Temperature conducting workpiece, surface treatment process thereof and portable temperature adjusting device
By spraying the adhesion enhancement layer and paint layer on the metal heat-conducting parts, combined with the design of temperature-sensitive color changes, the problem of easy blistering and falling off of the paint layer of the heat-conducting parts is solved, and the adhesion and corrosion resistance of the product are improved. , improving appearance and quality.
Patent Information
- Application Number
- CN202410719352.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
Existing metal heat-conducting parts come into contact with sweat during use, causing the paint layer to bubble and fall off, affecting the appearance and quality of the product.
A surface treatment process is adopted, which includes pre-treatment of the metal substrate, spraying the adhesion enhancement layer and paint layer, and enhancing the adhesion of the paint layer through components such as acrylic resin to form primer, color paint and varnish layers, and in the third Open-pore structures are carved into the two-tone paint layer to achieve temperature-sensitive color changes.
It significantly improves the adhesion and corrosion resistance of the paint layer, extends the service life, improves the appearance and quality of the product, prevents bubbling and shedding of the paint layer, and enhances the competitiveness of the product.
Smart Images

Figure CN118719501A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of material surface treatment, and in particular to a temperature-conducting workpiece and a surface treatment process thereof and a portable temperature regulating device. Background Art
[0002] Compared with other materials, metal has better thermal conductivity (conducting heat or cold), so metal parts are usually used for heat conduction in some devices with high thermal conductivity requirements. For example, portable refrigeration or heating products are common in life, and metal thermal conductive parts are usually installed on the outside of the product to conduct the cold or heat generated by the internal refrigeration or heating parts to the surface of the product and contact the skin of the user's neck and other parts, so as to bring a cool feeling to the user when the temperature is high, or bring a warm feeling to the user when the temperature is low.
[0003] When installing the thermal conductive component on the product, the surface of the metal thermal conductive component is usually spray-painted first in order to match the appearance of the product and to achieve a certain corrosion resistance. The existing processing technology usually involves pre-processing the metal thermal conductive component such as die-casting, whitening and passivation to form a passivation layer on the surface of the metal thermal conductive component, and then spray-painting the passivation layer. However, under this process, the adhesion of the paint on the metal thermal conductive component is insufficient, and the paint layer may bubble and fall off.
[0004] Moreover, the thermal conductive components need to be in direct contact with the skin. Especially in the summer when people sweat a lot, the long-term contact between the metal thermal conductive components and sweat can more easily cause the paint layer on the surface of the metal thermal conductive components to bubble and fall off, thereby causing the surface of the metal thermal conductive components to become rough, seriously affecting the appearance, quality and experience of the product. Summary of the invention
[0005] In view of this, the present application provides a temperature-conducting workpiece and a surface treatment process thereof and a portable temperature control device that can effectively solve the above-mentioned problems.
[0006] The present application provides a surface treatment process for a temperature conducting workpiece, comprising the following steps:
[0007] S1: providing a metal substrate and pre-treating the metal substrate to obtain a pre-treated workpiece;
[0008] S2: spraying a treatment agent on the pre-treated workpiece so that an adhesion enhancement layer is formed on the surface of the pre-treated workpiece; and
[0009] S3: spraying paint on the adhesion enhancement layer so that a paint layer is formed on the surface of the adhesion enhancement layer to obtain a temperature conducting workpiece.
[0010] In one embodiment, the treating agent includes acrylic resin.
[0011] In one embodiment, the treatment agent comprises the following components in terms of mass percentage: 38-42% polypropylene resin; 48-52% toluene; and 8-12% xylene.
[0012] In one embodiment, the S3 includes:
[0013] S31: spraying a primer on the adhesion enhancing layer so that a primer layer is formed on the surface of the adhesion enhancing layer;
[0014] S32: spraying a first color paint on the primer layer, so that a first color paint layer is formed on the surface of the primer layer;
[0015] S33: spraying a temperature-sensitive color paint on the first color paint layer, so that a temperature-sensitive color-changing paint layer is formed on the surface of the first color paint layer;
[0016] S34: spraying a second color paint on the thermochromic paint layer, so that a second color paint layer is formed on the surface of the thermochromic paint layer;
[0017] S35: spraying clear varnish on the second color paint layer, so that the clear varnish layer is formed on the surface of the second color paint layer.
[0018] In one embodiment, the S34 includes:
[0019] S341: Carving an open hole structure on the second color paint layer so that a portion of the thermochromic paint layer corresponding to the open hole structure is exposed.
[0020] In one embodiment, S2 includes: spraying the treatment agent on the pre-treated workpiece and then baking to obtain the adhesion enhancement layer, the baking temperature is 80° C. to 90° C., and the baking time is 12 min to 18 min;
[0021] The S31 comprises: spraying the primer on the adhesion enhancement layer and then baking to obtain the primer layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the primer is 11.9S to 12.9S;
[0022] The S32 comprises: spraying the first color paint on the primer layer and then baking to obtain the first color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the first color paint is 11.9S to 12.9S;
[0023] The S33 comprises: spraying the first color paint layer with the temperature-sensitive color paint and then baking to obtain the temperature-sensitive color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the temperature-sensitive color paint is 12.2S to 13.2S;
[0024] The S34 includes: spraying the second color paint on the thermochromic paint layer and then baking to obtain the second color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the second color paint is 10.5S to 11.5S;
[0025] The S35 comprises: spraying the varnish on the second color paint layer and then baking to obtain the varnish layer, the baking temperature is 55° C. to 65° C., the baking time is 3 min to 8 min, and the viscosity of the varnish is 8.5S to 9.5S.
[0026] In one embodiment, the thickness of the adhesion enhancement layer is 2μm to 8μm, the thickness of the primer layer is 19μm to 25μm, the thickness of the first color paint layer is 29μm to 35μm, the thickness of the thermochromic paint layer is 33μm to 40μm, the thickness of the second color paint layer is 5μm to 8μm, and the thickness of the varnish layer is 20μm to 30μm.
[0027] In one embodiment, the pre-processing in S1 includes:
[0028] S11: die-casting the metal substrate;
[0029] S12: performing a whitening treatment on the die-cast metal substrate to remove impurities on the surface of the metal substrate;
[0030] S13: performing a passivation treatment on the metal substrate after the whitening treatment, so that a passivation layer is formed on the surface of the metal substrate, and the adhesion enhancement layer is connected to the passivation layer.
[0031] The present application also provides a temperature-conducting workpiece, which is prepared by the surface treatment process as described above.
[0032] The present application also provides a portable temperature control device, comprising a shell, a temperature control component arranged in the shell, and a temperature conducting component thermally connected to the temperature control component, wherein the temperature conducting component is arranged on the outer surface of the shell and is the temperature conducting workpiece as described above.
[0033] In one embodiment, the paint layer includes a primer layer, a first color paint layer, a thermochromic paint layer, a second color paint layer and a clear paint layer, the second color paint layer is engraved with an open hole structure, and the thermochromic paint layer changes color by sensing the temperature of the temperature conducting workpiece. When the thermostatic component is cooling, the thermochromic paint layer presents a first color; when the thermostatic component is heating, the thermochromic paint layer fades or presents a second color.
[0034] In summary, the present application provides a temperature-conducting workpiece, a surface treatment process thereof, and a portable temperature control device, wherein the metal substrate is first pre-treated to obtain a pre-treated workpiece, and then a treatment agent is sprayed on the pre-treated workpiece to form an adhesion enhancement layer on the surface of the pre-treated workpiece, and finally paint is sprayed on the adhesion enhancement layer to form a paint layer on the surface of the adhesion enhancement layer to obtain a temperature-conducting workpiece, wherein the adhesion enhancement layer is used to enhance the adhesion of the paint layer on the pre-treated workpiece, so that the paint layer can be firmly and tightly attached to the pre-treated workpiece, greatly improving the problems of bubbling and falling off of the paint layer, extending the service life of the paint layer, enhancing the corrosion resistance of the product, and improving the appearance and quality of the product, thereby enhancing the competitiveness of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a flowchart of the surface treatment process of the temperature-conducting workpiece in this application.
[0036] Figure 2 for Figure 1 Flow chart of further processing of step S1 in .
[0037] Figure 3 for Figure 1 Flow chart of further processing of step S3 in .
[0038] Figure 4 This is a schematic structural diagram of the temperature conducting workpiece of the present application. DETAILED DESCRIPTION
[0039] Before describing the embodiments in detail, it should be understood that the present application is not limited to the detailed structure or component arrangement described below or in the drawings in the present application. The present application may be an embodiment implemented in other ways. Moreover, it should be understood that the words and terms used herein are only used for descriptive purposes and should not be interpreted restrictively. The words "including", "comprising", "having" and the like used herein are meant to include the items listed thereafter, their equivalents and other additional items. In particular, when describing "a certain element", the present application does not limit the number of the element to one, but may also include multiple elements.
[0040] like Figure 1 As shown, the present application provides a surface treatment process for a temperature-conducting workpiece, and the surface treatment process includes:
[0041] S1: providing a metal substrate and pre-treating the metal substrate to obtain a pre-treated workpiece. The pre-treatment can make the metal substrate into a desired shape, and can remove impurities such as dust, oxide layer and oil on the surface of the metal substrate. At the same time, a passivation layer can be formed on the surface of the metal substrate. The passivation layer is, for example, a dense oxide layer, which can be firmly and tightly attached to the surface of the metal substrate to protect the metal substrate, and can also reduce the surface roughness of the pre-treated workpiece.
[0042] S2: spraying a treatment agent onto the pre-treated workpiece to form an adhesion enhancement layer on the surface of the pre-treated workpiece.
[0043] S3: spraying paint on the adhesion enhancement layer to form a paint layer on the surface of the adhesion enhancement layer to obtain a thermal conductive workpiece. The paint layer can play a decorative and protective role, increase the aesthetics of the thermal conductive workpiece, and enhance the corrosion resistance of the thermal conductive workpiece.
[0044] The adhesion enhancement layer is used to enhance the adhesion of the paint layer on the pre-processed workpiece, so that the paint layer can be firmly and tightly attached to the pre-processed workpiece, greatly improving the problems of bubbling and shedding of the paint layer, extending the service life of the paint layer, enhancing the corrosion resistance of the product, improving the appearance and quality of the product, and thus improving the competitiveness of the product. In this embodiment, the metal substrate is an aluminum alloy, and in other embodiments, the metal substrate may also be other suitable metals.
[0045] like Figure 2 As shown, in this embodiment, the pre-processing in S1 includes:
[0046] S11: Die-casting the metal substrate to form the metal substrate into the shape and specifications required by the specific product.
[0047] S12: The metal substrate after die casting is subjected to whitening treatment to remove impurities on the surface of the metal substrate. The process flow of whitening treatment may include degreasing, pickling and alkali washing. For example, the oil stains on the surface of the metal substrate are cleaned by ultrasonic wave. In other embodiments, the metal substrate may be cleaned by aluminum alloy cleaning agent to remove various greases, stains, etc. attached to the surface of the metal substrate; or, an organic solution is sprayed on the surface of the metal substrate with oil stains, and the surface of the metal substrate is wiped repeatedly and then wiped with clean water, which can also remove the oil stains and other impurities on the surface of the metal substrate. Then, the metal substrate after degreasing treatment is immersed in a nitric acid solution with a concentration of 65% to 75%, and is taken out after soaking for 15s to 25s to remove the oxide layer and impurities on the surface of the metal substrate. The oxide layer is an aluminum oxide layer formed after the metal substrate is oxidized in the air. The aluminum oxide layer is coarse and easy to fall off, and has weak corrosion resistance; preferably, the metal substrate is immersed in a nitric acid solution with a concentration of 68% to 70% for 20s and then taken out. Finally, the pickled metal substrate is immersed in a sodium hydroxide solution with a concentration of 45% to 55%, and taken out after soaking for 15s to 25s to remove the nitric acid solution and impurities remaining on the surface of the metal substrate; preferably, the metal substrate is immersed in a sodium hydroxide solution with a concentration of 50% for 20s and then taken out.
[0048] S13: The metal substrate after the whitening treatment is passivated so that a passivation layer is formed on the surface of the metal substrate, and the adhesion enhancement layer is connected to the passivation layer. The principle of passivation is to use physical adsorption or pressure adsorption to make the film agent adhere to the surface of the substrate to protect the substrate. The aluminum film agent is mainly used for the chromium film treatment of aluminum and aluminum alloys, and the color of the film is from light yellow to dark golden yellow. In this embodiment, the process flow of the passivation treatment may include passivation, cleaning and baking. For example, the metal substrate is immersed in a chromic acid solution with a concentration of 60% to 65%, so that a dense passivation layer is formed on the surface of the metal substrate to improve the corrosion resistance of the metal substrate. The passivation layer is usually grayish white. Specifically, the passivation layer is a chromium oxide layer formed after the metal substrate undergoes a chemical reaction in the chromic acid solution. The passivation layer covers the entire surface of the metal substrate. The passivation layer has a dense texture and can be firmly and tightly attached to the surface of the metal substrate, which can improve the corrosion resistance of the metal substrate and reduce the roughness of the surface of the metal substrate; preferably, the concentration of the chromic acid solution is 62%. Then, the metal substrate is taken out from the chromic acid solution and the surface of the passivation layer is washed with water to remove the chromic acid solution and impurities remaining on the surface of the passivation layer. Finally, the metal substrate is baked in a temperature environment of 70°C to 80°C for 10min to 20min to remove the moisture remaining on the surface of the passivation layer, for example, the metal substrate is placed in an oven and the oven temperature is adjusted to 70°C to 80°C so that the moisture remaining on the surface of the passivation layer is fully evaporated; preferably, the baking temperature is 75°C and the baking time is 15min; finally, the pre-treated workpiece is obtained.
[0049] In this embodiment, the pre-treated workpiece is sprayed with a treatment agent, wherein the treatment agent can be an acrylic resin, which mainly plays a role in increasing the adhesion of the paint layer. After the treatment agent is sprayed on the metal substrate, the coating formed by the acrylic resin on the surface of the metal substrate interacts with the paint molecules, thereby enhancing the adhesion of the paint layer. The treatment agent includes the following components by mass percentage: 38-42% polypropylene resin; 48-52% toluene; 8-12% xylene. Preferably, the components of the treatment agent are: 40% polypropylene resin; 50% toluene; 10% xylene. The specific composition / component information of the treatment agent is shown in Table 1 below.
[0050] Table 1
[0051] Ingredient Name Mass percentage CAS NO. Polypropylene resin 40% 9003-07-0 Toluene (solvent) 50% 108-88-3 Xylene (solvent) 10% 1330-20-7
[0052] The physical and chemical properties of the treatment agent are as follows: the material state is liquid, the color is light yellow, the decomposition temperature is 130°C, the vapor pressure is less than 100 mbar (50°C), the flash point is 12°C, the viscosity is about 11000 mPa·s (23°C), the density is 0.92, the solubility is less than 10 mg / l (20°C), and the ignition temperature is about 450°C.
[0053] In this embodiment, the thickness of the adhesion enhancement layer is 2 μm to 8 μm. Preferably, the thickness of the adhesion enhancement layer is 5 μm.
[0054] like Figure 2 As shown, step S2 also includes: spraying the treatment agent on the pre-treated workpiece and then baking to obtain an adhesion enhancement layer, wherein the baking temperature is 80°C to 90°C, and the baking time is 12min to 18min. Preferably, the baking temperature is 85°C, and the baking time is 15min. Specifically, after the treatment agent is evenly sprayed on the surface of the passivation layer of the pre-treated workpiece, baking is performed so that the treatment agent is cured on the surface of the passivation layer to form an adhesion enhancement layer. As mentioned above, the treatment agent has the characteristics of high decomposition temperature, high viscosity, low solubility, etc. The obtained adhesion enhancement layer has stable performance, and the adhesion enhancement layer can be tightly and firmly connected to the passivation layer.
[0055] like Figure 3 As shown, step S3 includes:
[0056] S31: spraying primer on the adhesion enhancing layer so that a primer layer is formed on the surface of the adhesion enhancing layer. Specifically, the primer is, for example, white paint. In other embodiments, the primer may also be other colors. The white paint is evenly sprayed on the surface of the adhesion enhancing layer so that the white paint is tightly and firmly connected to the adhesion enhancing layer, and the adhesion enhancing layer can enhance the adhesion of the white paint through molecular action. Furthermore, after spraying the primer on the adhesion enhancing layer, baking is performed so that the white paint can be cured on the surface of the adhesion enhancing layer to form a primer layer and is tightly connected to the adhesion enhancing layer, wherein the baking temperature is 80°C to 90°C, the baking time is 20min to 40min, and the viscosity of the primer is 11.9S to 12.9S; preferably, the baking temperature is 85°C, the baking time is 30min, and the viscosity of the primer is 12.4S.
[0057] S32: Spray the first color paint on the primer layer so that the first color paint layer is formed on the surface of the primer layer. Specifically, the first color paint is, for example, orange paint. In other embodiments, the first color paint can also be other colors. The orange paint is evenly sprayed on the surface of the primer layer so that the orange paint is tightly and firmly connected to the primer layer. Furthermore, after the first color paint is sprayed on the primer layer, it is baked so that the orange paint can be cured on the surface of the primer layer to form the first color paint layer and is tightly connected to the primer layer, wherein the baking temperature is 80°C to 90°C, the baking time is 20min to 40min, and the viscosity of the first color paint is 11.9S to 12.9S; preferably, the baking temperature is 85°C, the baking time is 30min, and the viscosity of the color paint is 12.4S.
[0058] S33: Spraying the first paint layer with thermosensitive paint, so that a thermochromic paint layer is formed on the surface of the first paint layer. Specifically, the thermosensitive paint is, for example, thermosensitive blue paint. In other embodiments, the thermosensitive paint may also be other thermosensitive colors. The thermosensitive blue paint is evenly sprayed on the surface of the first paint layer, so that the thermosensitive blue paint is tightly and firmly connected to the first paint layer. Furthermore, after spraying the thermosensitive paint on the first paint layer, baking is performed so that the thermosensitive blue paint can be cured on the surface of the first paint layer to form a thermochromic paint layer, and is tightly connected to the first paint layer, wherein the baking temperature is 80°C to 90°C, the baking time is 20min to 40min, and the viscosity of the thermosensitive paint is 12.2S to 13.2S; preferably, the baking temperature is 85°C, the baking time is 30min, and the viscosity of the thermosensitive paint is 12.7S. Thermosensitive paint can show different colors according to different temperatures. For example, the thermosensitive paint changes color by sensing the temperature of the metal substrate. When the temperature of the metal substrate is low, the thermosensitive paint shows color, such as blue. When the temperature of the metal substrate is high, the thermosensitive paint does not show color, so as to show the color of the first paint layer. For example, when the thermochromic paint layer does not show color, it is transparent or translucent, so that the user can identify the temperature state of the current temperature-conducting workpiece through different colors.
[0059] S34: spray the second color paint on the thermochromic paint layer, so that the second color paint layer is formed on the surface of the thermochromic paint layer. Specifically, in the present embodiment, the second color paint is silver paint, and in other embodiments, the second color paint may also be other colors. The second color paint is evenly sprayed on the surface of the thermochromic paint layer, so that the second color paint is tightly and firmly connected to the thermochromic paint layer. Furthermore, the thermochromic paint layer is baked after the second color paint is sprayed, so that the second color paint can be cured on the surface of the thermochromic paint layer to form a second color paint layer, and is tightly connected to the thermochromic paint layer, wherein the baking temperature is 80℃~90℃, the baking time is 20min~40min, and the viscosity of the second color paint is 10.5S~11.5S; preferably, the baking temperature is 85℃, the baking time is 30min, and the viscosity of the second color paint is 11S. In other embodiments, the second color paint may also be pearlescent paint, which is also called mica paint. Mica is used instead of aluminum particles, and mica pigments coated with titanium dioxide and iron oxide are added to the paint base. When the light hits the mica particles, it takes on the colors of titanium dioxide and iron oxide, and then complex refraction and interference occur in the mica particles, so that users can see the second color paint reflecting complex, shiny light at different angles, thereby increasing the aesthetics of the product.
[0060] S35: Spray varnish on the second paint layer so that a varnish layer is formed on the surface of the second paint layer. Specifically, the varnish is, for example, UV paint, which is a photocurable paint, also known as a photosensitive paint. The UV paint is evenly sprayed on the surface of the second paint layer so that the UV paint is tightly and firmly connected to the second paint layer. Furthermore, the second paint layer is baked after the UV paint is sprayed, so that the UV paint can be cured on the surface of the second paint layer to form a varnish layer, and is tightly connected to the second paint layer, wherein the baking temperature is 55°C to 65°C, the baking time is 3min to 8min, and the viscosity of the varnish is 8.5S to 9.5S; preferably, the baking temperature is 60°C, the baking time is 5min, the viscosity of the varnish is 9S, and the UV light energy is 850Mj / Cm 2 After curing, UV paint will become hard, smooth, and transparent. It is also scratch-resistant, acid-resistant, and not easily deformed. It can also clearly show the color of the second paint layer, the thermochromic paint layer, or the first paint layer.
[0061] The thickness of the primer layer is 19 μm to 25 μm, the thickness of the first color paint layer is 29 μm to 35 μm, the thickness of the thermochromic paint layer is 33 μm to 40 μm, the thickness of the second color paint layer is 5 μm to 8 μm, and the thickness of the clear coat layer is 20 μm to 30 μm. Preferably, the thickness of the primer layer is 22 μm, the thickness of the color paint layer is 32 μm, the thickness of the thermochromic paint layer is 36.5 μm, the thickness of the second color paint layer is 6.5 μm, and the thickness of the clear coat layer is 25 μm.
[0062] like Figure 3 As shown, step S34 includes:
[0063] S341: Carve an open-pore structure on the second color paint layer, and the open-pore structure penetrates the second color paint layer in the thickness direction, so that the portion of the thermochromic paint layer corresponding to the open-pore structure is exposed. Preferably, the open-pore structure is made by 3D laser engraving technology, and the open-pore structure can be designed with various styles of texture patterns to increase the design aesthetics of the product. The open-pore structure exists under the UV paint layer and has no feel to the touch. The silver layer is laser engraved to expose the thermochromic paint, and the thermochromic paint can show different colors through temperature changes. When the temperature is low, the thermochromic paint is colored, and the laser engraved pattern is blue. When the temperature is high, the thermochromic paint does not show color, exposing the orange color of the bottom layer, and the laser engraved pattern is orange.
[0064] like Figure 4As shown, the present application also provides a temperature-conducting workpiece 10, which is made by the above-mentioned surface treatment process, and the temperature-conducting workpiece 10 can be applied to products that require temperature adjustment. The temperature-conducting workpiece 10 includes a metal substrate 12, a passivation layer 14, an adhesion enhancement layer 16 and a paint layer connected in sequence, wherein the paint layer includes a primer layer 18, a first color paint layer 20, a thermochromic paint layer 22, a second color paint layer 24 and a varnish layer 26 connected in sequence, wherein the second color paint layer 24 is engraved with an open hole structure (not shown) by a 3D laser engraving process, so that the portion of the thermochromic paint layer 22 corresponding to the open hole structure is exposed, and the present application does not limit the style of the open hole structure. In this embodiment, the primer layer 18 is white; the first color paint layer 20 is orange; the second color paint layer 24 is silver; the clear varnish layer 26 is a transparent UV paint; the second color paint layer formed after the second color paint is cured will cover the thermochromic paint layer. Therefore, the color of the first color paint layer or the thermochromic paint layer can only be seen from the second color paint layer through the open hole structure, that is, the color of the first color paint layer or the thermochromic paint layer can be seen from the outside, and the part outside the open hole structure appears silver. Specifically, the thermochromic paint layer 22 changes color according to the temperature of the temperature-conducting workpiece 10. For example, when the product is cooling, the temperature of the temperature-conducting workpiece 10 is low, and the thermochromic paint layer 22 appears as a first color, for example, blue, and the blue color of the thermochromic paint layer 22 shines through the open-pored structure, so that a blue texture pattern appears from the outside; when the product is heating, the temperature of the temperature-conducting workpiece 10 is high, and the thermochromic paint layer 22 loses color. For example, at this time, the thermochromic paint layer 22 is transparent or translucent, so that the second color of the first color paint layer 20 is revealed. The second color is orange, for example. The orange color of the first color paint layer 20 shines through the thermochromic paint layer 22 and shines through the open-pored structure, so that an orange texture pattern appears from the outside, which increases the coolness of the product and allows users to identify the current temperature state of the temperature-conducting workpiece according to the different colors presented by the paint layer.
[0065] The present application also provides a portable thermostat, which includes a shell, a thermostat disposed in the shell, and a thermally conductive part connected to the thermostat by thermal conduction. The thermal conductive part is the above-mentioned thermal conductive workpiece, which is disposed on the outer surface of the shell for contacting with the user's skin to achieve cooling or heating. The thermostat is, for example, a semiconductor refrigeration sheet. When the thermostat is powered on, the cold energy generated by the thermostat is transferred to the thermal conductive workpiece. When the human skin contacts the thermal conductive workpiece, the thermal conductive workpiece can transfer the cold energy to the human skin to achieve heat dissipation and cooling of the human body. Similarly, by changing the direction of the current inside the thermostat, the thermostat can also generate heat and transfer the heat to the thermal conductive workpiece, which then transfers the heat to the human skin to achieve heating of the human body.
[0066] Preferably, the shell is in an arc shape adapted to be worn on the human neck, so that the portable thermostat can be worn on the human neck, and the temperature-conducting workpiece can be arranged on the side of the shell close to the wearing space, so as to contact the human neck skin. The portable thermostat can also include a heat sink, which is fixedly connected to the shell and thermally connected to the thermostat. When the thermostat is working, the cold generated by the thermostat is transferred to the temperature-conducting workpiece, and the heat generated by the thermostat is transferred to the heat sink, which dissipates the heat outside the shell. With the assistance of the heat sink, a heat dissipation fan can be arranged to blow air to the heat sink to dissipate heat, so that the heat of the thermostat can be dissipated outside the shell in time, thereby improving the working efficiency of the thermostat. Furthermore, a fan can be arranged in the shell, and an air outlet is arranged on the shell corresponding to the fan. The wind generated by the fan is blown out from the air outlet, which can further improve the temperature control effect of the portable thermostat.
[0067] In summary, the present application provides a temperature-conducting workpiece, a surface treatment process thereof, and a portable temperature control device, wherein the metal substrate is first pre-treated to obtain a pre-treated workpiece, and then a treatment agent is sprayed on the pre-treated workpiece to form an adhesion enhancement layer on the surface of the pre-treated workpiece, and finally paint is sprayed on the adhesion enhancement layer to form a paint layer on the surface of the adhesion enhancement layer to obtain a temperature-conducting workpiece, wherein the adhesion enhancement layer is used to enhance the adhesion of the paint layer on the pre-treated workpiece, so that the paint layer can be firmly and tightly attached to the pre-treated workpiece, greatly improving the problems of bubbling and falling off of the paint layer, extending the service life of the paint layer, enhancing the corrosion resistance of the product, and improving the appearance and quality of the product, thereby enhancing the competitiveness of the product.
[0068] The concepts described herein may be implemented in other forms without departing from their spirit and characteristics. The specific embodiments disclosed should be considered illustrative rather than restrictive. Therefore, the scope of this application is determined by the appended claims rather than by the preceding description. Any changes within the literal meaning and equivalent scope of the claims should fall within the scope of these claims.
Claims
1. A surface treatment process for a temperature-conducting workpiece, characterized in that: The following steps are involved: S1: providing a metal substrate and pre-treating the metal substrate to obtain a pre-treated workpiece; S2: spraying a treatment agent on the pre-treated workpiece so that an adhesion enhancement layer is formed on the surface of the pre-treated workpiece; and S3: spraying paint on the adhesion enhancement layer so that a paint layer is formed on the surface of the adhesion enhancement layer to obtain a temperature conducting workpiece.
2. The surface treatment process for a temperature-conducting workpiece according to claim 1, characterized in that: The treating agent includes acrylic resin.
3. The surface treatment process for a temperature conducting workpiece according to claim 2, characterized in that: The treating agent comprises the following components in terms of mass percentage: 38-42% of polypropylene resin; 48-52% of toluene; and 8-12% of xylene.
4. The surface treatment process for a temperature conducting workpiece according to claim 1, characterized in that: The S3 includes: S31: spraying a primer on the adhesion enhancing layer so that a primer layer is formed on the surface of the adhesion enhancing layer; S32: spraying a first color paint on the primer layer, so that a first color paint layer is formed on the surface of the primer layer; S33: spraying a temperature-sensitive color paint on the first color paint layer, so that a temperature-sensitive color-changing paint layer is formed on the surface of the first color paint layer; S34: spraying a second color paint on the thermochromic paint layer, so that a second color paint layer is formed on the surface of the thermochromic paint layer; S35: spraying clear varnish on the second color paint layer, so that the clear varnish layer is formed on the surface of the second color paint layer.
5. The surface treatment process for a temperature conducting workpiece according to claim 4, characterized in that: The S34 includes: S341: Carving an open hole structure on the second color paint layer so that a portion of the thermochromic paint layer corresponding to the open hole structure is exposed.
6. The surface treatment process for a temperature conducting workpiece according to claim 4, characterized in that: The S2 comprises: spraying the treatment agent on the pre-treated workpiece and then baking to obtain the adhesion enhancement layer, the baking temperature is 80° C. to 90° C., and the baking time is 12 min to 18 min; The S31 comprises: spraying the primer on the adhesion enhancement layer and then baking to obtain the primer layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the primer is 11.9S to 12.9S; The S32 comprises: spraying the first color paint on the primer layer and then baking to obtain the first color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the first color paint is 11.9S to 12.9S; The S33 comprises: spraying the first color paint layer with the temperature-sensitive color paint and then baking to obtain the temperature-sensitive color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the temperature-sensitive color paint is 12.2S to 13.2S; The S34 includes: spraying the second color paint on the thermochromic paint layer and then baking to obtain the second color paint layer, the baking temperature is 80° C. to 90° C., the baking time is 20 min to 40 min, and the viscosity of the second color paint is 10.5S to 11.5S; The S35 comprises: spraying the varnish on the second color paint layer and then baking to obtain the varnish layer, the baking temperature is 55° C. to 65° C., the baking time is 3 min to 8 min, and the viscosity of the varnish is 8.5S to 9.5S.
7. The surface treatment process for a temperature conducting workpiece according to claim 4, characterized in that: The thickness of the adhesion enhancement layer is 2μm to 8μm, the thickness of the primer layer is 19μm to 25μm, the thickness of the first color paint layer is 29μm to 35μm, the thickness of the thermochromic paint layer is 33μm to 40μm, the thickness of the second color paint layer is 5μm to 8μm, and the thickness of the varnish layer is 20μm to 30μm.
8. The surface treatment process for a temperature conducting workpiece according to claim 1, characterized in that: The pre-processing in S1 includes: S11: die-casting the metal substrate; S12: performing a whitening treatment on the die-cast metal substrate to remove impurities on the surface of the metal substrate; S13: performing a passivation treatment on the metal substrate after the whitening treatment, so that a passivation layer is formed on the surface of the metal substrate, and the adhesion enhancement layer is connected to the passivation layer.
9. A temperature conducting workpiece, characterized in that: The temperature conducting workpiece is prepared by the surface treatment process described in any one of claims 1 to 8.
10. A portable temperature control device, characterized in that: It comprises a shell, a temperature regulating component arranged in the shell, and a temperature conducting component thermally connected to the temperature regulating component, wherein the temperature conducting component is arranged on the outer surface of the shell, and the temperature conducting component is the temperature conducting workpiece as claimed in claim 9.
11. The portable temperature control device according to claim 10, characterized in that: The paint layer includes a primer layer, a first color paint layer, a thermochromic paint layer, a second color paint layer and a clear paint layer. The second color paint layer is engraved with an open hole structure. The thermochromic paint layer changes color by sensing the temperature of the temperature conducting workpiece. When the thermostatic component is cooling, the thermochromic paint layer presents a first color; when the thermostatic component is heating, the thermochromic paint layer fades or presents a second color.