A method for preparing a high voltage lithium ion battery conductive slurry and its application

By using a combination of high molecular weight and low molecular weight surfactant and high-purity conductive carbon materials, high voltage conductive paste is prepared, which solves the problems of poor gas production expansion and high temperature circulation performance of high voltage lithium-ion batteries, and improves the stability of the battery and electrical performance.

CN118711898BActive Publication Date: 2024-12-06CHONGQING ZHONGRUN NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410793446.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-12-06
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

During use, high-voltage lithium-ion batteries have problems with poor gas production expansion and high-temperature cycling performance. Existing conductive dispersants such as PVP and PVDF are oxidized and decomposed at high voltages, affecting the thickness expansion and stability of the battery.

Method used

Using a combination of high molecular weight surfactant and low molecular weight surfactant, combined with high crystallinity and high purity conductive carbon materials, such as CNT or graphene, a high voltage conductive paste is prepared by adjusting the ratio of surfactant and stirring conditions. Improve the dispersion and stability of the battery.

Benefits of technology

It effectively reduces the gas production of the battery, improves the stability of high-temperature cycles, and the fluidity and viscosity of the battery, meets the requirements of automated production of battery production, improves the discharge capacity retention rate of the battery and reduces the thickness expansion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118711898B_ABST
    Figure CN118711898B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a high-voltage lithium-ion battery conductive slurry, comprising the following steps: adding a high molecular weight surfactant and a low molecular weight surfactant to an organic solvent, stirring to dissolve them to obtain a dispersant solution, adding a conductive carbon material to the obtained dispersant solution, stirring to fully wet and disperse them, and obtaining a composite conductive carbon material; and sand-milling and high-pressure homogenizing and dispersing the composite conductive carbon material to obtain a high-voltage conductive slurry. The present invention uses a high molecular weight surfactant to replace traditional PVP and PVDF dispersants, and the HUMO energy level is low, which is matched with a low molecular weight surfactant. By adjusting the ratio of the two surfactants, the slurry oxidation decomposition voltage reaches above 4.5V, reducing battery gas production, and ultimately improving the thickness expansion of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery materials, and specifically relates to a method for preparing a high-voltage lithium ion battery conductive slurry and an application thereof. Background Art

[0002] High-voltage lithium-ion batteries (>4.3V) have become an important direction of current technology research and development because they have higher energy density than traditional lithium-ion batteries. However, high-voltage lithium-ion batteries are prone to gas expansion and poor high-temperature cycle performance during use, which restricts their widespread application in terminal products. There are rich types of positive electrode materials used in high-voltage lithium-ion batteries, such as high-voltage lithium cobalt oxide, high-voltage ternary, nickel-manganese, lithium-rich manganese-based, etc. These transition metal salt oxide positive electrodes have a high upper charging limit voltage, generally reaching 4.3-4.5V, which can significantly improve the energy density of current lithium-ion batteries. However, transition metal salt oxide positive electrodes also generally have the problem of unsatisfactory electronic conductivity. In actual use, conductive agents need to be added to construct an electron transport conductive network to achieve good rate discharge and cycle performance. In recent years, CNT or graphene-type conductive slurries, with their excellent electronic conductivity and chemical stability, can greatly reduce the amount of traditional carbon black conductive agents used, and their market share is also increasing.

[0003] CNT or graphene conductive agent has a high specific surface area and nano-size agglomeration effect, so a small amount of dispersant needs to be added during the dispersion process to solve the problem of rapid dispersion, thereby improving the dispersion and stability of the slurry. Polyvinyl pyrrolidone (PVP) and polyvinylidene fluoride (PVDF) polymer dispersants are the mainstream dispersants used by conductive slurry manufacturers. PVP dispersant has a cyclic stereoscopic structure and a linear alkane straight chain structure, which makes CNT or graphene have good wetting and dispersibility in organic N-methylpyrrolidone (NMP) solvent; but because of its own structure The HUMO energy level is high, it will oxidatively decompose and generate a large amount of gas when it is >4.3V, thus affecting the thickness expansion problem of the battery. PVDF dispersant contains fluorine atoms, has a relatively high CF bond energy, and a low HUMO energy level. It has good oxidation stability, but it lacks a cyclic stereoscopic structure, and the wettability of the slurry is poor. It is also difficult to form a strong intermolecular force with graphene and CNT, which makes the slurry dispersion and stability poor. Summary of the invention

[0004] In order to solve the problems of thickness expansion and high-temperature cycle stability of high-voltage lithium-ion batteries in the prior art, a new type of surfactant dispersant and a conductive carbon material with high crystallinity, high purity and moderate specific surface area are effectively combined to jointly improve the thickness expansion and high-temperature cycle stability of high-voltage lithium-ion batteries.

[0005] The present invention solves the technical problem by adopting the following technical solutions:

[0006] An object of the present invention is to provide a method for preparing a high voltage lithium ion battery conductive paste, characterized in that it comprises the following steps:

[0007] 1) Preparation of dispersant solution

[0008] Adding a high molecular weight surfactant and a low molecular weight surfactant to an organic solvent, stirring to dissolve them to obtain a dispersant solution, wherein the molecular weight of the high molecular weight surfactant is 50,000 to 100,000;

[0009] 2) Preparation of composite conductive carbon materials

[0010] Add the conductive carbon material to the dispersant solution obtained in step 1), stir to fully wet and disperse it, and obtain a composite conductive carbon material; the conductive carbon material is CNT and / or graphene carbon material, and the CNT or graphene powder is D / I G Peak ratio ≤1.1, C content ≥99%;

[0011] 3) Obtain dispersed high voltage conductive slurry

[0012] The composite conductive carbon material obtained in step 2) is sand-milled and homogenized under high pressure to obtain a high-voltage conductive slurry.

[0013] Furthermore, the mass ratio of the high molecular weight surfactant to the low molecular weight surfactant is 5-20:2-10.

[0014] Furthermore, the high molecular weight surfactant is a structure in which a three-dimensional benzene ring is combined with a linear branched alkane. The high molecular weight surfactant having a structure in which a three-dimensional benzene ring is combined with a linear branched alkane is selected. The three-dimensional benzene ring structure is conducive to the wetting of the conductive carbon material, and the linear branched alkane structure is conducive to the dispersion of the conductive carbon material. By adjusting the molecular weight of the high molecular weight surfactant, the dispersibility of the dispersant is improved, and the agglomeration of the conductive carbon material itself caused by the excessive amount of adsorbed conductive carbon material and the high viscosity of the slurry is avoided, and the steric hindrance effect is not obvious and the dispersibility is poor due to the too high molecular weight.

[0015] Furthermore, the high molecular weight surfactant is selected from styrene-butadiene-styrene block copolymer (SBS) or polystyrene.

[0016] Furthermore, the low molecular weight surfactant is selected from any one of ethanolamine, piperazine and triethylenediamine. The low molecular weight surfactant has excellent dispersibility, reduces the amount of solvent adsorbed by the conductive carbon material, and thus improves the fluidity and viscosity of the slurry.

[0017] Furthermore, the added amount of the conductive carbon material is 2-5% of the mass of the conductive slurry.

[0018] Furthermore, the metal impurity content of the CNT or graphene powder is ≤200ppm, and the specific surface area is 150-350m 2 / g.

[0019] Furthermore, when the conductive carbon materials added are CNT and graphene powder, the mass ratio of the CNT to the graphene powder is 3-8:2-7.

[0020] Furthermore, the organic solvent is N-methylpyrrolidone (NMP).

[0021] Furthermore, the amount of NMP added is 97-99.3% of the total mass of the dispersant solution.

[0022] Furthermore, in step 1), the mechanical stirring speed is 800-1500 rpm, the stirring time is 2-4 h, and the stirring temperature is 35-50°C.

[0023] Furthermore, in step 2), the stirring speed is 1500-3000 rpm, and the stirring time is 2-6 h.

[0024] Furthermore, in step 3), the sanding equipment is a pin-type or turbine-type sanding device, and the sanding medium is zirconium oxide.

[0025] Furthermore, in step 3), the rotation speed during sand grinding is 1000-2000 rpm, the sand grinding time is ≥2h, and the particle size D50 of the delivered slurry is ≤3um.

[0026] Furthermore, the high-pressure homogenization pressure is 800-1200 bar, the homogenization times are ≥5 times, and the particle size of the shipped slurry D50 is ≤1 um.

[0027] Another object of the present invention is to provide an application of a high-voltage lithium-ion battery conductive paste in a high-voltage lithium-ion battery.

[0028] Compared with the prior art, the beneficial technical effects of the present invention are:

[0029] The present invention forms a high-voltage lithium-ion battery conductive slurry, which effectively combines a new type of surfactant dispersant and a conductive carbon material with high crystallinity, high purity and moderate specific surface area to jointly improve the thickness expansion and high-temperature cycle stability of high-voltage lithium-ion batteries. By selecting a high molecular weight surfactant to replace the traditional PVP and PVDF dispersants, the HUMO energy level is low, and it is matched with a low molecular weight surfactant. By adjusting the ratio of the two surfactants, the slurry oxidation decomposition voltage reaches more than 4.5V, reducing the gas production of the battery, and finally improving the thickness expansion of the battery; and improving the fluidity and viscosity of the slurry, so that the prepared high-voltage conductive slurry can better meet the automated production requirements of battery manufacturers.

[0030] The present invention selects high-purity, high-crystallization and moderate-specific-surface-area CNT or graphene powder to make it more suitable for the application scenario of high-voltage lithium-ion batteries, and further improve the gas production and cycle stability of the battery.

[0031] The present invention controls the particle size of the slurry, so that the dispersibility, long-term storage performance, and production and transportation costs of the slurry are reasonably improved.

[0032] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a SEM image of the high-voltage conductive paste of Example 3 in a method for preparing a high-voltage lithium-ion battery conductive paste and its application in the present invention.

[0034] Figure 2 The LSV curves of Examples 1-3 and Comparative Examples 1-3 in a method for preparing a high-voltage lithium-ion battery conductive paste and its application in the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection that the present invention is intended to protect.

[0036] In addition, unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0037] Embodiment 1:

[0038] A method for preparing a high-voltage lithium-ion battery conductive slurry comprises the following steps:

[0039] 1) Preparation of dispersant solution

[0040] At room temperature, 50g of high molecular weight surfactant SBS and 25g of low molecular weight surfactant ethanolamine were added to 4725kg NMP organic solvent to prepare a dispersant solution with a concentration of 1.56%. The solution was stirred and dissolved at a constant temperature of 45°C to obtain a dispersant solution. The molecular weight of SSB was 60,000 to 70,000. The mechanical stirring speed was 1200rpm and the stirring time was 2h.

[0041] 2) Preparation of composite conductive carbon materials

[0042] Add 200g of CNT conductive carbon material to the dispersant solution obtained in step 1), stir to fully wet and disperse it, and prepare a composite conductive carbon slurry with a carbon concentration of 4.0% and a dispersant concentration of 1.5%. The mechanical stirring speed is 2000rpm and the stirring time is 4h. The specific surface area of ​​the CNT powder used is 250m 2 / g,I D / I G The peak ratio is 0.9, the carbon content is 99.7%, and the total metal impurity content of the powder is 150ppm.

[0043] 3) Obtain dispersed high voltage conductive slurry

[0044] At room temperature, the composite conductive carbon material obtained in step 2) is sand-milled and dispersed by high-pressure homogenization to obtain a high-voltage conductive slurry. The size of the ball used for sand-milling is 0.8um, the material is zirconium oxide, the rotation speed is 1500rpm, the sand-milling time is 3h, and the particle size D50 is 2.5um; the high-pressure homogenization pressure is 900-1000bar, the homogenization times are 10 times, and the slurry particle size D50 is 0.7um.

[0045] Embodiment 2:

[0046] The difference from Example 1 is that the 200g CNT conductive carbon material in Example 1 is replaced by 200g graphene conductive carbon material, and the specific surface area of ​​the graphene powder is 280m 2 / g,I D / I G The peak ratio is 1.0, the carbon content is 99.3%, and the total metal impurity content of the powder is 50 ppm.

[0047] The particle size D50 of the high voltage conductive slurry obtained after high pressure homogenization is 0.6 um.

[0048] Embodiment 3:

[0049] The difference from Example 1 is that the 200g CNT conductive carbon material in Example 1 is replaced by 80g graphene conductive carbon material and 120g CNT conductive carbon material. The specific surface area of ​​the CNT powder is 250m 2 / g,I D / I G The peak ratio is 0.9, the carbon content is 99.7%, the total content of metal impurities in the powder is 150ppm; the specific surface area of ​​the graphene powder is 280m 2 / g,I D / I G The peak ratio is 1.0, the carbon content is 99.3%, and the total metal impurity content of the powder is 50 ppm. Figure 1 This is the SEM image of the conductive paste of this embodiment.

[0050] The particle size D50 of the high voltage conductive slurry obtained after high pressure homogenization is 0.8 um.

[0051] Comparative Example 1:

[0052] A method for preparing a high-voltage lithium-ion battery conductive slurry comprises the following steps:

[0053] 1) Preparation of dispersant solution

[0054] At room temperature, 50g of high molecular weight surfactant SBS and 25g of low molecular weight surfactant ethanolamine were added to 4725kg NMP organic solvent to prepare a dispersant solution with a concentration of 1.56%. The solution was stirred and dissolved at a constant temperature of 45°C to obtain a dispersant solution. The molecular weight of SSB was 60,000 to 70,000. The mechanical stirring speed was 1200rpm and the stirring time was 2h.

[0055] 2) Preparation of composite conductive carbon materials

[0056] Add 100g of CNT conductive carbon material to the dispersant solution obtained in step 1), stir to fully wet and disperse it, and prepare a composite conductive carbon slurry with a carbon concentration of 2.0% and a dispersant concentration of 1.5%. The mechanical stirring speed is 2000rpm and the stirring time is 4h. The specific surface area of ​​the CNT powder used is 500m 2 / g,I D / I G The peak ratio is 1.3, the carbon content is 97%, and the total metal impurity content of the powder is 4000ppm.

[0057] 3) Obtain dispersed high voltage conductive slurry

[0058] At room temperature, the composite conductive carbon material obtained in step 2) is sand-milled and dispersed by high-pressure homogenization to obtain a high-voltage conductive slurry. The ball size used in the sand-milling is 0.8um, the material is zirconium oxide, the rotation speed is 1500rpm, the sand-milling time is 3h, and the particle size D50 is 2.5um; the high-pressure homogenization pressure is 900-1000bar, the homogenization times are 10 times, and the slurry particle size D50 is 0.6um.

[0059] Comparative Example 2:

[0060] The difference from Comparative Example 1 is that 100 g of CNT conductive carbon material in Comparative Example 1 is replaced by 100 g of graphene conductive carbon material, and the specific surface area of ​​the graphene powder is 470 m 2 / g,I D / I G The peak ratio is 1.2, the carbon content is 96%, and the total metal impurity content of the powder is 500ppm.

[0061] The particle size D50 of the high voltage conductive slurry obtained after high pressure homogenization is 0.6 um.

[0062] Comparative Example 3:

[0063] A method for preparing a high-voltage lithium-ion battery conductive slurry comprises the following steps:

[0064] 1) Preparation of dispersant solution

[0065] At room temperature, 75 g of PVP was added to 4725 kg of NMP organic solvent to prepare a dispersant solution with a concentration of 1.56%, and the solution was stirred at a constant temperature of 45°C to dissolve the solution. The mechanical stirring speed was 1200 rpm and the stirring time was 2 hours.

[0066] 2) Preparation of composite conductive carbon materials

[0067] Add 200g of CNT conductive carbon material to the dispersant solution obtained in step 1), stir to fully wet and disperse it, and prepare a composite conductive carbon slurry with a carbon concentration of 4.0% and a dispersant concentration of 1.5%. The mechanical stirring speed is 2000rpm and the stirring time is 4h. The specific surface area of ​​the CNT powder used is 250m 2 / g,I D / I G The peak ratio is 0.9, the carbon content is 99.7%, and the total metal impurity content of the powder is 150ppm.

[0068] 3) Obtain dispersed high voltage conductive slurry

[0069] At room temperature, the composite conductive carbon material obtained in step 2) is sand-milled and dispersed by high-pressure homogenization to obtain a high-voltage conductive slurry. The ball size used in the sand-milling is 0.8um, the material is zirconium oxide, the rotation speed is 1500rpm, the sand-milling time is 3h, and the particle size D50 is 2.5um; the high-pressure homogenization pressure is 900-1000bar, the homogenization times are 10 times, and the slurry particle size D50 is 0.8um.

[0070] Test Example 1:

[0071] The conductive pastes obtained in each embodiment and comparative example were respectively mixed with PVDF glue in a mass ratio of 9:1 in NMP solvent to prepare test slurries. The obtained test slurry was coated on an aluminum foil with a thickness of 16um and a PET film with a thickness of 60um with a 100um scraper, and then dried, rolled, and punched into button-type discs with diameters of 12mm and 16mm. The 16mm PET film disc was tested for its resistivity using a four-probe resistivity tester. Lithium foil was used as the counter electrode and assembled with the above-prepared 12mm aluminum foil button-type disc into a button-type 2032 battery. The main components of the battery electrolyte are: lithium hexafluorophosphate is used as the lithium salt with a concentration of 1.0mol / L; the solvents are ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate with a mass ratio of 1:1:1. The thickness of the diaphragm is 20um, and it is a polyethylene microporous diaphragm. The battery was tested by linear sweep voltammetry (LSV) with a battery range of 3.8-4.8V and a scan rate of 1.0mV / s.

[0072] Table 1 shows the test values ​​of slurry particle size, viscosity and resistivity obtained in each embodiment and comparative example. Figure 2 It can be seen that, compared with Comparative Example 1 and Comparative Example 2, the CNT or graphene used in the embodiment of the present application has a low metal impurity content and a high carbon content, and the measured specific surface area and slurry viscosity of the conductive carbon material are significantly lower than those of Comparative Example 1 and Comparative Example 2. It can be seen that although the carbon content has a certain improvement on the resistivity of the slurry, the effect on the specific surface area and viscosity of the slurry is more obvious, which greatly increases the specific surface area and viscosity of the slurry, thereby affecting the stability of the slurry and affecting the electrical properties of the lithium-ion battery. It can be seen that the use of high-purity CNT or graphene conductive carbon materials is more conducive to obtaining conductive slurries with good electrical properties.

[0073] Table 1

[0074]

[0075] Test Example 2:

[0076] The conductive paste obtained from each embodiment and comparative example is mixed with high-voltage 4.45V lithium cobalt oxide positive electrode material and PVDF glue in a mass ratio of 1.5:95.5:3 in NMP solvent to prepare positive electrode slurry and prepare high-voltage lithium-ion batteries according to the same battery production process, and high-temperature cycle performance and thickness expansion rate tests are carried out respectively. Specifically, the lithium-ion battery after capacity separation is placed in a 45°C high-temperature box and connected to a charge and discharge tester, first charged to 4.45V with a 1C constant current and constant voltage, and the cut-off current is set to 0.02C; after standing for 10 minutes, it is discharged to 3.0V with a 1C constant current, and the cycle charge and discharge test is carried out for 200 weeks, and the discharge capacity is recorded each time. The battery thickness is tested with a micrometer before and after the test. The capacity retention rate at the 200th week (%) = discharge capacity at the 200th week / discharge capacity at the first week × 100%, and the battery expansion rate at the 200th week (%) = (battery thickness at the 200th week - battery thickness before cycle) / battery thickness before cycle × 100% were calculated respectively.

[0077] Table 2

[0078]

[0079]

[0080] Referring to Table 2, the electrical performance test results of lithium-ion batteries obtained by using the conductive slurries of various embodiments and comparative examples are shown. It can be seen that compared with the lithium-ion battery obtained by using PVP as a dispersant, the lithium-ion battery cycle performance obtained by the conductive slurry of the present application is significantly improved compared with that of comparative example 3, the discharge capacity retention rate is increased by 10%, and the thickness expansion rate is reduced by more than 4%. Comparative Example 1 and Comparative Example 2 use the dispersant of the present application to replace PVP, but use the slurry obtained by using CNT and graphene with high specific surface area, low purity and crystallinity, and low metal impurity content. The prepared lithium-ion battery has improved electrical performance after 200 cycles compared with comparative example 3, but compared with the embodiment of the present application, the lithium battery discharge capacity retention rate obtained by the embodiment of the present application is increased by more than 4%, and the thickness expansion rate is reduced by 3%. It can be seen that the slurry obtained by using the new surfactant dispersant in the present application has a significant improvement on the electrical performance of the lithium-ion battery compared with PVP as a dispersant, and the use of CNT and graphene with high purity and high specific surface area improves the electrical performance of the lithium-ion battery more significantly. It can be seen that the combination of the new surfactant dispersant and the conductive carbon material with high crystallinity, high purity and high specific surface area can jointly improve the high temperature cycle stability and thickness expansion problems of high voltage lithium-ion batteries.

[0081] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0082] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing a high voltage lithium ion battery conductive paste, characterized in that: The following steps are involved: 1) Preparation of dispersant solution Adding a high molecular weight surfactant and a low molecular weight surfactant to an organic solvent, stirring to dissolve them to obtain a dispersant solution, wherein the molecular weight of the high molecular weight surfactant is 50,000 to 100,000; the mass ratio of the high molecular weight surfactant to the low molecular weight surfactant is 5 to 20:2 to 10, the high molecular weight surfactant is a structure in which a three-dimensional benzene ring is combined with a linear branched alkane, and the low molecular weight surfactant is selected from any one of ethanolamine, piperazine, and triethylenediamine; 2) Preparation of composite conductive carbon materials Add the conductive carbon material to the dispersant solution obtained in step 1), stir to fully wet and disperse it, and obtain a composite conductive carbon material; the conductive carbon material is CNT and / or graphene carbon material, and the CNT and graphene powders are D / I G Peak ratio ≤1.1, C content ≥99%; 3) Obtain dispersed high voltage conductive slurry The composite conductive carbon material obtained in step 2) is sand-milled and homogenized under high pressure to obtain a high-voltage conductive slurry.

2. The method for preparing a high voltage lithium ion battery conductive paste according to claim 1, characterized in that: The high molecular weight surfactant is selected from styrene-butadiene-styrene block copolymer (SBS) or polystyrene.

3. The method for preparing a high voltage lithium ion battery conductive paste according to claim 1, characterized in that: The added amount of the conductive carbon material is 2-5% of the mass of the conductive slurry.

4. The method for preparing a high voltage lithium ion battery conductive paste according to claim 1, characterized in that: The metal impurity content of the CNT and graphene powder is ≤200ppm, and the specific surface area is 150-350m 2 / g.

5. The method for preparing a high voltage lithium ion battery conductive paste according to claim 1, characterized in that: The organic solvent is N-methylpyrrolidone.

6. A method for preparing a high voltage lithium ion battery conductive paste as claimed in claim 5, characterized in that: The amount of N-methylpyrrolidone added is 97-99.3% of the total mass of the dispersant solution.

7. Use of the high-voltage lithium-ion battery conductive slurry prepared according to the preparation method according to any one of claims 1 to 6 in a high-voltage lithium-ion battery.

Citation Information

Patent Citations

  • Electrode for secondary battery, binder for secondary battery electrode, and secondary battery

    CN102549820A

  • Lithium ion battery

    CN116404253A

  • Carbon nanotube-containing composition, complex having coating film comprising it, and method for manufacturing them

    JP2005281672A

  • Method for manufacturing active material for secondary batteries