3 concentration is relatively low. After collection, it is used to prepare the desorbent for the next cycle. The total desorption rate is 99.41%. The 201×7U strong alkaline anion exchange resin after desorption is washed with pure water and enters the next dynamic adsorption cycle for recycling to obtain washing water II, which is collected and treated.

[0037] S3, acid precipitation purification: The high-concentration sodium tungstate solution (second-stage desorption liquid) obtained in step S2 is neutralized and purified by acid precipitation with sulfuric acid. Sulfuric acid is added to the acid precipitation end point to an acid concentration of 4 mol / L. Stir at room temperature for 2 hours. After the acid precipitation is completed, filter and wash to obtain filtrate I and filter residue I. The acid precipitation filtrate I is collected and processed, and the filter residue I is stirred and washed three times. For the first washing, sulfuric acid solution is used as a detergent, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate II and filter residue II. Filtrate II is collected and processed, and filter residue II is washed for the second time. Sulfuric acid is used as a detergent for this washing, the acid concentration is 2 mol / L, the washing liquid-to-solid mass ratio is 1:1, and the stirring washing time is 1 hour. After the washing is completed, it is filtered to obtain filtrate III and filter residue III. Filtrate III is collected and processed, and filter residue III is washed for the third time. This time, hot pure water is used for washing, and the washing liquid-to-solid mass ratio is 4:1, stir and wash for 1h, filter after washing to obtain filtrate IV and residue IV, collect and treat filtrate IV, dissolve residue IV with hydrogen peroxide at room temperature, liquid-to-solid mass ratio is 5:1, dissolution time is 3h, after dissolution, heat the solution to 60-80℃, then add sulfuric acid and stir for acid precipitation, the end point of acid precipitation is when the concentration of sulfuric acid in the solution reaches 2mol / L, filter after acid precipitation, wash with hot pure water, obtain tungstic acid and washing water III after washing, dry tungstic acid and enter the next link, collect and treat acid precipitation mother liquor and washing water III after acid precipitation purification.

[0038] S4, oxidative roasting: the tungstic acid obtained in step S3 is oxidatively roasted at a temperature of 650°C to 750°C for 4 hours. After the roasting, tungsten oxide powder is obtained. The tungsten oxide powder is sampled and then analyzed by direct reading spectrometer for the content of each impurity element in the tungsten oxide powder. The results are as follows: Na 5.0 ppm, K 4.0 ppm, Mg 0.53 ppm, Al 3.25 ppm, Si 0.41 ppm, Ca 3.25 ppm, Ti 2.28 ppm, V 2.81 ppm, Mn 0.31 ppm, Fe 3.15 ppm, Co0.22 ppm, Ni 0.45 ppm, Cu 1.2 ppm, As 2.49 ppm, Mo 5.0 ppm, Cd 0.96 ppm, Cr 3.38ppm, Sn 2.57 ppm, Sb 1.34 ppm, Pb 0.23 ppm, Bi 0.32 ppm, P 3.0 ppm, and the total content of impurity elements is less than 50 ppm, which means that the quality of the tungsten oxide powder obtained in this embodiment exceeds the quality requirements of the national standard.

[0039] The above describes the main technical features and basic principles of the present invention and the related advantages. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the concept or basic features of the present invention. Therefore, no matter from which point of view, the above specific embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0040] In addition, it should be understood that although the present specification is described according to various implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation method may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for ion exchange ammonia-free smelting of tungsten, characterized in that: The following steps are involved: S1. Dynamic adsorption: Place 201×7U strong alkaline anion exchange resin in a simulated exchange column, soak the 201×7U strong alkaline anion exchange resin in pure water for 24 hours, then soak it in 0.5mol / L hydrochloric acid solution for 24 hours, wash it with clean water after soaking, then place a low concentration sodium tungstate solution in the simulated exchange column for dynamic adsorption, and finally wash it with pure water to obtain washing water I. After washing, the adsorption-saturated 201×7U strong alkaline anion exchange resin enters the next step, and washing water I is collected and processed; S2, ammonia-free desorption: the saturated 201×7U strong alkaline anion exchange resin in step S1 is dynamically desorbed, the desorbent is a mixed solution of sodium chloride and sodium hydroxide, the desorbed liquid is collected to obtain a high-concentration sodium tungstate solution, and enters the next step. The desorbed 201×7U strong alkaline anion exchange resin is washed with pure water and enters the next dynamic adsorption cycle for recycling to obtain washing water II, which is collected and processed; S3, acid precipitation purification: the high concentration sodium tungstate solution obtained in step S2 is neutralized and purified by acid precipitation with inorganic acid. After the neutralization and purification of the acid precipitation, it is filtered and washed to obtain filtrate I and filter residue I. The filtrate I is collected and processed. The filter residue I is stirred and washed three times to obtain filter residue IV. The filter residue IV is dissolved at room temperature with hydrogen peroxide. After the dissolution is completed, the dissolved solution is heated to 60°C to 80°C, and then sulfuric acid is added to stir the acid precipitation. The stirring speed is 40r / min to 60r / min. The end point of the stirring acid precipitation is that the sulfuric acid concentration in the solution is 1mol / L to 2mol / L. After the stirring acid precipitation is completed, it is filtered and washed with hot pure water. After washing, tungstic acid and washing water III are obtained. The tungstic acid is dried and enters the next link. The acid precipitation mother liquor and washing water III after the acid precipitation purification are collected and processed; S4, oxidative calcination: oxidative calcination of the tungstic acid obtained in step S3, the calcination temperature is 650°C to 750°C, the calcination time is 2h to 5h, and tungsten oxide powder is obtained after the calcination; In step S1, when the 201×7U strong alkaline anion exchange resin is soaked in pure water, the pure water level exceeds the resin layer by 2 cm, and the soaked 201×7U strong alkaline anion exchange resin is washed with clean water until the pH value of the simulated exchange column outlet water is 5-7, and the end point of dynamic adsorption is that the WO3 concentration in the simulated exchange column outlet water is ≥0.5g / L.

2. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: The simulated exchange column in step S1 is made of organic glass and has a size of φ4 cm×60 cm.

3. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: In step S2, the concentration of sodium chloride in the desorbent is 180 g / L to 220 g / L, and the concentration of sodium hydroxide is 0.5 g / L to 5 g / L.

4. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: In step S2, the desorption liquid is collected three times in the order of the desorption liquid discharge. The first time, 18% to 22% of the resin volume of the desorption liquid is collected for returning to the dynamic adsorption. The second time, 59% to 61% of the resin volume of the desorption liquid is collected to enter the next link. The desorption liquid collected this time is a high-concentration sodium tungstate solution. The third time, 19% to 21% of the resin volume of the desorption liquid is collected for preparing the desorbent for the next cycle.

5. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: During the neutralization acid precipitation purification process in step S3, stirring is performed at room temperature for 2 h to 3 h, and the neutralization acid precipitation purification end point is that the inorganic acid concentration in the solution is 2 mol / L to 4 mol / L.

6. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: The process of stirring and washing the filter residue I three times in step S3 is as follows: in the first stirring and washing, inorganic acid is used as a detergent, the acid concentration is 1mol / L~2mol / L, the washing liquid-solid mass ratio is 1:1, the stirring and washing time is 1h, and after the stirring and washing is completed, filtration is performed to obtain filtrate II and filter residue II, filtrate II is collected and processed, and filter residue II is stirred and washed for the second time. In this stirring and washing, inorganic acid is still used as a detergent, the acid concentration is 1mol / L~2mol / L, the washing liquid-solid mass ratio is 1:1, and the stirring and washing time is 1h. After the stirring and washing is completed, filtration is performed to obtain filtrate III and filter residue III, filtrate III is collected and processed, and filter residue III is stirred and washed for the third time. Hot pure water is used as a detergent for this stirring and washing, the washing liquid-solid mass ratio is 3:1~5:1, stirring and washing for 1h, and after the stirring and washing is completed, filtration is performed to obtain filtrate IV and filter residue IV, filtrate IV is collected and processed, and the stirring speed of the three times is 40r / min~60r / min.

7. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: When the filter residue IV is dissolved at room temperature with hydrogen peroxide in step S3, the liquid-to-solid mass ratio is 1:1 to 3:1, and the dissolution time is 1h to 3h.

8. The ion exchange ammonia-free smelting method of tungsten according to claim 1, characterized in that: In step S3, the inorganic acid is hydrochloric acid, sulfuric acid or nitric acid.