Combined type positive electrode material surface modification device and positive electrode material surface modification method

Through the combined cathode material surface modification device, the semi-permeable membrane and the ion diffusion drive of the multi-chamber concept are used to achieve uniform coating of the lithium-ion cathode material, solving the problem of performance deterioration caused by increased nickel content and improving the electrochemical performance. and safety, reducing cost and operational complexity.

CN118718935APending Publication Date: 2024-10-01SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310319848.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the nickel content of existing lithium-ion cathode materials increases, the cycle performance, thermal stability and safety deteriorate, leading to battery gas production and thermal runaway. Moreover, the existing surface coating method is costly, complex to operate and has low universality.

Method used

A combined cathode material surface modification device is used, using a semi-permeable membrane and a multi-chamber concept to drive the solute in the salt solution to slowly combine with the cathode material through ion diffusion to form a uniform coating material, combined with stirring and heat treatment, to achieve multiple surface modifications .

Benefits of technology

It improves the electrochemical performance and safety of the cathode material, reduces the modification cost, achieves uniform coating, is simple to operate, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718935A_ABST
    Figure CN118718935A_ABST
Patent Text Reader

Abstract

The invention relates to a combined type positive electrode material surface modification device and a positive electrode material surface modification method. The combined type device for modifying the surface of the positive electrode material comprises a reaction chamber; at least two ion chambers physically separated from the reaction chamber by an ion and / or molecule permeable membrane; and the stirring system is arranged at the bottom of the reaction chamber or / and the ion chamber. A semi-permeable membrane is used, solute molecules in a solution are selectively diffused to isolate macromolecular precipitates, a multi-chamber concept is introduced, so that ion chambers can be combined and used like building blocks, anions and cations are slowly combined to generate precipitation reaction or redox reaction to generate precipitates, and a coated substance is obtained; the types of coating substances are enriched, and single-weight or multi-coating can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to surface modification of lithium ion electrode materials, and in particular to a combined device for surface modification of lithium ion positive electrode materials and a method for surface modification of positive electrode materials, and belongs to the field of chemical energy storage batteries. Background Art

[0002] The rapid development of new energy vehicles has put forward higher requirements on the specific capacity and safety of positive electrode materials used in power batteries. Among the currently commercialized spinel, olivine and layered positive electrode materials, ternary layered positive electrode materials have attracted widespread attention due to their excellent specific capacity. Although the increase in nickel content can improve the specific capacity of the ternary positive electrode and reduce the cost, the cycle performance, thermal stability and safety of the ternary positive electrode material will deteriorate sharply with the increase in nickel content, which seriously restricts its practical application. The root cause of the above problems stems from the material properties of the high-nickel ternary positive electrode, including the dissolution of metal elements and the highly oxidizing Ni in the charged state. 4+ The side reaction with the electrolyte and the surface reconstruction occur, generating a high-impedance NiO phase and releasing active oxygen, leading to battery gas production and thermal runaway. At present, domestic and foreign scholars mainly coat the surface of ternary materials to inhibit the dissolution of transition metals and isolate highly active Ni 4+ Direct contact with the electrolyte solves the above shortcomings.

[0003] At present, the main methods for surface coating of positive electrode materials include coprecipitation, sol-gel, hydrothermal, chemical vapor deposition, atomic deposition, solid phase ball milling, etc., but there are still problems such as high cost and uneven coating. The precursor salts of sol-gel and hydrothermal methods are expensive and have low yields; chemical vapor deposition and atomic deposition methods have long processing time, strong toxicity and complex processes, and it is difficult to obtain a uniform coating layer by solid phase ball milling. In addition, the key to uniform coating lies in the regulation of the coating layer, and the key to the regulation of the coating layer lies in the slow deposition of the coating material on the surface of the coated material, and through diffusion control, the formation of separated two phases is avoided. At present, the uniform regulation strategies of the coating layer mainly include buffer solution, slow release of precipitation, catalyst assistance, charge interaction, etc. The above strategies can effectively realize the precise regulation of the coating layer and can significantly improve the performance of the positive electrode material, but there are also problems such as low universality and complex operation. Therefore, it is of great significance to develop a method that is easy to operate and uniformly coats the positive electrode material. Summary of the invention

[0004] In view of the above problems, the present invention provides a "combined" positive electrode material surface modification device and positive electrode material surface modification method.

[0005] In a first aspect, the present invention provides a combined positive electrode material surface modification device, comprising: Reaction chamber; at least two ion chambers physically separated from the reaction chamber by ion and / or molecule permeable membranes; And a stirring system is arranged at the bottom of the reaction chamber and / or the ion chamber.

[0006] In the present invention, osmotic pressure is formed based on the concentration difference on both sides of the membrane, and ion diffusion is used to modify the surface of the lithium ion positive electrode material, thereby improving its electrochemical performance and safety, reducing the modification cost, and improving the coating uniformity. In addition, the method is easy to combine ion chambers at will to achieve multiple material modifications on the positive electrode material. The method is easy to operate, has uniform coating, and is easy to scale up production.

[0007] Preferably, it further comprises a flow system respectively connected to the ion chamber and the reaction chamber; The flow system comprises: An ion chamber solution storage tank, and a first flow pump and a first flow pipeline connecting the ion chamber and the ion chamber solution storage tank; a reaction chamber suspension storage tank, and a second flow pump and a second flow pipeline connecting the reaction chamber and the reaction chamber suspension storage tank.

[0008] Preferably, the stirring system includes at least one of a magnetic stirring device, a mechanical stirring device and an ultrasonic stirring device.

[0009] Preferably, the ion chamber is arranged inside or outside the reaction chamber. Preferably, an external power supply device connecting the ion chamber and the reaction chamber is also included.

[0010] Preferably, the reaction chamber is used to contain a positive electrode material suspension, and the ion chamber is used to contain a salt solution; Alternatively, the reaction chamber is used to contain a salt solution, and the ion chamber is used to contain a positive electrode material suspension.

[0011] Preferably, the positive electrode material includes at least one of a lithium-treated positive electrode material and a positive electrode precursor material; the particle size of the positive electrode material is 1 to 100 μm; The lithium-ion positive electrode material comprises LiNi b Co c Mn 1-b-c O2 and LiNi m Co n Al 1-m-n At least one of O2, where 0≤b≤1, 0≤c≤1, 0≤m≤1, 0≤n≤1; The positive electrode precursor material includes Ni (1-y-z) Co y Mn z (OH)2 and Ni (1-a-d) Co a Al dAt least one of (OH)2, wherein 0≤y≤1, 0≤z≤1, 0≤a≤1, 0≤d≤1.

[0012] Preferably, the solute of the salt solution is selected from at least one of KOH, NaOH, LiOH, (NH4)2HPO4, NH4 H2PO4, H3PO4, NH3·H2O, LiF, NaF, KF, Cr(NO3)3, Al(NO3)3, Al2(SO4)3, AlCl3, MnCl3, Mn(NO3)2, Co(NO3)3, Co2(SO4)3, Fe(NO3)3, Fe2(SO4)3, FeCl3, Cr(NO3)3, Cr2(SO4)3, CrCl3, Zr(NO3)4, ZrO(NO3)2, ZrCl4, Zn(NO3)3, Na2SnO3, Zn(NO3)2, Ce(NO3)3, Sr(NO3)3, Mg(NO3)2, and TiBr4; wherein the solute undergoes a precipitation reaction or an oxidation-reduction reaction with the positive electrode material to generate a precipitate; The solvent of the salt solution includes at least one of distilled water, methanol, ethanol, isopropanol, n-butanol, isobutanol, cycloethanol, acetone, cyclohexanone, glycerol and ethyl acetate; The concentration of the salt solution is 0.01 mol / L to 10 mol / L.

[0013] Preferably, the solvent of the positive electrode material suspension includes at least one of distilled water, methanol, ethanol, isopropanol, n-butanol, isobutanol, cycloethanol, acetone, cyclohexanone, glycerol and ethyl acetate.

[0014] In a second aspect, the present invention provides a method for surface modification of a positive electrode material, comprising: (1) adding a positive electrode material suspension into an ion chamber and adding a salt solution into a reaction chamber; or, adding a positive electrode material suspension into a reaction chamber and adding a salt solution into an ion chamber; or, the reaction chamber is used to contain a salt solution and the ion chamber is used to contain a positive electrode material suspension; wherein the ion chamber and the reaction chamber are physically separated by an ion and / or molecule permeable membrane; (2) using the osmotic pressure generated by the concentration difference of ions and / or molecules on both sides of the permeable membrane as a driving force, and utilizing the property of the permeable membrane of ions and / or molecules to pass through ions and molecules but block macromolecules, so that the solute in the salt solution diffuses, so that the solute in the salt solution reacts with the positive electrode material to produce a precipitation reaction or an oxidation-reduction reaction to generate a precipitate, thereby forming a coating material on the surface of the positive electrode material or in the pores of its particles, and then separating and drying to obtain a positive electrode material with the coating material distributed on the surface; (3) heat-treating the positive electrode material with the coating material distributed on the surface to obtain a surface-modified positive electrode material. Preferably, the reaction device used is the above-mentioned combined positive electrode material surface modification device, which has high efficiency and can realize industrial and large-scale preparation.

[0015] In the present invention, a semipermeable membrane is used to isolate the coating or positive electrode material from the solute in the salt solution, so that the two are slowly combined to produce a precipitation reaction or an oxidation-reduction reaction to generate a precipitate, thereby obtaining a coated material. Or an external power supply is used to make the ion migration faster under the electric field. In addition, the concept of multiple chambers (not limited to one reaction chamber + one ion chamber) is introduced, so that the ion chambers can be used in combination like building blocks, enriching the types of coated materials, and achieving single or multiple coatings. Since the process of generating precipitation is controlled by the diffusion rate of ions in the semipermeable membrane, the supersaturation of the coated material in the reaction chamber system is always maintained at a low level, inhibiting the process of forming separated particles between the coated material and the positive electrode material, promoting its heterogeneous nucleation and growth on the surface of the positive electrode material, and realizing its uniform deposition on the surface of the positive electrode material particles under stirring, so as to achieve the purpose of coating or covering. The surface coating of the positive electrode material, primary particle grain boundary filling, surface element doping and other multiple surface modifications are achieved through subsequent heat treatment to improve the stability of the positive electrode material.

[0016] Preferably, the solid content of the positive electrode material in the positive electrode material suspension is 2wt% to 40wt%. The temperature of the precipitation reaction or the redox reaction is 20 to 100° C., and the time is 0.5 to 36 hours.

[0017] Preferably, the coating material in the positive electrode material with a coating material distributed on the surface includes at least one or more of Mn(OH)2, Co(OH)2, AlPO4, Mn3(PO4)2, Co3(PO4)2, Mn3(PO4)2, LaPO4, FePO4, Li3PO4, AlF3, LiAlO2, Li2ZrO3, Li4Ti5O12, Al2O3, TiO2, ZrO2, ZnO, Al(OH)3, Li2SnO4, Li3WO4, CoSnO4 and Zr(OH)4; The mass of the coating material is 0.1% to 10% of the mass of the positive electrode material.

[0018] Preferably, when the positive electrode material is a lithiated positive electrode material, the heat treatment temperature is 100 to 800° C., the heat treatment time is 2 to 10 hours, and the heat treatment atmosphere is pure oxygen or air.

[0019] Preferably, when the positive electrode material is a positive electrode precursor material, the obtained positive electrode material with a coating material distributed on the surface and lithium oxide are mixed and sintered to obtain a surface-modified positive electrode material; the lithium-containing oxide includes at least one of LiOH·H2O, LiNO3, Li2CO3, Li2O and Li2O2, and the molar ratio of the positive electrode material with a coating material distributed on the surface to the lithium-containing oxide is 1:(1.01~1.10).

[0020] Preferably, the sintering process includes: one-step sintering or two-step sintering; the atmosphere of the sintering process is pure oxygen or air; The one-step sintering includes: a sintering temperature of 600 to 850°C, a heat preservation time of 10h to 20h, and preferably a heating rate of 2 to 5°C / min for the one-step sintering; The two-step sintering includes: the first step sintering temperature is 300-500°C, and the holding time is 2h-4h; the second step sintering temperature is 700-850°C, and the holding time is 10h-20h; preferably, the heating rate of the two-step sintering is 2-5°C / min.

[0021] In a third aspect, the present invention provides a surface-modified positive electrode material prepared according to the above-mentioned surface modification method.

[0022] In a fourth aspect, a lithium-ion battery comprises: a negative electrode material, the surface-modified positive electrode material, and a separator or solid electrolyte for separating the surface-modified positive electrode material from the negative electrode material; Preferably, the separator includes a polypropylene separator (PP) or a celgard separator, and the solid electrolyte includes a garnet solid electrolyte, a NASICON solid electrolyte, a sulfide solid electrolyte and a perovskite solid electrolyte; Preferably, the negative electrode material is graphite, silicon carbon, silicon dioxide, silicon alloy, tin oxide, metallic lithium or lithium alloy.

[0023] Beneficial effects: The present invention uses a semipermeable membrane to selectively diffuse solute molecules in the solution and isolate macromolecular precipitates, and introduces the concept of multiple chambers, so that ion chambers can be used in combination like building blocks, so that anions and cations slowly combine to produce precipitation reactions or oxidation-reduction reactions to produce precipitation, thereby obtaining coated materials, enriching the types of coated materials, and achieving single or multiple coatings. The device and method keep the supersaturation of the coated material in the positive electrode material mixed liquid system at a low level, inhibit the process of the coated material forming particles separated from the positive electrode material due to homogeneous nucleation and growth, and promote heterogeneous nucleation and growth of the coated material on the surface of the positive electrode material, thereby achieving uniform coating on the surface of the positive electrode material under the action of the solid-liquid shear force provided by the stirring action; The present invention performs an in-situ reaction on the surface of the positive electrode material to achieve uniform coating, and can achieve multiple surface modifications such as surface coating of the positive electrode material, primary particle grain boundary filling, surface element doping, etc. through a heat treatment step, thereby further improving the stability of the active material under the synergistic effect of various factors; The basic driving force of the coating of the present invention comes from ion diffusion, and the principle is simple, the required drugs and solvents are cheap and easy to obtain, and the environment is friendly. Therefore, the present invention has strong versatility, convenient operation, green environmental protection, and high industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The device for surface modification of positive electrode materials in the present invention, in which: 1-reaction chamber, 2-ion chamber A, 3-ion chamber B, 4-semipermeable membrane, 5-stirring device; Figure 2 is an infrared spectrum of a positive electrode material, wherein the positive electrode material includes surface-modified Examples 1-4 and non-surface-modified Comparative Example 1; Figure 3 is an X-ray diffraction (XRD) diagram of the positive electrode material, wherein the positive electrode material includes Examples 1-4 with surface modification and Comparative Example 1 without surface modification Figure 4 1 is a scanning electron micrograph (SEM) of the positive electrode material, wherein the material includes the modified Example 1 and Example 2 and the Comparative Example 1 without surface modification. Figure 5 (A)- Figure 5 (C) is a comparison chart of the cycle stability of positive electrode materials, wherein the materials include Examples 1-3 with surface modification and Comparative Example 1 without surface modification; Figure 6 It is a rate comparison diagram of positive electrode materials, and the materials include Examples 1-2 with surface modification and Comparative Example 1 without surface modification. DETAILED DESCRIPTION

[0025] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0026] In the present disclosure, the device for surface modification of positive electrode materials based on ion exchange membrane includes a reaction chamber and an ion chamber, and a semipermeable membrane separating the reaction chamber and the ion chamber; wherein a stirring device is provided inside the reaction chamber. When the device of the present invention is used, the reaction chamber mixed solution and the ion chamber solution are first prepared, and then the reaction chamber mixed solution and the ion chamber solution are respectively injected into the reaction chamber and the ion chamber, and the stirring is always kept on during the coating.

[0027] In the present invention, an anion substance solution and a cation substance solution are configured, and the positive electrode material suspension and the salt solution constituting the coating material are placed in different ion chambers and reaction chambers respectively, and the positive electrode material is placed in the reaction chamber. A semipermeable membrane is used to isolate the reaction chamber and the ion chamber, and the diffusion of the solute in the semipermeable membrane is controlled so that it slowly combines with the positive electrode material, and a precipitation reaction or an oxidation-reduction reaction occurs to generate a precipitate, thereby obtaining the coating material on the surface of the positive electrode material or in the particle pores. The obtained modified positive electrode material is separated, dried, and heat-treated to obtain a surface-modified positive electrode material. The following is a detailed description of the surface modification method of the positive electrode material using the device.

[0028] Prepare an ion chamber solution. Dissolve a soluble substance that can provide ions of the coating material in a solvent to obtain an ion chamber solution. Optionally, disperse the positive electrode material in an aqueous solution or a salt solution to obtain a reaction chamber mixture. More preferably, the reaction chamber mixture is injected into the reaction chamber, and the ion chamber solution is injected into each ion chamber respectively. The positive electrode material is then coated, and after the coating is completed, the reaction chamber mixture is centrifuged and dried to obtain the coated positive electrode material. During the coating process, the reaction chamber is always stirred. The centrifugal speed can be 1000 to 8000 rpm, and the centrifugal time can be 1 to 8 min. Drying is vacuum drying, the drying temperature is 20 to 150°C, and the drying time is 24 to 48 hours.

[0029] When the coated material is a lithiated positive electrode material, the obtained coated positive electrode material is subjected to heat treatment. After the heat treatment process, the positive electrode material recovers its electrochemical activity, and the coating material coated on the surface of the positive electrode material will achieve surface coating and / or element doping of the positive electrode material through heat treatment.

[0030] When the coated material is a positive electrode precursor material, the obtained coated positive electrode precursor material is mixed with a lithium-containing compound such as LiOH·H2O at a molar ratio of 1:x (1.01-1.10) (for example, ball milling is performed to mix thoroughly), and then sintered. During the sintering process, the positive electrode precursor material and the lithium-containing oxide undergo a high-temperature solid-phase reaction to form a layered positive electrode material, and the coating material coated on the surface of the positive electrode precursor material will achieve surface coating and / or element doping of the positive electrode material at high temperature.

[0031] In the present invention, the positive electrode material includes a lithium-containing positive electrode material and a positive electrode precursor material. The particle size of the positive electrode material is 0.1 to 100 μm. In an optional embodiment, the positive electrode material is dispersed into an aqueous solution and / or a salt solution to obtain a mixed solution by ultrasonic dispersion, with an ultrasonic power of 100 to 500 W and an ultrasonic time of 1 to 180 min.

[0032] In general, the positive electrode material is dispersed in the reaction chamber solution of the above-mentioned "combined" positive electrode material surface modification device, and the osmotic pressure generated by the concentration difference on both sides of the membrane is used as the driving force. The semipermeable membrane can pass ions and molecules but block large molecules. The solute is diffused on both sides of the membrane, and the solute is combined in the reaction chamber to produce a precipitation reaction or an oxidation-reduction reaction to generate a precipitate, thereby forming a coating substance on the surface of the positive electrode material or in the particle pores of the positive electrode material. After separation and drying, the positive electrode material with the coating substance distributed on the surface is obtained.

[0033] In the present invention, the lithium-ion battery comprises: a positive electrode, a negative electrode and a diaphragm or solid electrolyte for separating the positive and negative electrode materials. The positive electrode material of the battery is the surface-modified positive electrode material based on the surface modification of the ion exchange membrane described in the present invention. The diaphragm or solid electrolyte includes PP, celgard, garnet-type solid electrolyte, NASICON-type solid electrolyte, sulfide solid electrolyte, perovskite-type solid electrolyte. The negative electrode is graphite, silicon carbon, silicon dioxide, silicon alloy, tin oxide, metallic lithium or lithium alloy.

[0034] Specifically, the surface-modified positive electrode material is uniformly mixed with conductive carbon and a binder to form a slurry and coated on an aluminum foil, and a cutting machine is used to cut the dried aluminum foil loaded with the slurry into small discs for use as the positive electrode. A full battery is assembled and tested and characterized.

[0035] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples in a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0036] Example 1 Assemble as Figure 1 The semi-permeable membrane used in the device is a regenerated cellulose membrane with a maximum permeable molecular weight of 14000 g / mol. Before use, it is soaked in deionized water at 80°C and boiled for 1 hour to enable it to have ion permeability.

[0037] The surface modification method of the positive electrode material in this embodiment 1 includes: Step 1): 4g of nickel-cobalt-manganese ternary precursor material (Ni 0.83 Co 0.12 Mn 0.05(OH)2) was mixed with deionized water in a mass ratio of 1:20, and the mixed solution was dispersed by ultrasound for 10 min to obtain a reaction chamber mixed solution; Step 2): dissolve Co(NO3)2 in water to prepare a 0.1 mol / L Co(NO3)2 solution as solution A; Step 3): dissolve (NH4)2HPO4 in water to prepare a 0.1 mol / L (NH4)2HPO4 solution as solution B; Step 4): Inject the reaction chamber mixed solution obtained in step 1) and the solution obtained in step 2) into the reaction chamber, ion chamber A and ion chamber B respectively, keep the stirring of the reaction chamber always on, and perform surface coating on the precursor, the coating time is 6 hours, and the coating temperature is 25°C. After the coating is completed, the reaction chamber mixed solution is centrifuged at a centrifugal speed of 3000rpm and a centrifugal time of 3min. The solid material obtained by centrifugation is dried in a vacuum oven at a drying temperature of 80°C and a drying time of 24h. A ternary positive electrode precursor material coated with surface Co3(PO4)2 is obtained; Step 5): The coated ternary precursor material obtained in step 4) is mixed with LiOH·H2O in a molar ratio of 1:1.05 by ball milling, and then sintered in two steps under a pure oxygen atmosphere: the first step is sintered at a temperature of 400°C and a holding time of 2 hours; the second step is sintered at a temperature of 750°C and a holding time of 12 hours; the heating rate is 3°C / min. A surface-modified positive electrode material is obtained.

[0038] The surface modified positive electrode material obtained in Example 1 was used as the positive electrode active material to prepare the electrode and assemble the button battery. Assembly and testing of CR2025 button battery: The surface modified positive electrode material, conductive carbon (Super P:VGCF=1:1), and polyvinylidene fluoride (PVDF) were made into a slurry according to a mass ratio of 8:1:1 and coated on aluminum foil. The dried aluminum foil loaded with the slurry was cut into small discs with a diameter of 1.2 cm by a cutting machine for use as the positive electrode, a metal lithium sheet was used as the negative electrode, Celgard was used as the diaphragm, and a 1M carbonate solution was used as the electrolyte (wherein the solvent was a mixed solution of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1, and the solute was LiPF6), and a CR2025 button battery was assembled in an argon glove box.

[0039] Example 2 The surface modification method of the positive electrode material in this embodiment 2 includes: Step 1): 4g of nickel-cobalt-manganese ternary precursor material (Ni 0.83 Co 0.12 Mn 0.05(OH)2) was mixed with deionized water in a mass ratio of 1:20, and the mixed solution was dispersed by ultrasound for 10 min to obtain a reaction chamber mixed solution; Step 2): dissolve Fe(NO3)3 in water to prepare a 0.1 mol / L Fe(NO3)3 solution as solution A; Step 3): dissolve (NH4)2HPO4 in water to prepare a 0.1 mol / L (NH4)2HPO4 solution as solution B; Step 4): Inject the reaction chamber mixed solution obtained in step 1) and the solution obtained in step 2) into the reaction chamber, ion chamber A and ion chamber B respectively, keep the stirring of the reaction chamber always on, and perform surface coating on the precursor, the coating time is 6 hours, and the coating temperature is 25°C. After the coating is completed, the reaction chamber mixed solution is centrifuged at a centrifugal speed of 3000rpm and a centrifugal time of 3min. The solid material obtained by centrifugation is dried in a vacuum oven at a drying temperature of 80°C and a drying time of 24h. A ternary positive electrode precursor material with surface FePO4 coating is obtained; Step 5): The coated ternary precursor material obtained in step 4) is mixed with LiOH·H2O in a molar ratio of 1:1.05 by ball milling, and then sintered in two steps under a pure oxygen atmosphere: the first step is sintered at a temperature of 400°C and a holding time of 2 hours; the second step is sintered at a temperature of 750°C and a holding time of 12 hours; the heating rate is 3°C / min. A surface-modified positive electrode material is obtained.

[0040] The surface modified positive electrode material obtained in Example 2 was prepared into an electrode and assembled into a button cell, and the preparation process was the same as that in Example 1.

[0041] Example 3 The surface modification method of the positive electrode material in this embodiment 3 includes: Step 1): 4g of nickel-cobalt-manganese ternary precursor material (Ni 0.83 Co 0.12 Mn 0.05 (OH)2) was mixed with deionized water in a mass ratio of 1:20, and the mixed solution was dispersed by ultrasound for 10 min to obtain a reaction chamber mixed solution; Step 2): dissolve La(NO3)3 in water to prepare a 0.1 mol / L La(NO3)3 solution as solution A; Step 3): dissolve (NH4)2HPO4 in water to prepare a 0.1 mol / L (NH4)2HPO4 solution as solution B; Step 4): Inject the reaction chamber mixed solution obtained in step 1) and the solution obtained in step 2) into the reaction chamber, ion chamber A and ion chamber B respectively, keep the stirring of the reaction chamber always on, and perform surface coating on the precursor, the coating time is 6 hours, and the coating temperature is 25°C. After the coating is completed, the reaction chamber mixed solution is centrifuged at a centrifugal speed of 3000rpm and a centrifugal time of 3min. The solid material obtained by centrifugation is dried in a vacuum oven at a drying temperature of 80°C and a drying time of 24h. A ternary positive electrode precursor material coated with LaPO4 on the surface is obtained; Step 5): The coated ternary precursor material obtained in step 4) is mixed with LiOH·H2O in a molar ratio of 1:1.05 by ball milling, and then sintered in two steps under a pure oxygen atmosphere: the first step is sintered at a temperature of 400°C and a holding time of 2 hours; the second step is sintered at a temperature of 750°C and a holding time of 12 hours; the heating rate is 3°C / min. A surface-modified positive electrode material is obtained.

[0042] The surface modified positive electrode material obtained in Example 3 was prepared into an electrode and assembled into a button cell, and the preparation process was the same as that in Example 1.

[0043] Example 4 The surface modification method of the positive electrode material in this embodiment 4 includes: Step 1): 4g of nickel-cobalt-manganese ternary precursor material (Ni 0.83 Co 0.12 Mn 0.05 (OH)2) was mixed with deionized water in a mass ratio of 1:20, and the mixed solution was dispersed by ultrasound for 10 min to obtain a reaction chamber mixed solution; Step 2): dissolve Sr(NO3)2 in water to prepare a 0.1 mol / L Sr(NO3)2 solution as solution A; Step 3): dissolve Na2SnO4 in water to prepare a 0.1 mol / L Na2SnO4 solution as solution B; Step 4): Inject the reaction chamber mixed solution obtained in step 1) and the solution obtained in step 2) into the reaction chamber, ion chamber A and ion chamber B respectively, keep the stirring of the reaction chamber always on, and perform surface coating on the precursor, the coating time is 6 hours, and the coating temperature is 25°C. After the coating is completed, the reaction chamber mixed solution is centrifuged at a centrifugal speed of 3000rpm and a centrifugal time of 3min. The solid material obtained by centrifugation is dried in a vacuum oven at a drying temperature of 80°C and a drying time of 24h. A ternary positive electrode precursor material coated with SrSnO4 on the surface is obtained; Step 5): The coated ternary precursor material obtained in step 4) is mixed with LiOH·H2O in a molar ratio of 1:1.05 by ball milling, and then sintered in two steps under a pure oxygen atmosphere: the first step is sintered at a temperature of 400°C and a holding time of 2 hours; the second step is sintered at a temperature of 750°C and a holding time of 12 hours; the heating rate is 3°C / min. A surface-modified positive electrode material is obtained.

[0044] The surface modified positive electrode material obtained in Example 4 was prepared into an electrode and assembled into a button battery, and the process was the same as in Example 1.

[0045] Comparative Example 1 The nickel-cobalt-manganese ternary precursor material (Ni 0.83 Co 0.12 Mn 0.05 (OH)2) was directly mixed with LiOH·H2O in a molar ratio of 1:1.05 by ball milling, and then sintered in two steps under a pure oxygen atmosphere: the first step was sintered at 400°C for 2 hours; the second step was sintered at 750°C for 12 hours; the heating rate was 3°C / min. A surface-modified positive electrode material was obtained.

[0046] The surface modified positive electrode material obtained in this comparative example 1 was prepared into an electrode and assembled into a button cell, and the process was the same as that in Example 1.

[0047] Figure 1 A device for modifying the surface of a positive electrode is shown respectively. The device is mainly divided into a reaction chamber, an ion chamber, a semipermeable membrane, and a stirring or flow system. When in use, the anions and cations constituting the coating material are placed in the ion chamber respectively, and the positive electrode material is placed in the reaction chamber. The components in the accompanying drawings are not drawn to scale, but the focus is on the principles of the given exemplary embodiments and devices. It should be understood that the present application is not limited to the details or methods set forth in the specification or shown in the accompanying drawings. It should also be understood that the terms used in this disclosure are for descriptive purposes only and should not be considered restrictive.

[0048] Figure 2 The infrared spectra of the positive electrode precursors are shown, and the positive electrode precursors include surface-modified Examples 1-3 and non-surface-modified Comparative Example 1. Figure 2 It can be seen that compared with Comparative Example 1, Examples 1-3 have vibration absorption peaks of PO bonds, indicating that phosphates have been successfully introduced, indicating that the method of the present invention can successfully introduce deposition materials.

[0049] Figure 3The X-ray diffraction (XRD) diagram of the positive electrode is shown, and the positive electrode materials include Examples 1-4 that have been surface modified and Comparative Example 1 that has not been surface modified. All diffraction peaks match well with the typical hexagonal a-NaFeO2 structure (JCPDF card number 01-089-4533, space group R-3m), which represents the main phase of NCM. The a-NaFeO2 type crystal structure is an ordered rock salt type, with Li and Me ions occupying alternating (111) layers. NCM has a layered NaFeO2 structure, R-3m space group, with alternating layers formed by LiO6 and MO6 octahedra. From Figure 3 It can be seen that the main diffraction peaks of all samples match well with the JCPDF card with R-3m space group, which indicates that the surface modification by the method of the present invention does not change the layered structure of the NCM material.

[0050] Figure 4 The scanning electron micrograph (SEM) of the positive electrode material is shown, and the positive electrode material includes Examples 1-2 which have been surface-modified and Comparative Example 1 which has not been surface-modified. Figure 4 It can be seen that both the modified positive electrode material and the unmodified positive electrode material are secondary particles formed by the dense stacking of primary particles, but the modified positive electrode material has a special surface morphology, which is beneficial to improving the rate performance of the positive electrode material.

[0051] Figure 5 (A)-(C) compare the cycle performance of the positive electrode materials obtained in Example 1, Example 2 and Example 3 after surface modification and Comparative Example 1 without surface modification. The results show that the cycle performance of the positive electrode material surface modified by the method of the present invention is significantly improved. After cycling under the same conditions, the capacity retention rate of the positive electrode material using the surface modification is significantly higher than that of the positive electrode material without surface modification, indicating that the surface modification implemented by the present invention can significantly improve the cycle stability of the positive electrode material. The effectiveness of the device and method of the present invention is fully demonstrated.

[0052] Figure 6 A rate comparison diagram of positive electrode materials is shown, and the materials include Example 1 and Example 2 which have been surface modified, and Comparative Example 1 which has not been surface modified. The results show that the rate performance of the nickel-cobalt-manganese positive electrode material after surface modification based on the device and method of the present invention is significantly improved, and more capacity can be released under high rate conditions, which fully demonstrates the effectiveness of the device and method of the present invention.

[0053] Comparative Example 1 It is suggested to refer to Example 1 and add a second solute that can react with the solute in the salt solution in the positive electrode material suspension as Comparative Example 1. Add corresponding parameters and data for comparison with Example 1.

[0054] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A combined positive electrode material surface modification device, characterized in that: include: Reaction chamber; at least two ion chambers physically separated from the reaction chamber by ion and / or molecule permeable membranes; And a stirring system is arranged at the bottom of the reaction chamber and / or the ion chamber.

2. The combined positive electrode material surface modification device according to claim 1, characterized in that: Also included are flow systems respectively connected to the ion chamber and the reaction chamber; The flow system comprises: an ion chamber solution storage tank, and a first flow pump and a first flow conduit connecting the ion chamber and the ion chamber solution storage tank; A reaction chamber suspension liquid storage tank, and a second flow pump and a second flow pipeline connecting the reaction chamber and the reaction chamber suspension liquid storage tank.

3. The combined positive electrode material surface modification device according to claim 1, characterized in that: The stirring system includes at least one of a magnetic stirring device, a mechanical stirring device and an ultrasonic stirring device.

4. The combined positive electrode material surface modification device according to claim 1, characterized in that: The ion chamber is arranged inside or outside the reaction chamber.

5. The combined positive electrode material surface modification device according to claim 1, characterized in that: Also included is an external power supply device connecting the ion chamber and the reaction chamber.

6. The combined positive electrode material surface modification device according to claim 1, characterized in that: The ion and / or molecule permeable membrane comprises at least one of an organic membrane and an inorganic membrane; The organic membrane includes at least one of semipermeable membranes made of regenerated cellulose membrane, polyamide membrane, etc.; The inorganic membrane includes at least one of a ceramic semipermeable membrane, a metal semipermeable membrane, a metal oxide semipermeable membrane, a porous glass semipermeable membrane, a zeolite semipermeable membrane, and an inorganic polymer semipermeable membrane.

7. The combined positive electrode material surface modification device according to claim 1, characterized in that: The reaction chamber is used to contain a positive electrode material suspension, and the ion chamber is used to contain a salt solution; Alternatively, the reaction chamber is used to contain a salt solution, and the ion chamber is used to contain a positive electrode material suspension.

8. The combined positive electrode material surface modification device according to claim 7, characterized in that: The positive electrode material includes at least one of a lithium-treated positive electrode material and a positive electrode precursor material; the particle size of the positive electrode material is 1 to 100 μm; The lithium-ion positive electrode material comprises LiNi b Co c Mn 1-b-c O2 and LiNi m Co n Al 1-m-n At least one of O2, where 0≤b≤1, 0≤c≤1, 0≤m≤1, 0≤n≤1; The positive electrode precursor material includes Ni (1-y-z) Co y Mn z (OH)2 and Ni (1-a-d) Co a Al d At least one of (OH)2, wherein 0≤y≤1, 0≤z≤1, 0≤a≤1, 0≤d≤1.

9. The combined positive electrode material surface modification device according to claim 7, characterized in that: The solute of the salt solution is selected from at least one of KOH, NaOH, LiOH, (NH4)2HPO4, NH4 H2PO4, H3PO4, NH3·H2O, LiF, NaF, KF, Cr(NO3)3, Al(NO3)3, Al2(SO4)3, AlCl3, MnCl3, Mn(NO3)2, Co(NO3)3, Co2(SO4)3, Fe(NO3)3, Fe2(SO4)3, FeCl3, Cr(NO3)3, Cr2(SO4)3, CrCl3, Zr(NO3)4, ZrO(NO3)2, ZrCl4, Zn(NO3)3, Na2SnO3, Zn(NO3)2, Ce(NO3)3, Sr(NO3)3, Mg(NO3)2, and TiBr4; wherein the solute undergoes a precipitation reaction or an oxidation-reduction reaction with the positive electrode material to generate a precipitate; The solvent of the salt solution includes at least one of distilled water, methanol, ethanol, isopropanol, n-butanol, isobutanol, cycloethanol, acetone, cyclohexanone, glycerol and ethyl acetate; The concentration of the salt solution is 0.01 mol / L to 10 mol / L.

10. The combined positive electrode material surface modification device according to any one of claims 7 to 9, characterized in that: The solvent of the positive electrode material suspension includes at least one of distilled water, methanol, ethanol, isopropanol, n-butanol, isobutanol, cycloethanol, acetone, cyclohexanone, glycerol and ethyl acetate.

11. A method for surface modification of a positive electrode material, characterized in that: include: (1) adding a positive electrode material suspension into an ion chamber and adding a salt solution into a reaction chamber; or, adding a positive electrode material suspension into a reaction chamber and adding a salt solution into an ion chamber; or, the reaction chamber is used to contain a salt solution and the ion chamber is used to contain a positive electrode material suspension; wherein the ion chamber and the reaction chamber are physically separated by an ion and / or molecule permeable membrane; (2) using the osmotic pressure generated by the concentration difference of ions and / or molecules on both sides of the permeable membrane as a driving force, and utilizing the property of the permeable membrane to pass ions and molecules but block macromolecules, so that the solute in the salt solution diffuses, so that the solute in the salt solution reacts with the positive electrode material to produce a precipitation reaction or an oxidation-reduction reaction to generate a precipitate, thereby forming a coating material on the surface of the positive electrode material or in the pores of its particles, and then separating and drying to obtain a positive electrode material with the coating material distributed on the surface; (3) The positive electrode material with the coating material distributed on the surface is heat-treated to obtain a surface-modified positive electrode material.

12. The surface modification method according to claim 11, characterized in that: The reaction device used is a combined positive electrode material surface modification device as described in any one of claims 1-11.

13. The surface modification method according to claim 11, characterized in that: The solid content of the positive electrode material in the positive electrode material suspension is 2wt% to 40wt%; The temperature of the precipitation reaction or the redox reaction is 20 to 100° C., and the time is 0.5 to 36 hours.

14. The surface modification method according to claim 11, characterized in that: The positive electrode material having a coating material distributed on the surface thereof includes at least one or more of Mn(OH)2, Co(OH)2, AlPO4, Mn3(PO4)2, Co3(PO4)2, Mn3(PO4)2, LaPO4, FePO4, Li3PO4, AlF3, LiAlO2, Li2ZrO3, Li4Ti5O12, Al2O3, TiO2, ZrO2, ZnO, Al(OH)3, Li2SnO4, Li3WO4, CoSnO4 and Zr(OH)4; The mass of the coating material is 0.1% to 10% of the mass of the positive electrode material.

15. The surface modification method according to any one of claims 11 to 14, characterized in that: When the positive electrode material is a lithiated positive electrode material, the heat treatment temperature is 100 to 800° C., the heat treatment time is 2 to 10 hours, and the heat treatment atmosphere is pure oxygen or air.

16. The surface modification method according to any one of claims 11 to 14, characterized in that: When the positive electrode material is a positive electrode precursor material, the obtained positive electrode material with a coating material distributed on the surface and lithium oxide are mixed and sintered to obtain a surface-modified positive electrode material; the lithium-containing oxide includes at least one of LiOH·H2O, LiNO3, Li2CO3, Li2O and Li2O2, and the molar ratio of the positive electrode material with a coating material distributed on the surface to the lithium-containing oxide is 1: (1.01-1.10).

17. The surface modification method according to claim 16, characterized in that: The sintering process includes: one-step sintering or two-step sintering; the atmosphere of the sintering process is pure oxygen or air; The one-step sintering includes: a sintering temperature of 600 to 850°C, a heat preservation time of 10h to 20h, and preferably a heating rate of 2 to 5°C / min for the one-step sintering; The two-step sintering includes: the first step sintering temperature is 300-500°C, and the holding time is 2h-4h; the second step sintering temperature is 700-850°C, and the holding time is 10h-20h; preferably, the heating rate of the two-step sintering is 2-5°C / min.

18. A surface-modified positive electrode material prepared by the surface modification method according to any one of claims 11 to 17.

19. A lithium ion battery comprising: A negative electrode material, a surface-modified positive electrode material as claimed in claim 18, and a separator or a solid electrolyte for separating the surface-modified positive electrode material and the negative electrode material; Preferably, the separator includes a polypropylene separator (PP) or a celgard separator, and the solid electrolyte includes a garnet solid electrolyte, a NASICON solid electrolyte, a sulfide solid electrolyte and a perovskite solid electrolyte; Preferably, the negative electrode material is graphite, silicon carbon, silicon dioxide, silicon alloy, tin oxide, metallic lithium or lithium alloy.