Regeneration method of catalyst

By combining physical cleaning and heat treatment purging methods in the tube reactor, the problem of coking on the acrylic catalyst surface is solved, the removal rate and reactor efficiency are improved, the catalyst re-coking rate is reduced, and the reaction conversion rate is improved.

CN118719170APending Publication Date: 2024-10-01PINGHU PETROCHEM
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410852703.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Coking on the surface of the acrylic acid catalyst reduces the catalyst activity. Existing regeneration methods cannot effectively remove the coking, resulting in dust residue and an increase in the re-coking rate of the catalyst, affecting the reaction conversion rate and production costs.

Method used

Combining physical cleaning and heat treatment purging methods in the tubular reactor, through multi-stage heating, adjusting air and nitrogen fluxes, and using high-pressure nitrogen purging to directly remove coking and dust on the catalyst surface, improving the removal rate and overall reactor efficiency.

Benefits of technology

The coking removal rate on the catalyst surface is significantly improved, the catalyst re-coking rate is reduced, the reactor conversion efficiency is improved, and the efficiency of a single decoking method is increased by more than 20%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917239240000061
    Figure BDA0004917239240000061
  • Figure BDA0004917239240000062
    Figure BDA0004917239240000062
  • Figure BDA0004917239240000071
    Figure BDA0004917239240000071
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst regeneration, in particular to a regeneration method of a catalyst, the catalyst is regenerated in a tubular reactor, the regeneration method comprises physical cleaning and heat treatment purging, and the physical cleaning comprises the following steps: cooling and discharging the reactor, taking out a dustproof silk screen at the top of the reactor, and cleaning carbon deposit at the upper part of the reactor; adopting a negative pressure type suction pump to suck out inert small balls at the upper part of the tube nest of the reactor, detecting the pressure drop of the tube nest, and sucking out the catalyst at the lower part until the pressure drop meets the pressure drop standard; the heat treatment purging comprises the steps of controlling multi-section heating of the reactor, introducing air and / or inert gas, and monitoring the carbon content of an outlet of the reactor; maintaining the temperature of the reactor, reducing the introduction amount of air and / or inert gas, and monitoring the carbon content at the outlet of the reactor; naturally cooling the reactor, and increasing the introduction amount of air and / or inert gas; and high-pressure nitrogen is used for purging the tube nest of the reactor. The regeneration method can remove coke and dust on the surface of the catalyst, reduce the re-coking rate of the catalyst and improve the conversion rate of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst regeneration, in particular to a catalyst regeneration method, and specifically to a catalyst regeneration method for preparing acrylic acid from acrolein. Background Art

[0002] The acrylic acid production process is mostly a two-stage reaction. The first stage catalyst oxidizes propylene to acrolein, and the second stage reaction oxidizes acrolein to acrylic acid. Vanadium and molybdenum catalysts are commonly used for acrylic acid catalysts. Alumina is used as a carrier. The catalyst concentration is adjusted by inert beads to achieve the best reaction effect. However, the catalyst surface is easy to fall off, is afraid of water, and is deactivated at high temperature. The effective components are sublimated and lost. The catalyst surface is coked, resulting in a decrease in reaction conversion rate and an increase in system pressure drop, which affects the continuous production of chemical industry and increases production costs.

[0003] At present, the catalyst regeneration methods are mainly divided into physical method, chemical method and biological method. The details are as follows:

[0004] Physical methods include heat treatment, which burns off impurities such as carbon and ash by heating the catalyst; mechanical vibration, which uses mechanical force to remove pollutants on the catalyst surface; and purge, which uses compressed air or vacuum to remove fly ash from the catalyst surface.

[0005] Chemical methods include pickling, which uses acidic solutions to dissolve accumulated dust and harmful substances; chemical washing, which soaks the catalyst in acid and alkali solutions to remove surface pollutants; and chemical reaction, which adds specific chemical reagents to react with substances on the catalyst surface.

[0006] Biological methods include microbial methods, which use biological bacteria to metabolize and decompose dust and harmful substances; and enzyme methods, which use specific enzymes to decompose dust and harmful substances.

[0007] The coking on the surface of acrylic acid catalyst leads to the decrease of catalyst activity, but the existing catalyst regeneration method cannot effectively remove the coking on the catalyst surface. The dust left after removing the coking on the surface is easy to remain in the shell-and-tube reactor, which increases the catalyst coking rate. Summary of the invention

[0008] The purpose of the present invention is to solve the problems of low removal rate of coke on the surface of acrylic acid catalyst and residual coke dust described in the above background technology. A regeneration method for acrolein oxidation to acrylic acid catalyst is proposed. The regeneration method can directly remove coke on the catalyst surface in the reactor, greatly improving the removal rate of coke and dust.

[0009] The technical solution adopted by the present invention to solve the technical problem is: a catalyst regeneration method, the catalyst is regenerated in a tubular reactor, the upper part of the tubular reactor is filled with inert balls and the lower part is filled with catalyst, the regeneration method includes physical cleaning and heat treatment purging,

[0010] The physical cleaning comprises the following steps:

[0011] 1) Cool down the reactor, remove the dust screen on the top of the reactor, and clean the carbon deposits on the top of the reactor;

[0012] 2) Use a negative pressure suction pump to suck out the inert balls on the upper part of the reactor tubes, test the pressure drop of the tubes, and suck out the catalyst at the lower part until the pressure drop meets the pressure drop standard;

[0013] The heat treatment purge comprises:

[0014] 1) Controlling the multi-stage temperature rise of the reactor, introducing air and / or inert gas, and monitoring the carbon content at the reactor outlet;

[0015] 2) Maintain the reactor temperature, reduce the amount of air and / or inert gas introduced, and monitor the carbon content at the reactor outlet;

[0016] 3) The reactor is cooled naturally, and the amount of air and / or inert gas introduced is increased;

[0017] 4) Use high-pressure nitrogen to purge the reactor tubes.

[0018] In the above technical scheme, the reactor tubes are first physically cleaned to avoid the inability to perform heat treatment purging when the tubes are blocked. Physical cleaning greatly improves the utilization rate of the reactor tubes and the decoking accuracy. During the heat treatment purging process, multiple stages of heating are first performed, and hot air and / or inert gas are used to effectively remove the coke on the catalyst surface. Then, the reactor temperature is maintained, and the amount of air and / or inert gas introduced is reduced to ensure that the catalyst surface temperature is stable and the coke removal efficiency is improved. Then, the amount of air and / or inert gas introduced is increased to ensure that all dust in the gaps between the catalysts is blown out. Finally, high-pressure nitrogen is used for purging to further remove dust and reduce the rate of catalyst re-coking.

[0019] Preferably, the pressure drop standard is 13-18Kpa.

[0020] In the above technical solution, the pressure reduction standard is determined and adjusted according to the operation cycle of the reactor.

[0021] Preferably, the step 1) of heat treatment purging is specifically:

[0022] S1. The reactor is heated from 250°C to 280°C at a heating rate of 5°C / h, with an air flux of 1-5t / h and an inert gas flux of 0.5-1t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered;

[0023] S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 5-10t / h, and the inert gas flux is 0.5-1t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered;

[0024] S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 5-10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0025] S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 5-10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0026] S5. The reactor is heated from 320°C to 330°C at a heating rate of 2°C / h and an air flux of 5-10t / h until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered.

[0027] Preferably, the step 2) of heat treatment purging is specifically as follows: maintaining the reactor temperature at 330° C., reducing the air flux to 0.5-1 t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%.

[0028] Preferably, the step 3) of heat treatment purging is specifically: stopping heating the reactor and introducing air until the reactor temperature drops to 270° C., and the air flux is 10-20 t / h.

[0029] Preferably, in the step 4) of heat treatment purging, the pressure of high-pressure nitrogen is 1.5-2.0 MPa.

[0030] Preferably, the inert gas is nitrogen.

[0031] Preferably, the physical cleaning further comprises step 3), adding fresh catalyst for replenishment according to the service life of the catalyst.

[0032] Preferably, the carbon content is the sum of the mass fractions of carbon dioxide and carbon monoxide.

[0033] Preferably, the catalyst comprises any one or more elements selected from the group consisting of aluminum, vanadium, cobalt, molybdenum, iron, silicon, manganese, bismuth, copper and antimony.

[0034] The beneficial effects of the present invention are:

[0035] 1. The present invention combines physical cleaning and thermal treatment purging, which improves the efficiency by more than 20% compared with a single decoking method;

[0036] 2. The present invention adopts multi-stage heating to adjust the air and nitrogen flux, further improves the removal rate of coking on the catalyst surface, removes dust in the gap between catalysts, and reduces the rate of catalyst re-coking;

[0037] 3. The present invention can be directly carried out in a tubular reactor, and after treatment, the reactor tubular flux can be restored, thereby improving the overall conversion efficiency of the reactor. DETAILED DESCRIPTION

[0038] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0039] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0040] The present invention is now further described in conjunction with specific examples. The following examples are only for explaining the present invention, but do not constitute a limitation of the present invention. The test samples and test processes used in the following examples include the following (if the specific experimental conditions are not indicated in the examples, they are usually in accordance with conventional conditions or the conditions recommended by the reagent company; the reagents, consumables, etc. used in the following examples, if not otherwise specified, can all be obtained from commercial channels).

[0041] The catalyst of the invention is a catalyst for preparing acrylic acid from acrolein. The invention is carried out in a second tubular reactor in an acrylic acid production process. The upper part of the second tubular reactor is filled with inert small balls, and the lower part is filled with the catalyst for preparing acrylic acid from acrolein.

[0042] Example 1

[0043] A catalyst regeneration method, the regeneration method is physical cleaning and thermal treatment purging;

[0044] The specific steps for physical cleaning are as follows;

[0045] 1) Cool down the reactor, clean the top head of the reactor, take out the top dust screen, and clean the carbon deposits on the upper part of the reactor;

[0046] 2) Use a negative pressure suction pump to suck out all the inert balls on the top of the tubes, measure the pressure drop of the reactor tubes through an instrument, remove carbon deposits from the tubes with a pressure drop higher than the pressure drop standard, and suck out the catalyst until the pressure drop of the tubes meets the pressure drop standard;

[0047] 3) Calculate the catalyst dosage and ratio according to the service life and replenish the catalyst.

[0048] The specific steps of heat treatment purging are as follows:

[0049] S1, the reactor is heated from 250°C to 280°C, the heating rate is 5°C / h, the air flux is 1t / h, and the inert gas flux is 0.5t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered;

[0050] S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 5t / h, and the inert gas flux is 0.5t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered;

[0051] S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 5t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0052] S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 5t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0053] S5, the reactor is heated from 320°C to 330°C, the heating rate is 2°C / h, the air flux is 5t / h, until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered;

[0054] S6. Maintain the reactor temperature at 330°C and reduce the air flux to 0.5 t / h until the carbon content at the reactor outlet is less than 0.5%;

[0055] S7, stop heating the reactor and introduce air until the reactor temperature drops to 270° C., and the air flux is 10 t / h;

[0056] S8. Use high-pressure nitrogen to purge the reactor tubes, and the pressure of the high-pressure nitrogen is 1.5 MPa.

[0057] The above inert gas is nitrogen, and the carbon content is the sum of carbon dioxide and carbon monoxide contents.

[0058] Example 2

[0059] A catalyst regeneration method, the regeneration method is physical cleaning and thermal treatment purging;

[0060] The specific steps for physical cleaning are as follows;

[0061] 1) Cool down the reactor, clean the top head of the reactor, take out the top dust screen, and clean the carbon deposits on the upper part of the reactor;

[0062] 2) Use a negative pressure suction pump to suck out all the inert balls on the top of the tubes, measure the pressure drop of the reactor tubes through an instrument, remove carbon deposits from the tubes with a pressure drop higher than the pressure drop standard, and suck out the catalyst until the pressure drop of the tubes meets the pressure drop standard;

[0063] 3) Calculate the catalyst dosage and ratio according to the service life and replenish the catalyst.

[0064] The specific steps of heat treatment purging are as follows:

[0065] S1. The reactor is heated from 250°C to 280°C at a heating rate of 5°C / h, with an air flux of 5t / h and an inert gas flux of 0.8t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered;

[0066] S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 10t / h, and the inert gas flux is 1t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered;

[0067] S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0068] S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0069] S5, the reactor is heated from 320°C to 330°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered;

[0070] S6. Maintain the reactor temperature at 330° C. and reduce the air flux to 1 t / h until the carbon content at the reactor outlet is less than 0.5%;

[0071] S7, stop heating the reactor and introduce air until the reactor temperature drops to 270° C., and the air flux is 20 t / h;

[0072] S8. Use high-pressure nitrogen to purge the reactor tubes, and the pressure of the high-pressure nitrogen is 2 MPa.

[0073] The above inert gas is nitrogen, and the carbon content is the sum of carbon dioxide and carbon monoxide contents.

[0074] The reactor heat exchange medium temperature and conversion rate of the catalysts after regeneration in Example 1 and Example 2 were respectively detected, wherein the conversion rate was calculated by measuring the acrylic acid content at the bottom outlet of the second tubular reactor by gas chromatograph. The comparative data before and after regeneration of the catalyst in Example 1 are shown in Table 1, and the comparative data before and after regeneration of the catalyst in Example 2 are shown in Table 2.

[0075] Table 1 Comparison of data before and after catalyst regeneration in Example 1

[0076]

[0077] Table 2 Comparison of data before and after catalyst regeneration in Example 2

[0078]

[0079] In the above table, "pressure drop at 100% load" refers to the pressure drop data when the reactor is started up to 100% load conditions, indicating that the operating conditions before and after catalyst regeneration are the same; "heat exchange medium temperature" is the heat exchange medium temperature in the second reactor, indicating the temperature when the reactor is running.

[0080] It can be seen from Tables 1 and 2 that before the catalyst is regenerated, the temperature of the heat exchange medium in the second reactor is higher than the temperature after regeneration. Under normal circumstances, the higher the temperature of the heat exchange medium in the second reactor, the higher the conversion rate of the catalyst. After the regeneration method of the present invention, the temperature of the heat exchange medium in the second reactor decreases, but the catalyst conversion rate increases, indicating that the regeneration effect of the present invention is significant.

[0081] Comparative Example 1

[0082] A catalyst regeneration method, the regeneration method is heat treatment purging, the specific steps are as follows;

[0083] S1. The reactor is heated from 250°C to 280°C at a heating rate of 5°C / h, with an air flux of 5t / h and an inert gas flux of 0.8t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered;

[0084] S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 10t / h, and the inert gas flux is 1t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered;

[0085] S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0086] S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0087] S5, the reactor is heated from 320°C to 330°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered;

[0088] S6. Maintain the reactor temperature at 330° C. and reduce the air flux to 1 t / h until the carbon content at the reactor outlet is less than 0.5%;

[0089] S7, stop heating the reactor and introduce air until the reactor temperature drops to 270° C., and the air flux is 20 t / h;

[0090] S8. Use high-pressure nitrogen to purge the reactor tubes, and the pressure of the high-pressure nitrogen is 2 MPa.

[0091] The above inert gas is nitrogen, and the carbon content is the sum of carbon dioxide and carbon monoxide contents.

[0092] The regenerated catalyst of Comparative Example 1 was tested, and the test items and methods were the same as those of Example 1. The test data are shown in Table 3.

[0093] Table 3 Comparative Example 1 Data Comparison Before and After Catalyst Regeneration

[0094]

[0095] It can be seen from Table 3 that without physical cleaning before heat treatment purging, the reactor temperature must be raised to 272°C for the catalyst conversion rate to reach 99.3%. However, after physical cleaning, the reactor temperature only needs to be 267°C. It can be seen that at the same temperature, the catalyst conversion rate is lower without physical cleaning. This may be because, without physical cleaning, the hot air cannot accurately blow away the coke on the catalyst surface, resulting in lower decoking efficiency.

[0096] Comparative Example 2

[0097] A catalyst regeneration method, the regeneration method is physical cleaning and thermal treatment purging;

[0098] The specific steps for physical cleaning are as follows;

[0099] 1) Cool down the reactor, clean the top head of the reactor, take out the top dust screen, and clean the carbon deposits on the upper part of the reactor;

[0100] 2) Use a negative pressure suction pump to suck out all the inert balls on the top of the tubes, measure the pressure drop of the reactor tubes through an instrument, remove carbon deposits from the tubes with a pressure drop higher than the pressure drop standard, and suck out the catalyst until the pressure drop of the tubes meets the pressure drop standard;

[0101] 3) Calculate the catalyst dosage and ratio according to the service life and replenish the catalyst.

[0102] The specific steps of heat treatment purging are as follows:

[0103] S1. The reactor is heated from 250°C to 280°C at a heating rate of 5°C / h, with an air flux of 5t / h and an inert gas flux of 0.8t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered;

[0104] S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 10t / h, and the inert gas flux is 1t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered;

[0105] S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0106] S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered;

[0107] S5, the reactor is heated from 320°C to 330°C, the heating rate is 2°C / h, the air flux is 10t / h, until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered;

[0108] S6. Maintain the reactor temperature at 330°C and reduce the air flux to 1 t / h until the carbon content at the reactor outlet is detected to be less than 0.5%.

[0109] The above inert gas is nitrogen, and the carbon content is the sum of carbon dioxide and carbon monoxide contents.

[0110] The catalysts regenerated in Example 2 and Comparative Example 2 were used normally, and the pressure drop of the reactor was monitored online in real time by DCS. When the monitoring showed that the pressure drop of the reactor was greater than 26 KPa at 100% load, it was determined that the catalyst was coked again. The detection results are shown in Table 4.

[0111] Table 4 Comparison of catalyst re-coking time of Example 2 and Comparative Example 2

[0112] project Re-coking time (month) Example 2 8-10 Comparative Example 2 4-6

[0113] As can be seen from Table 4, in Comparative Example 2, in the absence of high-throughput air purge and nitrogen purge in steps S7 and S8, the catalyst re-coking rate increased significantly. This may be because the dust residue in the gaps and on the surface of the catalyst provided conditions for the subsequent re-generation of coke.

[0114] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0115] The above is a detailed introduction to a catalyst regeneration method provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for regenerating a catalyst, characterized in that: The catalyst is regenerated in a shell-and-tube reactor, the upper part of the shell-and-tube reactor is filled with inert small balls and the lower part is filled with catalyst. The regeneration method includes physical cleaning and heat treatment purging. The physical cleaning comprises the following steps: 1) Cool down the reactor, remove the dust screen on the top of the reactor, and clean the carbon deposits on the top of the reactor; 2) Use a negative pressure suction pump to suck out the inert balls on the upper part of the reactor tubes, test the pressure drop of the tubes, and suck out the catalyst at the lower part until the pressure drop meets the pressure drop standard; The heat treatment purge comprises: 1) Controlling the multi-stage temperature rise of the reactor, introducing air and / or inert gas, and monitoring the carbon content at the reactor outlet; 2) Maintain the reactor temperature, reduce the amount of air and / or inert gas introduced, and monitor the carbon content at the reactor outlet; 3) The reactor is cooled naturally, and the amount of air and / or inert gas introduced is increased; 4) Use high-pressure nitrogen to purge the reactor tubes.

2. The regeneration method according to claim 1, characterized in that: The pressure drop standard is 13-18Kpa.

3. The regeneration method according to claim 1, characterized in that: The step 1) of heat treatment purging is specifically: S1. The reactor is heated from 250°C to 280°C at a heating rate of 5°C / h, with an air flux of 1-5t / h and an inert gas flux of 0.5-1t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%, and then the next step is entered; S2, the reactor is heated from 280°C to 300°C, the heating rate is 5°C / h, the air flux is 5-10t / h, and the inert gas flux is 0.5-1t / h, until the carbon content at the reactor outlet is detected to be less than 0.2%, and then the next step is entered; S3, the reactor is heated from 300°C to 310°C, the heating rate is 2°C / h, the air flux is 5-10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered; S4, the reactor is heated from 310°C to 320°C, the heating rate is 2°C / h, the air flux is 5-10t / h, until the carbon content at the reactor outlet is detected to be less than 0.3%, and then the next step is entered; S5. The reactor is heated from 320°C to 330°C at a heating rate of 2°C / h and an air flux of 5-10t / h until the carbon content at the reactor outlet is detected to be less than 0.1%, and then the next step is entered.

4. The regeneration method according to claim 1, characterized in that: The step 2) of heat treatment purging is specifically as follows: maintaining the reactor temperature at 330° C., reducing the air flux to 0.5-1 t / h, until the carbon content at the reactor outlet is detected to be less than 0.5%.

5. The regeneration method according to claim 1, characterized in that: The step 3) of heat treatment purging is specifically: stop heating the reactor and introduce air until the reactor temperature drops to 270° C., and the air flux is 10-20 t / h.

6. The regeneration method according to claim 1, characterized in that: In the step 4) of heat treatment purging, the pressure of high-pressure nitrogen is 1.5-2.0 MPa.

7. The regeneration method according to claim 1, characterized in that: The inert gas is nitrogen.

8. The regeneration method according to claim 1, characterized in that: The physical cleaning also includes step 3), adding fresh catalyst for replenishment according to the service life of the catalyst.

9. The regeneration method according to claim 1, characterized in that: The carbon content is the sum of the mass fractions of carbon dioxide and carbon monoxide.

10. The regeneration method according to claim 1, characterized in that: The catalyst contains any one or more elements of aluminum, vanadium, cobalt, molybdenum, iron, silicon, manganese, bismuth, copper and antimony.

Citation Information

Patent Citations

  • Internal regeneration method of alumina catalyst for ethanol dehydration

    CN102294277A

  • Regeneration process of SCR (Selective Catalytic Reduction) denitration catalyst

    CN117065805A

  • Solid catalyst cleaning device in tubular reactor

    CN211802966U

  • Improved method and apparatus for catalyst activation

    GB849929A