Antiskid braid and preparation and application thereof

By screen-printing silicone parts arranged at intervals on the anti-slip webbing, combined with nylon, vinylon and other materials, the problems of complex structure and poor anti-slip effect of the existing anti-slip webbing are solved, and the fit and comfort of the quilt core and quilt cover are achieved. promote.

CN118716818APending Publication Date: 2024-10-01LUOLAI LIFESTYLE TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410747989.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing anti-slip webbing has problems such as complex structure, inconvenient operation, and poor anti-slip effect, which affects the fit between the quilt core and the quilt cover and the comfort of use.

Method used

The screen printing process is used to print spaced silicone parts on the sub-belt. Liquid silicone rubber and curing agent are used to prepare the anti-slip layer. The silicone parts are spaced 30 to 50mm apart. The anti-slip webbing is made of nylon, vinylon, polyester and other materials, and is heated through The pressing process is used to embed the quilt around the core.

Benefits of technology

It achieves an effective fit between the quilt core and the quilt cover, improves the comfort and warmth retention effect, reduces the tediousness of organization, and improves the user's sleep quality. At the same time, the anti-slip layer is not easy to deform, harden, stick to hair and get dust, and has a strong and durable effect. advantage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118716818A_ABST
    Figure CN118716818A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of textile preparation, and provides an anti-slip woven tape and preparation and application thereof.The anti-slip woven tape comprises a sub-tape and a master tape, the sub-tape and the master tape are integrally formed, and the shrinkage rate of the sub-tape and the master tape is 3-5%; an anti-skid layer is printed on each sub-belt, each anti-skid layer comprises a plurality of silica gel parts which are arranged at intervals, the silica gel parts are prepared by taking liquid silicone rubber and a curing agent as raw materials through silk-screen printing, and the interval between every two adjacent silica gel parts is 30-50mm. The anti-skid braid is simple in structure, the micro-damping effect is achieved through the anti-skid layer, the use comfort of a quilt core is not affected, and the anti-skid effect can be effectively achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textile preparation, and in particular to an anti-slip webbing and its preparation and application. Background Art

[0002] During sleep, the fit between the quilt core and the quilt cover has always been the focus of users. However, when the existing quilt core and quilt cover are used together, they often do not fit well and are easy to slip off due to material differences, washing wear and tear, etc., which not only affects the user's sleep quality, but also increases the difficulty of quilt arrangement.

[0003] At present, the anti-skid material used for the quilt core is mostly a fabric anti-skid coating. For example, the patent application document with the publication number CN105040483A provides an anti-skid fabric, the main structure includes an anti-skid layer, fabric, an upper surface and a lower surface, the fabric of the cloth structure is composed of an upper surface and a lower surface, the anti-skid layer is attached to the upper surface by adhesive, and the anti-skid fabric composed of the anti-skid layer and the fabric is comfortable and anti-skid. The acrylic anti-skid agent is attached to one side of the fabric surface by printing, coating or spraying, which increases the friction coefficient of the surface and prevents the surface from sliding relative to the contact object, does not make the anti-skid surface of the fabric uneven, and does not fall off or fail after multiple washings. The other side of the fabric surface is not processed in any way to retain its original appearance and performance. However, this anti-skid coating affects the softness of the fabric when it is used.

[0004] Alternatively, the existing technology develops anti-slip webbing, which is mostly made of full silicone with a thickness of 3 to 5 mm. However, after long-term use, the silicone part will be covered with dust and hair, resulting in a poor user experience.

[0005] Although there are some anti-slip products on the market, most of them have problems such as complex structure, inconvenient operation and poor anti-slip effect. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides an anti-skid webbing and its preparation and application to solve the problems of complex structure, inconvenient operation and poor anti-skid effect of most anti-skid products in the prior art.

[0007] To achieve the above and related purposes, the present invention adopts the following technical solutions:

[0008] A first aspect of the present invention provides an anti-slip webbing, comprising a sub-belt and a main belt, wherein the sub-belt and the main belt are integrally formed, and the shrinkage rate of the sub-belt and the main belt is 3-5%;

[0009] The sub-belt is printed with an anti-skid layer, which includes a plurality of silicone parts arranged at intervals. The silicone parts are made of liquid silicone rubber and a curing agent and are prepared by screen printing. Adjacent silicone parts are spaced 30 to 50 mm apart.

[0010] In one embodiment of the present application, the material of the sub-belt and the main belt is one or more of nylon, vinylon, polyester, and polypropylene.

[0011] In one embodiment of the present application, the width of the sub-band is 2 to 5 mm;

[0012] And / or, the width of the mother tape is 8 to 15 mm.

[0013] A second aspect of the present invention provides a method for preparing an anti-slip webbing, comprising the following steps:

[0014] (1) Weaving, high-temperature shaping, and pre-shrinking the raw yarn to prepare an integrally formed sub-belt and mother belt;

[0015] (2) Using liquid silicone rubber and curing agent as raw materials to prepare printing silicone;

[0016] (3) Printing silicone is brushed onto the sub-belt through a screen printing process to form a plurality of silicone parts, and the silicone parts are brushed with color to obtain a non-slip webbing.

[0017] In one embodiment of the present application, in step (1), the temperature of high temperature setting is 200-250°C.

[0018] In one embodiment of the present application, in step (2), the mass ratio of liquid silicone rubber to curing agent is (10-15): (1.5-2).

[0019] In one embodiment of the present application, in step (3), the thickness of the silicone portion is 0.08-0.12 mm;

[0020] And / or, the printing interval between adjacent silicone parts is 30 to 50 mm.

[0021] In one embodiment of the present application, in step (3), after brushing and coloring, multiple drying passes are performed, and each drying pass is kept for 5 to 15 seconds.

[0022] A third aspect of the present invention provides a quilt core, comprising the above-mentioned anti-slip webbing, or comprising the anti-slip webbing obtained according to the above-mentioned preparation method.

[0023] In one embodiment of the present application, the anti-slip webbing is made into a welt by a hot pressing process, and is arranged around the quilt core by a sewing process.

[0024] The beneficial technical effects of the present invention are:

[0025] The anti-skid webbing of the present invention is suitable for quilt cores of various specifications and materials, and can effectively solve the problem that the quilt core and the quilt cover do not fit well and are easy to slip off. By using the anti-skid webbing of the present invention, the cost and efficiency of webbing production can be significantly improved, while the comfort and warmth retention of the quilt core can be improved, the tediousness of arrangement can be reduced, and the sleep quality of users can be improved.

[0026] The anti-skid webbing of the present invention has a simple structure and has a micro-damping effect through the ultra-thin anti-skid layer, which does not affect the comfort of the quilt core and can effectively prevent skidding. In addition, the several silicone parts in the ultra-thin anti-skid layer are not easy to deform, harden, stick to hair and dust, and have the advantages of being firm and durable.

[0027] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:

[0029] Figure 1 This is a schematic diagram of the anti-slip webbing structure;

[0030] Figure 2 Schematic diagram of the structure of the silicone part;

[0031] Figure 3 It is a schematic diagram of the quilt core structure.

[0032] Reference numerals

[0033] 1: anti-slip webbing; 11: sub-belt; 12: main belt; 3: anti-slip layer; 31: silicone part; 4: quilt core. DETAILED DESCRIPTION

[0034] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as the general understanding of a person of ordinary skill in the art to which the present invention belongs. It should be understood that certain features of the present invention (described in the context of separate embodiments for clarity) may also be provided in combination in a single embodiment. On the contrary, multiple features of the present invention (described in the context of a single embodiment for brevity) may also be provided separately or in any suitable combination or in any other described embodiment of the present invention when appropriate. Certain features described in the context of various embodiments will not be considered as essential features of those embodiments unless the embodiment is inoperable without those elements. The present invention is further described below by specific specific examples, but it should be noted that the specific process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention, and the protection scope of the present invention cannot be limited thereto. All equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.

[0035] The present invention provides an anti-slip webbing, such as Figure 1 As shown, it includes a sub-belt 11 and a main belt 12, the sub-belt 11 and the main belt 12 are integrally formed, and the shrinkage rate of the sub-belt 11 and the main belt 12 is 3-5%;

[0036] The sub-belt 11 is printed with an anti-slip layer 3, which includes a plurality of silicone parts 31 arranged at intervals. The silicone parts 31 are made of liquid silicone rubber and a curing agent and are prepared by screen printing. Adjacent silicone parts 31 are spaced 30 to 50 mm apart.

[0037] Furthermore, the anti-skid layer 3 of the present application is made of silicone material because it has good elasticity, wear resistance and anti-skid performance. The hardness of the silicone can be adjusted according to actual needs. The existing anti-skid belt usually selects silicone with a hardness of 50 to 70A on Shore A, while the Shore A hardness of the silicone part 31 of the present application is lower than 50A.

[0038] Furthermore, the anti-slip layer 3 of the present application is distributed on the outside of the sub-belt 11 , and a plurality of silicone parts 31 are printed by a screen printing scraper, thereby ensuring the consistency of shape and size of the silicone parts 31 .

[0039] Furthermore, the material of the sub-belt 11 and the main belt 12 is one or more of nylon, vinylon, polyester, and polypropylene.

[0040] Furthermore, the width of the sub-tape 11 is 2 to 5 mm, and the width of the main tape 12 is 8 to 15 mm.

[0041] Furthermore, since the present application adopts screen printing, the surface pattern of the anti-slip webbing 1 can be made into a film printing plate of any pattern as needed, and the silicone part 31 of various shapes can be made, such as Figure 2As shown, there is a convex silicone portion 31, etc.

[0042] Furthermore, the anti-skid webbing 1 of the present application is provided with an ultra-thin anti-skid layer 3, which ensures the anti-skid effect while not affecting the softness of the fabric.

[0043] Furthermore, the anti-skid layer 3 of the present application can also be made of elastic materials such as rubber, thermoplastic elastomer, etc. Alternatively, the present application can also add textures or convex points on the outer side of the anti-skid webbing 1 to increase its anti-skid performance.

[0044] The present invention also provides a method for preparing an anti-slip webbing, comprising the following steps:

[0045] (1) Weaving, high-temperature shaping, and pre-shrinking the raw yarn to prepare an integrally formed sub-belt and mother belt;

[0046] (2) Using liquid silicone rubber and curing agent as raw materials to prepare printing silicone;

[0047] (3) Printing silicone is brushed onto the sub-belt through a screen printing process to form a plurality of silicone parts, and the silicone parts are brushed with color to obtain a non-slip webbing.

[0048] Furthermore, in step (1), the raw yarn used in the present application is a high-elastic yarn selected from one or more of nylon, vinylon, polyester, and polypropylene. The present application uses the high-elastic yarn for weaving on a ribbon loom, and uses 200-250°C for high-temperature shaping to increase the flatness of the ribbon and perform pre-shrinkage, with the shrinkage rate controlled at 3-5%.

[0049] Furthermore, in step (2), the mass ratio of liquid silicone rubber to curing agent is (10-15):(1.5-2).

[0050] Further, in step (2), the preparation method of printing silica gel is as follows:

[0051] A. Preparation of base glue: weigh 100 parts by mass of vinyl silicone oil, 3-7 parts of hexamethyldisilazane, 30-50 parts of fumed silica (hydrophilic type), 3-6 parts of hydroxy silicone oil, and 5-25 parts of vinyl MQ silicone resin, mix them, raise the temperature to 160°C, maintain -0.095MPa, and degas for 2h to obtain the base glue.

[0052] The vinyl silicone oil is composed of the following components: 800-10,000 parts of DMC, 2-5 parts of vinyl double heads, 5-15 parts of vinyl ring bodies, and 0.05-0.2 parts of tetramethylammonium hydroxide catalyst; DMC, vinyl double heads, and vinyl ring bodies are added into a reaction kettle, the temperature is raised to 60-70°C, vacuumed and dehydrated for 1 hour, the vacuum is removed and the tetramethylammonium hydroxide catalyst is added, the temperature is raised to 110-115°C, and the polymerization is stirred for 2 hours. When the viscosity of the material remains unchanged, the temperature is raised to 190-200°C, the catalyst is broken at a constant temperature for 1 hour, and the low molecular weight is removed by vacuuming.

[0053] The fumed silica (hydrophilic type) is composed of the following components: 100 parts of silica and 7 to 18 parts of hexamethyldisilazane; the speed of the agitator is controlled at 35 r / min, the temperature is 120° C., and the pressure is maintained at -0.095 MPa for 1 hour to obtain the fumed silica.

[0054] B. Weigh 100-120 parts of base rubber and 1.3-1.7 parts of platinum catalyst, add two equal parts of base rubber and one part of platinum catalyst, mix well to obtain liquid silicone rubber, i.e. component a.

[0055] C. Add another equal portion of the base glue to the curing agent, put each component into the dispersant, disperse and stir for 30 minutes, mix evenly and filter to obtain component B.

[0056] The curing agent is composed of the following components: 10,000 to 15,000 parts of DMC, 2 to 5 parts of hydrogen-containing double heads, 1 to 3 parts of high-hydrogen silicone oil KF-99, 8 to 25 parts of hexamethyldisiloxane, and 1.2 to 1.7 parts of acidic cationic resin; the components are put into a mixer at a temperature of 65 to 70°C, refluxed for 2 hours, and then heated to 115 to 120°C, stirred and polymerized for 3 hours, and the liquid is filtered and put into a reactor, and low molecular weight is removed under reduced pressure at 120°C to obtain the product.

[0057] D. Mix component a and component b in the ratio of (10-15) by mass and (0.5-2) by mass for 1 hour to obtain printing silica gel.

[0058] Further, in step (3), the screen printing process is specifically as follows:

[0059] Drawing board out film: determine the anti-slip webbing pattern and interval, out film, film aperture 150 ~ 170 mesh;

[0060] Plate making: Install the opened film on the printing plate;

[0061] Laying tape at the punching position: according to the width of the anti-slip webbing, set the corresponding infrared position, the sub-tape width is 2-5mm, the mother tape width is 8-15mm, to provide a contrast for the neatness of the anti-slip webbing. The tape is laid by machine positioning, the laying accuracy is plus or minus tolerance 0.3%, and the printing plate length is 45 meters;

[0062] Multiple printing: Lay the printing plate, manually brush silica gel, the thickness of the silica gel part is 0.08-0.12mm, the printing interval is 30-50mm, 1 brushing to shape, 1 brushing to color, and dry it in a 150-200℃ dryer for 10 times, staying for 5-15 seconds each time.

[0063] Furthermore, after the drying is completed, the present application can also perform post-processing such as cleaning and ironing on the anti-slip webbing.

[0064] like Figure 3 As shown, the present invention further provides a quilt core, comprising the above-mentioned anti-slip webbing 1, or comprising the anti-slip webbing 1 obtained according to the above-mentioned preparation method.

[0065] Furthermore, the anti-skid webbing 1 is made into a stripe shape matching the edge of the quilt core 4 by a hot pressing process, and is set around the quilt core 4 by a sewing process. After the production is completed, the quilt core 4 with the anti-skid webbing 1 can be put into the quilt cover. Due to the micro-damping effect of the anti-skid webbing 1, the quilt core 4 is not easy to slide in the quilt cover, and it is convenient to fit and remove. The anti-skid webbing 1 of the present application effectively solves the problem that the quilt core 4 and the quilt cover do not fit well and are easy to slip off, and improves the comfort and warmth of the quilt.

[0066] Furthermore, the length of the anti-skid webbing 1 of the present application is calculated based on the circumference of the quilt core 4 to ensure that the anti-skid webbing 1 can completely wrap around the quilt core 4 .

[0067] Furthermore, when the anti-slip webbing 1 of the present application is sewn around the quilt core 4, sewing thread that matches the material of the quilt core 4 can be used to ensure firmness and aesthetics.

[0068] The present invention is described in detail below by specific examples. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0069] Example 1

[0070] (1) 150D polyester high elastic yarn is used for weaving on a weaving machine, and high temperature setting is performed at 200°C to increase the flatness of the weaving and pre-shrink it, and the shrinkage rate is controlled at 3%. The width of the prepared sub-belt is 2mm, and the width of the master belt is 10mm.

[0071] (2) A. Preparation of base rubber: Weigh 100 parts by weight of vinyl silicone oil (viscosity 5000 mPa·s, vinyl mass fraction 0.16%), 6 parts of hexamethyldisilazane, 40 parts of fumed silica (hydrophilic type) (specific surface area 380 m 2 / g), 5 parts of hydroxy silicone oil (mass fraction 10%, viscosity 20-30mm 2 / s), 15 parts of vinyl MQ silicone resin (RH-S11), mixed, heated to 160°C, maintained at -0.095 MPa, and degassed for 2 hours to obtain a base glue.

[0072] The vinyl silicone oil is composed of the following components: 10,000 parts of DMC, 5 parts of vinyl double heads, 8 parts of vinyl ring bodies, and 0.15 parts of tetramethylammonium hydroxide catalyst; DMC, vinyl double heads, and vinyl ring bodies are added into a reaction kettle, the temperature is raised to 70°C, vacuumed and dehydrated for 1 hour, the vacuum is removed and the tetramethylammonium hydroxide catalyst is added, the temperature is raised to 115°C, and the polymerization is stirred for 2 hours. When the viscosity of the material remains unchanged, the temperature is raised to 190°C, the catalyst is broken at a constant temperature for 1 hour, and the low molecular weight is removed by vacuuming.

[0073] The fumed silica (hydrophilic type) is composed of the following components: 100 parts of silicon dioxide and 15 parts of hexamethyldisilazane; the speed of the agitator is controlled at 35 r / min, the temperature is 120° C., and the pressure is maintained at -0.095 MPa for 1 hour to obtain the fumed silica.

[0074] B. Weigh 100 parts of base rubber, 1.5 parts of platinum catalyst (mass fraction 3000×10 -6 ), add platinum catalyst to one part of the base rubber, mix well to obtain liquid silicone rubber, i.e. component a.

[0075] C. Add another equal portion of the base glue to the curing agent, put each component into the dispersant, disperse and stir for 30 minutes, mix evenly and filter to obtain component B.

[0076] The curing agent is composed of the following components: 10,000 parts of DMC, 2 parts of hydrogen-containing double heads, 3 parts of high-hydrogen silicone oil KF-99, 15 parts of hexamethyldisiloxane, and 1.3 parts of acidic cationic resin; the components are put into a mixer at a temperature of 65°C, refluxed for 2 hours, and then heated to 115°C, stirred and polymerized for 3 hours, the liquid is filtered and put into a reactor, and low molecular weight is removed under reduced pressure at 120°C to obtain the product.

[0077] D. The mass ratio of liquid silicone rubber to curing agent is 10:1.5. Mix component a and component b at a mass ratio of 10:0.5 for 1 hour to obtain printing silicone.

[0078] (3) Drawing board and film: determine the anti-slip webbing pattern and interval, and draw film, the film aperture is 160 mesh;

[0079] Plate making: Install the opened film on the printing plate;

[0080] Laying tape at the punching position: according to the width of the anti-slip webbing, set the corresponding infrared position, the sub-tape width is 2mm, the mother tape width is 10mm, to provide a contrast for the neatness of the anti-slip webbing. The tape is laid by machine positioning, the laying accuracy is plus or minus tolerance 0.3%, and the printing plate length is 45 meters;

[0081] Second printing: lay the printing plate, manually brush silicone, the thickness of the silicone part is 0.08mm, the printing interval is 30mm, brush it once to shape, brush it once to color, use a 180℃ dryer to dry it 10 times, stay for 10 seconds each time, and get the anti-slip webbing.

[0082] (4) The anti-slip webbing is made into a strip that matches the edge of the quilt core through a hot pressing process, and is set around the quilt core through a sewing process. The quilt core specification is 200cm*230cm.

[0083] Example 2

[0084] The difference between this embodiment and embodiment 1 is that:

[0085] (1) Sub-tape width 3mm, main tape 10mm.

[0086] (2) A. Preparation of base rubber: Weigh 100 parts by weight of vinyl silicone oil (viscosity 5000 mPa·s, vinyl mass fraction 0.16%), 5 parts of hexamethyldisilazane, 35 parts of fumed silica (hydrophilic type) (specific surface area 380 m 2 / g), 4 parts of hydroxy silicone oil (mass fraction 10%, viscosity 20-30mm 2 / s), 20 parts of vinyl MQ silicone resin (RH-S11), mixed, heated to 160°C, maintained at -0.095 MPa, and degassed for 2 hours to obtain a base glue.

[0087] D. The mass ratio of liquid silicone rubber to curing agent is 11:1.5. Mix component a and component b in a mass ratio of 11:1 for 1 hour to obtain printing silicone.

[0088] (3) Laying tape at the punching position: According to the width of the anti-slip webbing, set the corresponding infrared position. The sub-tape width is 3mm and the mother tape width is 10mm. This provides a contrast for the neatness of the anti-slip webbing. The tape is laid by machine positioning. The laying accuracy has a positive and negative tolerance of 0.3%. The length of the printing plate is 45 meters.

[0089] Example 3

[0090] The difference between this embodiment and embodiment 1 is that:

[0091] (1) Sub-tape width 3.5mm, master tape 10mm.

[0092] (2) A. Preparation of base rubber: Weigh 100 parts by weight of vinyl silicone oil (viscosity 5000 mPa·s, vinyl mass fraction 0.16%), 7 parts of hexamethyldisilazane, 45 parts of fumed silica (hydrophilic type) (specific surface area 380 m 2 / g), 6 parts of hydroxy silicone oil (mass fraction 10%, viscosity 20-30mm 2 / s), 25 parts of vinyl MQ silicone resin (RH-S11), mixed, heated to 160°C, maintained at -0.095 MPa, and degassed for 2 hours to obtain a base glue.

[0093] D. The mass ratio of liquid silicone rubber to curing agent is 12:1.5. Mix component a and component b in a mass ratio of 12:1.5 for 1 hour to obtain printing silicone.

[0094] (3) Laying tape at the punching position: According to the width of the anti-slip webbing, set the corresponding infrared position. The sub-tape width is 3.5mm and the mother tape width is 10mm. This provides a contrast for the neatness of the anti-slip webbing. The tape is laid by machine positioning. The laying accuracy has a positive and negative tolerance of 0.3%. The length of the printing plate is 45 meters.

[0095] Example 4

[0096] The difference between this embodiment and embodiment 1 is that:

[0097] (1) Sub-tape width 2.2 mm, master tape 10 mm, setting temperature 210°C.

[0098] (2) The thickness of the silicone part is 0.10 mm and the printing interval is 40 mm.

[0099] Example 5

[0100] The difference between this embodiment and embodiment 1 is that:

[0101] (1) Sub-tape width 2.2 mm, master tape 10 mm, setting temperature 220°C.

[0102] (2) The thickness of the silicone part is 0.12 mm and the printing interval is 50 mm.

[0103] Comparative Example 1

[0104] The difference between this comparative example and Example 1 is that no silicone part is printed on the ribbon.

[0105] Performance Testing

[0106] Friction coefficient: According to GB 10006-1988 "Test method for friction coefficient of plastic film and sheet", the friction coefficient of the anti-slip webbing of Examples 1, 4, 5 and Comparative Example 1 was tested using the MXD-02 friction coefficient tester developed and produced by Labthink. The test method is as follows:

[0107] The friction coefficient is the ratio of the friction force generated between the contact surfaces and the pressure acting vertically on the surface of the object when the fabric and the webbing are in contact. The specific implementation process is to use a fabric slider with a known pressure value to apply pressure to the webbing sample, so that the test sample and the friction surface slide relative to each other. By testing the force value of the sample before and during sliding, the static friction coefficient and dynamic friction coefficient of the test sample can be obtained.

[0108] Test samples: anti-slip webbings prepared according to Examples 1, 4, and 5, and the webbing of Comparative Example 1 without adding silicone.

[0109] Lay the webbing flat on the quilt cover fabric and stick 5 strips tightly to make a 63mm×100mm test specimen; the friction surface is the steel plate test bench of the testing equipment.

[0110] Test process:

[0111] (1) Randomly cut the webbing samples to make three specimens of 63 mm × 100 mm.

[0112] (2) Cut the fabric sample to be used into a sample of 63 mm × 100 mm and fix it on the slider with a fixing device.

[0113] (3) Use a connecting spring to connect the slider with the clamped sample to the force sensor of the equipment, and then place the slider on the steel plate test bench of the equipment without impact. The sliding direction of the sample should be parallel to the traction direction.

[0114] (4) Set the test parameters such as test speed and test stroke, click the test option, and the test starts.

[0115] (5) The sample is kept still on the test bench surface for 15 seconds. After the sample is in full contact with the test bench surface, relative sliding begins to occur automatically. The equipment automatically records the force value during the test and calculates and displays the static friction coefficient and dynamic friction coefficient of the sample after the test.

[0116] (6) Repeat steps (2) to (5) until all three samples have been tested.

[0117] The test results are shown in Table 1.

[0118] The experimental data and analysis are as follows:

[0119] Table 1 Friction coefficient of the anti-slip webbing of the embodiment and the webbing of the comparative example

[0120]

[0121]

[0122] As shown in Table 1, the static friction coefficient and dynamic friction coefficient between the ordinary webbing and the fabric in Comparative Example 1 are 0.417 and 0.388 respectively. After adding a silicone anti-skid layer to the surface of the webbing, the static friction coefficient and dynamic friction coefficient between the webbing and the fabric are improved. When the printing interval of the silicone is 30mm, the friction coefficient of the anti-skid webbing is increased by about 1.5 times; when the printing interval of the silicone is less than 30mm, the friction between the anti-skid webbing and the quilt cover is too large during actual use, and too high a silicone content will cause problems such as dust staining.

[0123] Therefore, the anti-slip webbing of the present application can effectively achieve the anti-slip effect through the anti-slip layer, and at the same time, the thickness of the silicone part and the printing interval are controlled in the present application to achieve the best anti-slip and dust-free effect. In the silicone screen printing process, the printing interval is preferably within 30 to 50 mm.

[0124] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. An anti-slip webbing, It is characterized in that It comprises a sub-belt and a main belt, wherein the sub-belt and the main belt are integrally formed, and the shrinkage rate of the sub-belt and the main belt is 3-5%; The sub-belt is printed with an anti-slip layer, which includes a plurality of silicone parts arranged at intervals. The silicone parts are made of liquid silicone rubber and a curing agent and are prepared by screen printing. The intervals between adjacent silicone parts are 30 to 50 mm.

2. The anti-slip webbing according to claim 1, It is characterized in that The material of the sub-belt and the main belt is one or more of nylon, vinylon, polyester, and polypropylene.

3. The anti-slip webbing according to claim 1, It is characterized in that The width of the sub-band is 2 to 5 mm; And / or, the width of the mother tape is 8 to 15 mm.

4. A method for preparing an anti-slip webbing, It is characterized in that The following steps are involved: (1) Weaving, high-temperature shaping, and pre-shrinking the raw yarn to prepare an integrally formed sub-belt and mother belt; (2) Using liquid silicone rubber and curing agent as raw materials to prepare printing silicone; (3) The printed silicone is brushed onto the sub-belt to form a plurality of silicone parts through a screen printing process, and the silicone parts are brushed with color to obtain the anti-slip webbing.

5. The preparation method according to claim 4, It is characterized in that In the step (1), the temperature of high temperature setting is 200-250°C.

6. The preparation method according to claim 4, It is characterized in that In the step (2), the mass ratio of liquid silicone rubber to curing agent is (10-15): (1.5-2).

7. The preparation method according to claim 4, It is characterized in that In the step (3), the thickness of the silicone portion is 0.08 to 0.12 mm.

8. The preparation method according to claim 4, It is characterized in that In the step (3), after brushing and coloring, multiple drying passes are performed, and each drying pass is stopped for 5 to 15 seconds.

9. A quilt core, It is characterized in that The invention comprises the anti-skid webbing according to any one of claims 1 to 3, or comprises the anti-skid webbing obtained by the preparation method according to any one of claims 4 to 8.

10. The quilt core according to claim 9, It is characterized in that The anti-slip webbing is made into a welt shape by a hot pressing process, and is arranged around the quilt core by a sewing process.