Method for resource utilization of lime slag hazardous waste
Through the gasification reaction of lime slag and raw coal, low melting point slag can be used for road construction and crude gas for chemical industry, which solves the high cost and environmental pollution problems in the treatment of hazardous waste of lime slag and achieves resource efficiency. utilization and environmental benefits.
Patent Information
- Application Number
- CN202310333654.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
The existing lime slag hazardous waste treatment technology has problems such as high cost, large energy consumption, serious environmental pollution and waste of resources. Moreover, the traditional landfill process is not environmentally friendly and cannot realize resource utilization.
Lime slag is mixed with raw coal for gasification reaction to generate crude gas and low melting point slag. The latter can be used for road construction, and the crude gas can be used for chemical industry or fuel, avoiding secondary pollution and waste of resources.
It achieves efficient cracking and resource utilization of lime slag, reduces processing costs, improves environmental benefits, reduces environmental pollution, and the process is simple and easy to implement.
Smart Images

Figure CN118719780A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a solid waste treatment method, in particular to a method for resource utilization of lime slag hazardous waste, and belongs to the field of comprehensive waste utilization and environmental protection. Background Art
[0002] A lime milk plant uses quicklime as raw material to produce lime milk, and produces a large amount of lime slag as a by-product. Lime slag has high water content and strong alkalinity, and is defined as solid hazardous waste. At present, the technologies for treating lime slag hazardous waste mainly include chemical solidification, thermal treatment and physical solidification.
[0003] Chemical solidification is to mix lime slag with a curing agent and form a solid similar to concrete through chemical reaction, so as to achieve the purpose of stabilizing hazardous waste. This method can not only reduce the volume of waste, but also reduce the toxicity of pollutants and improve the stability of lime slag. However, chemical solidification requires the use of a large amount of curing agent, which increases the treatment cost.
[0004] Thermal treatment uses high-temperature pyrolysis to thermally decompose lime slag, thereby achieving the purpose of stabilizing hazardous waste. This method can completely decompose organic pollutants and harmful substances and reduce the impact of lime slag on the environment. For example, a company uses high-temperature incineration to treat lime slag. Through the storage, drying, calcination and other processes of lime slag, the recycled calcium oxide (i.e. lime) is widely used in the construction industry, achieving pollution-free treatment of lime slag and beneficial to environmental protection. However, thermal treatment consumes a lot of energy, which will increase processing costs and carbon emissions.
[0005] Physical solidification is to compact the lime slag into a dense granular material to achieve the purpose of hazardous waste treatment. This method can reduce the volume of waste and reduce treatment costs. However, physical solidification cannot reduce the toxicity of pollutants and requires other methods of treatment.
[0006] In addition, the use of landfill technology to bury hazardous solid waste in special landfills cannot be directly utilized as resources, the treatment cost is high, and it is not environmentally friendly. The treatment cost is high, the area occupied is large, and it is easy to infiltrate and pollute groundwater. The traditional lime slag treatment method not only wastes resources, but also causes serious pollution to the soil, water and other environments. The current development trend of lime slag hazardous waste treatment technology should be to combine a variety of treatment technologies, such as comprehensive utilization, resource utilization, and greening, to reduce the volume of waste and pollution to the environment, while achieving a win-win situation of economic and social benefits. The continuous development of lime slag hazardous waste treatment technology will help promote the sustainable development of industrial production and environmental protection. Therefore, finding an efficient lime slag treatment method is of great significance for sustainable development. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention aims to provide a method for recycling hazardous waste lime slag. The method is simple, low-cost, does not cause secondary pollution, and has high practical value.
[0008] In order to achieve the above technical objectives, the present invention provides a method for resource utilization of lime slag hazardous waste, which comprises mixing lime slag and raw coal to obtain pulverized coal, and then placing the pulverized coal in a gasifier for gasification reaction to obtain raw coal gas.
[0009] The present invention mixes lime slag with high ash melting point raw coal to make it meet the quality standard of pulverized coal gasifier for coal entering the furnace, and produces raw coal gas through gasification reaction in the gasifier. The lime slag can be completely cracked in the gasifier, which greatly reduces the processing cost and improves the environmental protection benefit. The lime slag acts as a flux and reacts with the ash in the coal to generate low melting point slag, which is finally discharged from the gasifier in the form of slag. The pH value of the slag is neutral and can be used for road construction, further improving the resource utilization efficiency.
[0010] As a preferred solution, the mass ratio of the lime slag to the raw coal is 1 to 10:80 to 100. By controlling the mixing ratio of the lime slag and the raw coal within a reasonable range, it is possible to ensure that the ash content, ash melting point, potassium and sodium content in the ash, silicon-aluminum ratio (mass percentage ratio of SiO2 to Al2O3) and calcium oxide content of the pulverized coal formed thereby meet the quality requirements of the entrained-flow pulverized coal water-cooled wall gasifier for the raw materials entering the furnace.
[0011] As a preferred solution, the lime slag contains calcium oxide, silicon dioxide and aluminum oxide components, and the content of calcium oxide is not less than 65wt%, and the total content of silicon dioxide and aluminum oxide is not less than 15wt%.
[0012] The composition of lime slag affects the properties of the pulverized coal material formed. The lime slag with this composition can be well mixed with the raw coal to improve the gasification efficiency.
[0013] Calcium oxide can reduce the ash melting point of pulverized coal. When the calcium oxide content is lower than 65wt%, the gasifier is prone to slag blockage. Too low content of silicon dioxide and aluminum oxide will affect the silicon-aluminum ratio of pulverized coal, thereby affecting the temperature operating space of the gasifier, which may cause fluctuations in the process operation of the gasifier and cause shutdown.
[0014] As a preferred solution, the lime sludge further contains water, and the water content does not exceed 15wt%.
[0015] As a preferred solution, the particle size of the lime slag is ≤70 μm.
[0016] As a preferred solution, the mass ratio of SiO2 to Al2O3 in the raw coal is less than 1.5: 1. The silicon-aluminum ratio in the raw coal is controlled within a suitable range so that it can be adapted to the lime slag and improve the gasification reaction efficiency.
[0017] As a preferred solution, the ash melting point of the pulverized coal is 1180-1400°C, more preferably 1280-1450°C.
[0018] As a preferred solution, the particle size of the pulverized coal is 10 to 200 μm, more preferably 10 to 100 μm.
[0019] As a preferred solution, the calcium oxide content in the ash of the pulverized coal is 5-15wt%, the mass ratio of SiO2 to Al2O3 is 1.5-3.5:1, and the total content of potassium oxide and sodium oxide is 1-3wt%. More preferably, the calcium oxide content in the ash of the pulverized coal is 8-13wt%.
[0020] As a preferred solution, the conditions of the gasification reaction are: pressure of 5.2-7.2 MPaG and temperature of 1350-1600°C.
[0021] As a preferred solution, the raw coal gas contains carbon monoxide, methane, hydrogen and carbon dioxide.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) By mixing the lime slag hazardous waste with raw coal, the lime slag can be cracked through gasification reaction. The low melting point slag produced can be directly used for road construction. At the same time, the raw coal gas produced can be used as raw materials for chemical enterprises or civil fuel. It does not emit gas to the atmosphere and does not affect the environment, thus generating excellent economic benefits and environmental protection responsibilities;
[0024] (2) Raw materials are easily available, the process is simple, no other raw and auxiliary materials need to be added, and there is no need to set up waste recovery and treatment processes. The treatment cost is low, simple and efficient;
[0025] (3) The lime slag is fully gasified under high temperature and weak reduction conditions, which does not cause waste of organic matter and secondary environmental pollution, does not affect the operation of existing processes, and has strong system adaptability;
[0026] (4) It effectively transforms lime slag hazardous waste into treasure, reduces the harm to the environment caused by landfill disposal of hazardous waste, and improves resource utilization efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the process flow chart of Example 1. DETAILED DESCRIPTION
[0028] The present invention will be further described below by way of examples, which are not intended to further limit the content of the present invention. Those skilled in the art should understand that equivalent replacements made to the technical features of the present invention, or corresponding improvements, still fall within the protection scope of the present invention.
[0029] The lime slag composition analysis data used in the present invention are as follows:
[0030] raw materials Analysts <![CDATA[SiO2]]> <![CDATA[Al2O2]]> <![CDATA[Fe2O3]]> CaO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[P2O5]]> Lime slag XRF 15.30 5.03 1.21 75.15 0.36 0.68 0.16 0.11
[0031] Example 1
[0032] The lime slag is first commissioned to other factories to be ground into particle sizes between 10-70um, loaded and unloaded by tank trucks, and transported to the lime slag silo with nitrogen. The lime slag is mixed with high ash melting point raw coal, and the ash melting point of the pulverized coal gasifier is prepared in a medium-speed coal mill to meet the quality standards of the pulverized coal gasification furnace. Then it is transported to the pulverized coal gasifier through the pulverized coal lock hopper system for gasification reaction to generate high-temperature and high-pressure raw coal gas.
[0033] The raw coal is mixed with lime slag and ground into pulverized coal. The specific formula of various material specifications is shown in Table 1, the properties of raw coal.
[0034] Table 1
[0035] raw materials Specification Mass(g) Remark Raw coal HM178+158+152(1:1:1) 300 Outsourcing Lime slag Median diameter D50 3.6 Self-produced hazardous waste
[0036] Table 2
[0037]
[0038] Table 3
[0039]
[0040] Table 3 shows the raw material ash analysis. The results are calculated by the coal blending software. The ash content is 15.65% after adding 1.2% powdered lime slag. The FT is between 1390-1420℃. The gasification reaction pressure is controlled to be 5.2-7.2MPaG. The temperature of the gasification reaction is about 1400℃, which meets the quality standard of the coal entering the furnace. The effective gas load is estimated to be 96%-98%. Most of the carbon is converted into effective components carbon monoxide and hydrogen, and a small amount is converted into carbon dioxide and hydrogen sulfide. The specific raw coal gas composition test is shown in Table 4.
[0041] Table 4
[0042]
[0043] Comparative Example 1
[0044] The method of Example 1 is used to prepare raw coal gas, except that limestone powder is mixed with raw coal and ground into pulverized coal. The specific formula of various material specifications of this comparative example is shown in Table 5.
[0045] Table 5
[0046] raw materials Specification Mass(g) Remark Pulverized coal HM178+158+152(1:1:1) 300 Outsourcing Limestone powder Median diameter D50 3.6 Self-produced hazardous waste
[0047] Among them, the composition of limestone powder is shown in Table 6.
[0048] Table 6
[0049] raw materials Analysts <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[P2O5]]> limestone XRF 0.98 1.32 0.96 94.51 0.10 0.48 0.50 0.01
[0050] Table 7
[0051]
[0052] Table 7 shows the ash analysis of the mixture of limestone and raw coal, where the contents of SiO2 and Al2O3 in limestone are 0.98 and 1.32, respectively, and the main component is GaO3. The coal blending software calculates that the ratio of HM 187:155:152 (1:1:1): limestone powder, and the silicon-aluminum ratio of pulverized coal is 1.45:1, which does not meet the requirements of the silicon-aluminum ratio of the coal entering the furnace (1.5-3.5:1), and coal gas preparation cannot be performed. From the results of this comparative example, it can be seen that since lime slag and raw coal have special components, their reasonable blending can meet the requirements of the coal entering the pulverized coal gasifier.
[0053] Comparative Example 2
[0054] The lime slag produced by the lime milk device is treated by landfilling, and the treatment cost is about 1,000 yuan / ton. The storage capacity of the dedicated solid hazardous waste landfill is 50,000 tons, while the output of lime slag is 3,000 tons / year. After 15 years, the dedicated solid hazardous waste landfill can no longer operate, and it will pollute groundwater and damage the ecological environment.
Claims
1. A method for recycling hazardous waste lime slag, characterized in that: The lime slag and raw coal are mixed to obtain pulverized coal, and the pulverized coal is then placed in a gasifier for gasification reaction to obtain raw coal gas.
2. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The mass ratio of the lime slag to the raw coal is 1-10:80-100.
3. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The lime slag contains calcium oxide, silicon dioxide and aluminum oxide components, wherein the content of calcium oxide is not less than 65wt%, and the total content of silicon dioxide and aluminum oxide is not less than 15wt%.
4. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The lime mud further contains water, and the content of water does not exceed 15wt%.
5. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The particle size of the lime slag is ≤70 μm.
6. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The mass ratio of SiO2 to Al2O3 in the raw coal is less than 1.5:
1.
7. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The ash melting point of the pulverized coal is 1180-1400° C.; the particle size of the pulverized coal is 10-200 μm.
8. The method for recycling hazardous waste lime slag according to claim 1 or 7, characterized in that: In the ash of the pulverized coal, the content of calcium oxide is 5-15wt%, the mass ratio of SiO2 to Al2O3 is 1.5-3.5:1, and the total content of potassium oxide and sodium oxide is 1-3wt%.
9. The method for recycling hazardous waste lime slag according to claim 1, characterized in that: The conditions of the gasification reaction are: pressure of 5.2-7.2 MPaG and temperature of 1350-1600°C.
10. A method for recycling hazardous waste lime slag according to claim 1 or 9, characterized in that: The raw gas contains carbon monoxide, methane, hydrogen and carbon dioxide.
Citation Information
Patent Citations
Method for lowering fusing temperature of coal ash
CN105542901A
Hazardous waste treatment method
CN113217915A
Process for producing coal gas
DE3507635A1
Method for gasifying carbonaceous raw material
JP2007231203A
Catalytic gasification method of coal
KR1019900006486A