Method for improving photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO

By etching and modifying Cu2MoS4 nanosheets and combining them with ZnO nanoparticles to form Cu2MoS4/ZnO composite materials, the problem of poor photocatalytic hydrogen evolution performance of Cu2MoS4/ZnO photocatalytic materials is solved, and its efficiency and stability are significantly improved.

CN118719097AInactive Publication Date: 2024-10-01HARBIN UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410743487.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The Cu2MoS4/ZnO photocatalytic material has low visible light utilization rate and fast photogenerated carrier recombination rate, resulting in its poor photocatalytic hydrogen evolution performance.

Method used

By etching and modifying the Cu2MoS4 nanosheets to increase the exposed edge area, and combining the in-situ loading of ZnO nanoparticles to form a Cu2MoS4/ZnO composite material, the heterojunction structure is used to promote the transfer and separation of photogenerated electrons and holes.

Benefits of technology

The photocatalytic hydrogen evolution performance of the Cu2MoS4/ZnO composite material is significantly improved, the hydrogen evolution efficiency is increased by about 103%, and the stability and efficiency of the material are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719097A_ABST
    Figure CN118719097A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, and relates to the field of photocatalytic composite materials. The invention provides a method for solving the problem of poor photocatalytic hydrogen evolution performance caused by low visible light utilization rate and high photon-generated carrier recombination rate of pure Cu2MoS4. The method comprises the following steps: 1, preparing a Cu2MoS4 nanosheet through a solvothermal method; 2, carrying out etching modification on the Cu2MoS4 nanosheet through strong acid; and 3, preparing the Cu2MoS4 / ZnO composite photocatalytic material by adopting a solvothermal method. According to the method, on the basis of a Cu2MoS4 / ZnO heterostructure, a Cu2MoS4 nanosheet is modified by adopting an acid etching method, reaction active sites are increased by exposing an edge area, and the utilization rate of photo-induced electrons is improved, so that the photocatalytic hydrogen evolution performance of the Cu2MoS4 / ZnO composite material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photocatalytic materials, and specifically relates to a method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO. Background Art

[0002] With the increasing depletion of energy, the concept of sustainable development has become a hot topic today. Hydrogen has become the object of research by researchers around the world because of its advantages such as no pollution, renewable and high energy density. Therefore, the development of efficient light-driven catalysts for water decomposition of hydrogen has become the focus of attention in recent years. Cu2MoS4, as one of the typical TTMs, has a unique layered structure and can be used as a carrier for other photocatalytic materials. It has a relatively narrow band gap (about 1.68eV), a suitable position of the valence conduction band, and good visible light absorption rate. It is used in photoelectrocatalysis, lithium batteries, supercapacitors and other fields, but the high electron-hole recombination rate and poor charge transfer rate are still important constraints for pure Cu2MoS4. Zinc oxide (ZnO) is an important metal oxide material with a band gap of 3.21eV. It is abundant in nature, has stable physical and chemical properties, is non-toxic and has excellent strong oxidation ability. It is an ideal photocatalytic material. However, the relatively fast recombination of photogenerated carriers in ZnO itself and the fact that it only absorbs ultraviolet light greatly affect its application in the field of photocatalytic hydrogen evolution.

[0003] According to the analysis of factors affecting photocatalytic activity and the research on methods for improving photocatalytic activity, it is known that the photocatalytic activity of photocatalytic materials can be improved by regulating material morphology, constructing heterojunctions, loading co-catalysts and manufacturing defects, so as to improve the photocatalytic hydrogen evolution performance of the material. In addition, for sheet materials, their edges are usually used as active centers for catalytic reactions. Cu2MoS4, as a typical sheet material, can enhance the photocatalytic activity of the material by adjusting the microstructure of the edge. At present, there are few research reports on the edge engineering of Cu2MoS4 nanosheets, especially the research on the use of edge engineering to enhance the photocatalytic hydrogen evolution of Cu2MoS4 composite materials. Therefore, based on the previous research, the present invention invents a method for etching and modifying Cu2MoS4 nanosheets, the purpose of which is to increase the exposed area of ​​the edge of the sheet material by etching and modification, thereby exposing more reactive sites, and then improving the photocatalytic performance of the composite material. Summary of the invention

[0004] The present invention mainly provides a method to solve the problem of low visible light utilization rate and fast recombination rate of photogenerated carriers of pure Cu2MoS4, which leads to poor photocatalytic hydrogen evolution performance under the existing technical conditions. The edge position of the sheet material is usually used as the active center of the catalytic reaction, and the Cu2MoS4 nanosheet is etched and modified. The reaction active sites are increased by exposing the edge area, so as to achieve a significant improvement in the photocatalytic hydrogen evolution performance of the Cu2MoS4 / ZnO composite material.

[0005] In order to solve the above problems, the present invention provides a method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, which is specifically carried out in the following steps:

[0006] Step S1, adding 80-110 mg Na2MoO4, 50-70 mg Cu2O, and 160-190 mg TAA to 20-40 ml EG solution, and ultrasonicating until the solution is evenly mixed and the powder particles are completely dissolved, transferring the obtained solution to a reaction kettle and keeping it at 160-220° C. for 22-26 hours, then repeatedly centrifugally washing with deionized water and ethanol, and then drying in a vacuum drying oven to obtain Cu2MoS4 nanosheets;

[0007] Step S2: Add 30-60 mg of Cu2MoS4 nanosheets prepared in S1 to 10-30 ml of 2-5 M HCl (or HNO 3、 H2SO4), ultrasonically treating for 10 to 15 minutes until the Cu2MoS4 nanosheets are uniformly dispersed in the solution, then stirring for 2 to 8 hours, washing the solution with deionized water and ethanol by centrifugation, and then drying in a vacuum drying oven to obtain etched Cu2MoS4 nanosheets;

[0008] Step S3, dispersing 0.18-0.19 g C4H6O4Zn and 0.3-0.5 g NaOH in 20-40 ml EG solvent, and ultrasonicating until the solution is uniform;

[0009] Step S4, dissolving 10-30 mg of etched Cu2MoS4 nanosheets prepared in S2 in the solvent of S3 until uniformly mixed, then transferring the solution to a reactor, keeping it warm at 130-160°C for 22-26 hours, then centrifugally washing with deionized water and ethanol, and drying in a vacuum drying oven to obtain etched Cu2MoS4 / ZnO;

[0010] Preferably, in step S1, the reaction solution is EG.

[0011] Preferably, in step S1, the solution needs to be ultrasonicated for 20 to 60 minutes until the solution turns brown and has no sediment.

[0012] Preferably, in step S1, the temperature is kept at 160-220° C. for 22-26 hours.

[0013] Preferably, in step S1, the centrifuge speed is 7000-10000 r / min, and the number of washing times is 5-8 times.

[0014] Preferably, in step S2, the strong acid is HCl, HNO3 and H2SO4.

[0015] Preferably, in step S2, the concentration of the strong acid is 2-5M.

[0016] Preferably, in step S2, the stirring time is 2 to 8 hours.

[0017] Preferably, in step S4, the reaction temperature of the experiment is 130-160°C.

[0018] The present invention adopts a solvothermal method to prepare Cu2MoS4 nanosheets, etches and modifies the Cu2MoS4 nanosheets by an acid etching method, loads ZnO nanoparticles in situ on the surface of the etched Cu2MoS4 nanosheets, and prepares a Cu2MoS4 / ZnO composite photocatalyst. The innovation of this method is that, based on the construction of the Cu2MoS4 / ZnO heterogeneous structure, the edge position of the sheet material is usually used as the active center of the catalytic reaction, and the reaction active site is increased by etching and modifying the exposed edge area, thereby promoting the transfer of photogenerated electrons and holes, improving the utilization rate of photogenerated electrons, and significantly improving the photocatalytic hydrogen evolution performance of the Cu2MoS4 / ZnO composite material. Compared with the unetched Cu2MoS4 / ZnO photocatalytic material, the etched and modified Cu2MoS4 / ZnO composite material exhibits lower fluorescence spectrum intensity, lower interface transfer resistance and lower hydrogen evolution overpotential, which greatly promotes the effective separation of photogenerated electron-hole pairs, so that the photocatalytic hydrogen evolution performance of the composite material is significantly improved. Sodium sulfide nonahydrate and anhydrous sodium sulfite were used as sacrificial agents, and a xenon lamp was used to simulate the sunlight. A hydrogen evolution experiment was conducted with 10 mg of the composite material and 50 ml of deionized water (the sacrificial agent concentrations were 0.08 M and 0.2 M, respectively). The results showed that the hydrogen evolution efficiency of the unetched Cu2MoS4 / ZnO composite material was about 550 μmol·g -1 ·h -1 , while the hydrogen evolution efficiency of the etched modified composite material reached about 1115 μmol·g -1 ·h -1 (Increased by about 103%), which is about 13.9 times that of pure Cu2MoS4. After cycle testing, the photocatalytic material still has good stability and hydrogen evolution performance after four cycles.

[0019] On the other hand, the present invention also provides a material for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, which is prepared by the method for preparing the material for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO as described above.

[0020] The beneficial effects of a material for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO provided by the present invention compared with the prior art are the same as the preparation method of a material for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the preparation process of Cu2MoS4 / ZnO material in an embodiment of the present invention;

[0022] Figure 2 is the XRD spectra of Cu2MoS4 nanosheets etched with different acids;

[0023] Figure 3 It is the XRD spectra of Cu2MoS4 / ZnO materials etched by different acids;

[0024] Figure 4 (a), (b) and (c) are SEM images of Cu2MoS4 etched by HCl, H2SO4 and HNO3, respectively; (d), (e) and (f) are SEM images of Cu2MoS4 / ZnO etched by HCl, H2SO4 and HNO3, respectively;

[0025] Figure 5 It is the hydrogen production performance diagram of unetched and different acid-etched Cu2MoS4 / ZnO materials; DETAILED DESCRIPTION

[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0027] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention can be combined with each other. The meanings of the terms "comprising", "including", "containing", and "having" are non-restrictive, that is, other steps and other ingredients that do not affect the results can be added. The above terms cover the terms "consisting of" and "essentially consisting of". Unless otherwise specified, materials, equipment, and reagents are commercially available.

[0028] The embodiment of the present invention provides a method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, such as Figure 1 As shown, the following steps are included:

[0029] Step S1, adding 90 mg Na2MoO4, 60 mg Cu2O, and 180 mg TAA to 30 ml EG solution, and ultrasonicating until the solution is evenly mixed and the powder particles are completely dissolved, and the obtained solution is transferred to a reactor and kept at 200° C. for 24 hours, and then repeatedly centrifuged and washed with deionized water and ethanol, and then dried in a vacuum drying oven to obtain Cu2MoS4 nanosheets;

[0030] Step S2: Add 50 mg of Cu2MoS4 nanosheets prepared in S1 to 20 ml of 4M HCl (or HNO 3、 H2SO4), ultrasonically treating the solution for 10 min until the Cu2MoS4 nanosheets are uniformly dispersed in the solution, then stirring for 5 h, washing the solution with deionized water and ethanol by centrifugation, and then drying in a vacuum drying oven to obtain etched Cu2MoS4 nanosheets;

[0031] Step S3, dispersing 0.184 g C4H6O4Zn and 0.4 g NaOH in 30 ml EG solvent, and ultrasonicating until the solution is uniform;

[0032] Step S4, dissolving 20 mg of etched Cu2MoS4 nanosheets prepared in S2 in the solvent of S3 until mixed evenly, then transferring the solution to a reactor, keeping it warm at 150°C for 24 hours, then centrifugally washing with deionized water and ethanol, and drying in a vacuum drying oven to obtain etched Cu2MoS4 / ZnO;

[0033] In step S1, Na2MoO4, Cu2O and TAA are added to the EG solution, and then ultrasonicated for 20 to 60 minutes until the solution is evenly mixed, until the solution turns brown and there is no sediment in the solution, which means that the powder particles are completely dissolved. The obtained solution is transferred to a reactor lined with polytetrafluoroethylene and kept warm for 22 to 26 hours at a temperature of 160 to 220°C. Then, the obtained lower precipitate is repeatedly centrifuged and washed in a centrifuge with deionized water and anhydrous ethanol and then dried.

[0034] EG has good solubility for both organic and inorganic substances. Choosing EG as a solvent can make Na2MoO4, Cu2O and TAA all well dissolved, thereby ensuring that the three are fully reacted in the mixed solution. By reacting at a temperature of 160-200°C and keeping the temperature for 22-26h, the Na2MoO4 in the mixed solution can be fully reacted. 4、 Cu2O and TAA react fully, and a suspension solution containing a reaction product is obtained after the reaction.

[0035] The suspension solution can be centrifuged, washed and dried to obtain powdered Cu2MoS4 nanosheet material.

[0036] Specifically, the suspension solution is centrifuged at 7000-10000 r / min, and after removing the supernatant, the precipitate is washed 5-8 times with deionized water and anhydrous ethanol to remove impurities in the precipitate, and a relatively pure Cu2MoS4 material can be obtained. After drying at 60-90°C for 12-24 hours, a powdered Cu2MoS4 material with a black color can be obtained. Deionized water and anhydrous ethanol are selected for washing because, on the one hand, water will not react with the reaction product, and washing with water will not introduce new impurities. On the other hand, anhydrous ethanol has good volatility and will not react with the reaction product, avoiding residues in the reaction product.

[0037] In step S2, the Cu2MoS4 nanosheets prepared in step S1 are added to 10-30 ml of 2-5 M strong acid, ultrasonicated and stirred, the solution is washed by centrifugation with deionized water and ethanol, and then dried in a vacuum drying oven to obtain etched Cu2MoS4 nanosheets.

[0038] Specifically, ultrasound is required for 10 to 15 minutes until the Cu2MoS4 nanosheets are evenly dispersed in the solution, and then the solution is stirred at room temperature for 2 to 8 hours. After stirring, the solution is centrifuged and washed 5 to 8 times with deionized water and anhydrous ethanol in a centrifuge at a speed of 7000 to 10000 r / min, and then dried at 60 to 90°C for 12 to 24 hours to obtain the etched Cu2MoS4 nanosheet sample.

[0039] In step S3, C4H6O4Zn and NaOH are dispersed in 20-40 ml of EG solvent and ultrasonicated until the solution is uniform.

[0040] Specifically, the reaction solution added is EG.

[0041] In step S4, the etched Cu2MoS4 nanosheets prepared in step S2 are dissolved in the solvent of S3 until the mixture is uniform, and the Cu2MoS4 nanosheets are added while stirring to make the Cu2MoS4 nanosheets uniformly dispersed, and then the solution is transferred to a reaction kettle and kept warm at a temperature of 130 to 160° C. for 22 to 26 hours. During the reaction, ZnO particles grow on the etched Cu2MoS4 nanosheets to obtain etched Cu2MoS4 / ZnO.

[0042] After the reaction is completed, the reaction solution is centrifuged, washed and dried to obtain the Cu2MoS4 / ZnO photocatalytic material.

[0043] Specifically, during the centrifugation process, the speed of the centrifuge is set to 7000-10000 r / min, deionized water and ethanol are used for washing 5-8 times, and after washing, vacuum drying is performed for 12-24 hours to obtain the Cu2MoS4 / ZnO photocatalytic material.

[0044] Another embodiment of the present invention provides a method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, which is prepared by using the above-mentioned method for preparing a Cu2MoS4 / ZnO composite photocatalytic material.

[0045] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on the conditions recommended by the manufacturer.

[0046] Example 1

[0047] 1.1. Add 90 mg Na2MoO4, 60 mg Cu2O, and 180 mg TAA to 30 ml EG solution, and perform ultrasonic treatment until the solution is evenly mixed and the powder particles are completely dissolved. The obtained solution is transferred to a reactor and kept at 200°C for 24 hours, and then repeatedly centrifuged and washed with deionized water and ethanol, and then dried in a vacuum drying oven to obtain Cu2MoS4 nanosheets;

[0048] 1.2. Add 50 mg of the prepared Cu2MoS4 nanosheets into 20 ml of 4M HCl, ultrasonicate for 10 min until the Cu2MoS4 nanosheets are evenly dispersed in the solution, then stir for 5 h, wash the solution with deionized water and ethanol by centrifugation, and then dry it in a vacuum drying oven to obtain Cu2MoS4 nanosheets after HCl etching;

[0049] 1.3. Disperse 0.184g C4H6O4Zn and 0.4g NaOH in 30ml EG solvent and sonicate until the solution is uniform;

[0050] 1.4. Dissolve 20 mg of the prepared HCl-etched Cu2MoS4 nanosheets in the solvent of 1.3 until uniformly mixed, then transfer the solution to a reactor, keep it at 150°C for 24 hours, then centrifuge and wash with deionized water and ethanol, and dry in a vacuum drying oven to obtain HCl-etched Cu2MoS4 / ZnO;

[0051] Example 2

[0052] 2.1. Add 90 mg Na2MoO4, 60 mg Cu2O, and 180 mg TAA to 30 ml EG solution, and perform ultrasonic treatment until the solution is evenly mixed and the powder particles are completely dissolved. The obtained solution is transferred to a reactor and kept at 200°C for 24 hours, and then repeatedly centrifuged and washed with deionized water and ethanol, and then dried in a vacuum drying oven to obtain Cu2MoS4 nanosheets.

[0053] 2.2. Add 50 mg of the prepared Cu2MoS4 nanosheets into 20 ml of 4M HNO3, ultrasonicate for 10 min until the Cu2MoS4 nanosheets are evenly dispersed in the solution, then stir for 5 h, wash the solution with deionized water and ethanol by centrifugation, and then dry it in a vacuum drying oven to obtain Cu2MoS4 nanosheets after HNO3 etching;

[0054] 2.3. Disperse 0.184g C4H6O4Zn and 0.4g NaOH in 30ml EG solvent and sonicate until the solution is uniform;

[0055] 2.4. Dissolve 20 mg of the prepared HNO3-etched Cu2MoS4 nanosheets in the solvent of 1.3 until mixed evenly, then transfer the solution to a reactor, keep it at 150°C for 24 hours, then centrifuge and wash with deionized water and ethanol, and dry it in a vacuum drying oven to obtain HNO3-etched Cu2MoS4 / ZnO;

[0056] Example 3

[0057] 3.1. Add 90 mg Na2MoO4, 60 mg Cu2O, and 180 mg TAA to 30 ml EG solution, and perform ultrasonic treatment until the solution is evenly mixed and the powder particles are completely dissolved. The obtained solution is transferred to a reactor and kept at 200°C for 24 h, and then repeatedly centrifuged and washed with deionized water and ethanol, and then dried in a vacuum drying oven to obtain Cu2MoS4 nanosheets.

[0058] 3.2. Add 50 mg of the prepared Cu2MoS4 nanosheets into 20 ml of 4M H2SO4, ultrasonicate for 10 min until the Cu2MoS4 nanosheets are evenly dispersed in the solution, then stir for 5 h, wash the solution with deionized water and ethanol by centrifugation, and then dry it in a vacuum drying oven to obtain Cu2MoS4 nanosheets after H2SO4 etching;

[0059] 3.3. Disperse 0.184g C4H6O4Zn and 0.4g NaOH in 30ml EG solvent and sonicate until the solution is uniform;

[0060] 3.4. Dissolve 20 mg of the prepared H2SO4-etched Cu2MoS4 nanosheets in 1.3% solvent until mixed evenly, then transfer the solution to a reactor, keep it warm at 150°C for 24 hours, then centrifuge and wash with deionized water and ethanol, and dry in a vacuum drying oven to obtain H2SO4-etched Cu2MoS4 / ZnO;

[0061] Comparative Example 1

[0062] 4.1. Add 90 mg Na2MoO4, 60 mg Cu2O, and 180 mg TAA to 30 ml EG solution, and perform ultrasonic treatment until the solution is evenly mixed and the powder particles are completely dissolved. The obtained solution is transferred to a reactor and kept at 200°C for 24 h, and then repeatedly centrifuged and washed with deionized water and ethanol, and then dried in a vacuum drying oven to obtain Cu2MoS4 nanosheets.

[0063] Comparative Example 2

[0064] 5.1. Disperse 0.184 g C4H6O4Zn and 0.4 g NaOH in 30 ml EG solvent, ultrasonicate until the solution is uniform, then transfer the solution to a reactor, keep it at 150°C for 24 h, then centrifuge and wash with deionized water and ethanol, and dry it in a vacuum oven to obtain ZnO;

[0065] Experimental Example 1

[0066] The Cu2MoS4 / ZnO composite photocatalytic materials obtained in the examples were respectively spectrally analyzed using an X'Pert PRO Cu-Kα diffractometer manufactured by Panalytical Analytical Instrument Company, wherein the scanning angle 2θ during the diffraction process was in the range of 10°-80°.

[0067] The results are as follows Figure 2 and Figure 3 As shown, Figure 2 and Figure 3 The horizontal axis represents the scanning angle, and the vertical axis represents the peak intensity. Figure 2 The three curves in the middle represent the XRD spectra of Cu2MoS4 nanosheets etched by HCl, H2SO4, and HNO3 of the same concentration (4M) from top to bottom. Figure 3 The three curves in the figure represent the XRD spectra of Cu2MoS4 / ZnO composite materials etched by HCl, HNO3, and H2SO4 of the same concentration (4M) from top to bottom. Figure 2 It can be seen that the phase composition of Cu2MoS4 after acid etching has not changed significantly, and the synthesized Cu2MoS4 still has a I phase structure. Its diffraction peaks at 2θ=17.641°(002), 18.621°(011), 29.301°(112), 31.541°(013), 37.741°(022), 46.301°(123), 47.541°(220), 49.561°(024), 51.041°(222), 54.841°(006), and 56.881°(132) correspond to those of unetched Cu2MoS4. Figure 3It can be seen that after the Cu2MoS4 / ZnO composite material is etched with different acids, no new characteristic peaks appear in its XRD spectrum, only the characteristic peaks of Cu2MoS4 and ZnO, which indicates that the phase composition of the etched Cu2MoS4 nanosheets and ZnO particles remains unchanged.

[0068] Experimental Example 2

[0069] The Cu2MoS4 nanosheets and Cu2MoS4 / ZnO composite photocatalytic materials obtained in Example 1 were characterized and observed using a field emission scanning electron microscope (FE-SEM, Sirion200, Philip).

[0070] The results are as follows Figure 4 As shown, from Figure 4 It can be clearly seen from ac that the sheet structure of the Cu2MoS4 samples after HCl, H2SO4, and HNO3 etching is basically maintained, and the edges of the Cu2MoS4 nanosheets after strong acid etching appear jagged, among which the Cu2MoS4 after HCl etching is the most obvious ( Figure 4 a). It can be seen that acid etching does not destroy the flaky structure of Cu2MoS4, and the length of the etched Cu2MoS4 flakes is about 2μm. Figure 4 It can be seen from the figure that after loading ZnO, the flake morphology of Cu2MoS4 is maintained, and many nanoparticles can be seen on the surface and at its edges. It is worth noting that the loaded ZnO particles are most obvious at the edges of Cu2MoS4 after HCl etching. Among all the samples, the Cu2MoS4 / ZnO composite material etched by HCl has the highest photocatalytic performance ( Figure 5 Photocatalytic test results in ).

[0071] Experimental Example 3

[0072] The Cu2MoS4 / ZnO composite photocatalytic materials obtained in Example 1 were respectively used to carry out photocatalytic water decomposition and hydrogen evolution experiments compared with the unetched Cu2MoS4 / ZnO composite photocatalytic materials to verify the influence of different acid etching on the hydrogen evolution performance of the composite materials.

[0073] The specific experimental method is as follows: a top-irradiated reactor with an argon lamp of 300W power was used as the reaction instrument and light source, respectively; 10mg of unetched Cu2MoS4 / ZnO composite photocatalyst material, HCl-etched Cu2MoS4 / ZnO composite photocatalyst material, HNO3-etched Cu2MoS4 / ZnO composite photocatalyst material and H2SO4-etched Cu2MoS4 / ZnO composite photocatalyst material were uniformly dispersed in 50mL of water, and Na2SO3 (0.2M) and Na2S·9H2O (0.08M) were used as sacrificial agents. Photocatalytic hydrogen experiments were carried out at a temperature of 5°C. Every hour, the generated hydrogen was quantitatively analyzed and detected by gas chromatography, and the hydrogen production efficiency was calculated.

[0074] The results are as follows Figure 5 As shown, Figure 5 The horizontal axis represents the catalytic time, and the vertical axis represents the hydrogen production. Figure 5 It can be seen that the hydrogen evolution efficiency of the unetched Cu2MoS4 / ZnO composite material is about 545μmol·g -1 ·h -1 The hydrogen evolution efficiency of Cu2MoS4 / ZnO composites etched by 4M HCl, HNO3 and H2SO4 was improved. The hydrogen evolution efficiency of Cu2MoS4 / ZnO composites etched by H2SO4 was about 568μmol·g -1 ·h -1 The hydrogen evolution efficiency of the Cu2MoS4 / ZnO composite material etched by HNO3 is about 658μmol·g -1 ·h -1 The Cu2MoS4 / ZnO composite material etched by HCl has the highest hydrogen evolution efficiency, which is about 1115 μmol·g -1 ·h -1 (Compared with the unetched, the hydrogen evolution efficiency increased by about 103%). It can be seen that the use of HCl etching modification can significantly improve the hydrogen evolution efficiency of the Cu2MoS4 / ZnO composite material. The reason may be that after modification, the active edge area of ​​Cu2MoS4 is increased to compound with ZnO, which enhances the light absorption of the composite material, which is beneficial to the photocatalytic composite material to accelerate the separation and migration efficiency of photogenerated electrons and holes, thereby improving the photocatalytic hydrogen evolution activity.

[0075] In summary, the preparation method of the Cu2MoS4 / ZnO composite photocatalytic material provided in the embodiment of the present invention, the prepared Cu2MoS4 / ZnO composite photocatalytic material is a binary composite material, composed of Cu2MoS4 nanosheets and ZnO nanoparticles. Among them, the ZnO nanoparticles are grown in situ on the surface of the Cu2MoS4 nanosheets, and the two materials form a heterojunction structure at the interface junction. The Cu2MoS4 nanosheets are etched with a strong acid, so that the edges of the Cu2MoS4 nanosheets are serrated, the exposed area of ​​the edge parts is increased, and more reactive sites are provided, thereby promoting the formation of a heterojunction structure between the Cu2MoS4 nanosheets and ZnO at the interface junction. The heterojunction structure can be used as an electron-hole transfer channel, so that the photogenerated electrons formed after the Cu2MoS4 is illuminated are quickly transferred and combined with the holes formed on the ZnO surface, thereby promoting the separation and migration efficiency of photogenerated electrons and holes, and then improving the photocatalytic hydrogen evolution activity.

[0076] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, characterized in that The method is specifically carried out in the following steps: Step S1, add 80-110 mg Na2MoO4, 50-70 mg Cu2O, and 160-190 mg TAA to 20-40 ml EG solution, perform ultrasonic treatment until the solution is evenly mixed and the powder particles are completely dissolved, transfer the obtained solution to a reaction kettle and keep it at 160-220° C. for 22-26 hours, then wash it repeatedly by centrifugation with deionized water and ethanol, and then dry it in a vacuum drying oven to obtain Cu2MoS4 nanosheets; Step S2: Add 30-60 mg of Cu2MoS4 nanosheets prepared in S1 to 10-30 ml of 2-5 M HCl (or HNO 3、 H2SO4), ultrasonically treating for 10 to 15 minutes until the Cu2MoS4 nanosheets are uniformly dispersed in the solution, then stirring for 2 to 8 hours, washing the solution with deionized water and ethanol by centrifugation, and then drying in a vacuum drying oven to obtain etched Cu2MoS4 nanosheets; Step S3, dispersing 0.18-0.19 g C4H6O4Zn and 0.3-0.5 g NaOH in 20-40 ml EG solvent, and ultrasonicating until the solution is uniform; Step S4, dissolving 10-30 mg of etched Cu2MoS4 nanosheets prepared in S2 in the solvent of S3 until mixed evenly, then transferring the solution to a reactor, keeping it warm at 130-160°C for 22-26 hours, then centrifugally washing with deionized water and ethanol, and drying in a vacuum drying oven to obtain etched Cu2MoS4 / ZnO.

2. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: In the step S1, the reaction solvent is EG.

3. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: In step S1, the solution needs to be ultrasonicated for 20 to 60 minutes until the solution turns brown and there is no sediment in the solution.

4. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: In step S1, the temperature is kept at 160-220° C. for 22-26 hours.

5. The method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: In step S1, the centrifuge speed is 7000-10000 r / min, and the washing times are 5-8 times.

6. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: The strong acids used in step S2 are HCl, HNO3 and H2SO4.

7. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: The concentration of the strong acid used in step S2 is 2-5M.

8. The method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: The stirring time in step S2 is 2 to 8 hours.

9. The method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO according to claim 1, characterized in that: The reaction temperature in the experiment in step S4 is 130-160°C.

10. A method for improving the photocatalytic hydrogen evolution performance of Cu2MoS4 / ZnO, characterized in that: The Cu2MoS4 / ZnO composite photocatalytic material is prepared by the preparation method of the Cu2MoS4 / ZnO composite photocatalytic material as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of zigzag Cu2MoS4 nanosheet and application in electrocatalysis and photocatalysis

    CN105597786A

  • Cu2MoS4 / ZnO composite photocatalytic material as well as preparation method and application thereof

    CN116273072A

  • Layered bimetallic sulfide nano material as well as preparation method and application thereof

    CN116899593A