Mixed 3D printing process combining metal powder bonding 3D printing with precision casting
By designing a feeding structure and using a high-temperature-resistant shell in the metal powder bonding 3D printing process, the sintering reaches above the melting point of the metal, which solves the problems of low strength and poor consistency of parts in the existing technology, and achieves high strength and high strength of parts. High qualification rate production.
Patent Information
- Application Number
- CN202410740253.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
AI Technical Summary
The existing metal powder adhesive spraying process results in low structural strength of parts, poor strength performance consistency, and low qualification rate. This is mainly due to high porosity and uncertain distribution, deformation risk and difficulty in strength performance control during the sintering process.
A hybrid 3D printing process using metal powder bonding 3D printing and precision casting is used to design a feeding structure. A high-temperature-resistant shell is set outside the green body. During sintering, the temperature reaches above the melting point of the metal. A solid shell is formed by wrapping it with castables or ceramic sand. Eliminates internal pores and increases density and strength.
It significantly improves the structural strength and strength performance consistency of parts, reduces deformation, improves the pass rate, and ensures high-quality production of parts.
Smart Images

Figure CN118720161A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal powder binder spray additive manufacturing. Background Art
[0002] Metal powder binder jetting is a 3D printing process that uses a liquid binder to bond powdered metal material layer by layer to create a robust and complex shape (green). Finally, through sintering and post-processing, the desired metal part is obtained.
[0003] Compared to traditional metal injection molding and other forms of metal 3D printing, metal powder binder jetting offers several advantages: 1) Wide range of material choices: The metal powder binder jetting process is compatible with a wide variety of currently available metal powder materials. Theoretically, binder jetting can be used with any powdered metal material and binder liquid. 2) Cold working: The metal powder binder jetting printing process is performed at room temperature, avoiding problems associated with thermal residual stress and allowing unbonded powder around the part in the build box to be recycled, thus saving material costs. 3) Large print volume: Due to the absence of thermal residual stress effects, metal powder binder jetting allows for large print table volumes. This makes it possible to print single large parts or combine many different parts into a single print run. 4) No supports: For any part geometry produced by binder jetting, the powder bed typically provides sufficient support, meaning greater design freedom (especially for creating internal channels), less material waste, and less time and labor for removing supports. 5) High speed: Binder jetting is fast and productive, allowing for the cost-effective production of large quantities of parts. 6) Multifunctional output: Binder spraying can produce various densities with controlled porosity according to sintering temperature and time, thus having a wide range of applications.
[0004] Although existing metal powder binder spraying processes have many advantages as mentioned above, they still have some shortcomings, mainly including the following:
[0005] 1) The resulting metal powder parts (green blanks) have high porosity: The metal powder binder jet printing process is essentially a layer-by-layer stacking of powder. Therefore, due to the limitation of powder packing density, the printed metal powder parts (green blanks) have a large porosity (15%-40%), resulting in low structural strength of the parts.
[0006] 2) Uncertainty exists in the porosity distribution of metal powder parts (green blanks): The porosity of metal powder parts (green blanks) printed by metal powder binder jet printing is affected by multiple factors such as powder, powder spreader, binder, powder flowability, and environmental parameters, resulting in a significant random distribution. Even parts of the same specification printed at different locations on the same machine exhibit density differences. Similarly, parts of the same specification printed at the same location but in different batches also show density differences. Furthermore, parts of the same specification printed at the same location on different machines also exhibit density differences. This poses a significant challenge to controlling the strength performance of the parts, leading to poor consistency in their strength properties.
[0007] 3) Deformation Risk: To make the metal powder parts (green blanks) printed with metal powder binders more compact, a heat treatment process (sintering) is required. The sintering temperature is lower than the melting point of the metal powder, generally 90% of the melting point, to increase the strength of the green blank. Due to the uncertainty of the porosity distribution of the metal powder parts (green blanks), uneven shrinkage and geometric deformation will occur during the sintering process. This cannot be avoided by design and pre-calculation alone, and it is particularly serious for large-sized parts with large differences in wall thickness, resulting in a low yield rate.
[0008] 4) Difficulty in controlling the consistency of part strength performance: The thermal field distribution and temperature profile of the sintering furnace directly affect the sintering results. In actual production, metal powder parts (green blanks) themselves have differences in composition, particle size distribution, binder composition and ratio, and porosity distribution. These differences, combined with the differences in the thermal field of the sintering furnace and the heat transfer of the green blank, along with the process parameters (temperature profile) during sintering, lead to difficulties in controlling the strength performance of the sintered parts. Even with the same metal material and printing parameters, placing them in different positions within the same sintering furnace and using the same temperature profile will result in different strength performances for the parts.
[0009] Therefore, the existing metal powder binder spraying process has the defects of low structural strength, poor consistency of strength performance and low pass rate of the resulting parts. Summary of the Invention
[0010] The purpose of this invention is to provide a hybrid 3D printing process that combines metal powder bonding 3D printing with precision casting. This invention offers advantages such as high structural strength, good consistency in strength performance, and a high yield rate for the resulting parts.
[0011] The technical solution of this invention: a hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, comprising the following sequential steps,
[0012] a. Design the feeding structure according to the shape of the part. Based on the porosity, wall thickness distribution and metal solidification sequence of the 3D printed part using metal powder binder jetting, determine the size, quantity and location of the feeding structure to obtain the design drawing.
[0013] b. Based on the design drawings, a green part is obtained using a metal powder binder jet 3D printing process. The green part has an integrally formed shrinkage compensation structure.
[0014] d. A high-temperature resistant shell is installed on the outside of the green blank.
[0015] e. Place the green billet according to the feeding direction of the feeding structure, sinter the green billet, so that the green billet temperature reaches above the melting point of the metal powder, the density of the green billet is increased, and after the green billet cools, it is taken out and sorted to obtain the finished product.
[0016] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, step d involves placing the green blank into a mold with venting holes, pouring castable into the mold to embed the green blank within it, and then firing the mold after the castable has solidified to remove excess moisture. This hardens the castable within the mold, causing the binder in the green blank to vaporize. The hardened castable forms a shell enveloping the green blank.
[0017] Alternatively, the green body can be repeatedly coated with slurry and sprayed with ceramic sand, so that the cured ceramic sand forms a shell that encapsulates the green body.
[0018] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, in step a, the total volume of the compensation structure is 0.101 times the volume of the part.
[0019] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, there is a step c between step d and step d. In step c, the metal powder that is not firmly bonded on the green blank is first cleaned, then the green blank is immersed in wax, and then the excess wax is removed to improve the surface finish of the green blank.
[0020] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, the mold in step d is box-shaped.
[0021] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, in step d, the mold is sintered in a sintering furnace according to the corresponding temperature curve.
[0022] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, the sintering method in step e is electromagnetic induction heating.
[0023] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, in step e and step d, the calcination method is any one, two or more combinations of microwave heating, natural gas heating and electric heating.
[0024] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, in step f, the mold on the outside of the green blank is first removed, and then the green blank along with the solidified casting material is placed in a vacuum or protective gas environment for sintering, with electromagnetic induction heating used during sintering.
[0025] In the aforementioned hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, in step d, when the green blank is embedded in the castable, if the green blank material is aluminum alloy and the castable contains a reducing agent;
[0026] Alternatively, when repeatedly applying slurry and spraying ceramic sand onto green bodies, if the green body material is aluminum alloy and the slurry contains a reducing agent.
[0027] Compared with existing technologies, this invention creatively combines the existing metal powder binder jet 3D printing process with precision thermoforming technology. A shrinkage-compensating structure is integrally printed on the green blank, and a high-temperature resistant shell is set on the outside of the green blank. During heat treatment, the green blank melts, greatly eliminating the internal porosity, significantly increasing density, and substantially enhancing structural strength. Because the resulting part has extremely low internal porosity, it exhibits good density consistency throughout, resulting in consistent strength performance. Since the heat treatment is performed on the solidified castable, the deformation of the heat-treated part is minimal, significantly increasing the yield rate. In summary, this invention has the advantages of high structural strength, good strength performance consistency, and a high yield rate. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the green body in Example 1.
[0029] Figure 2 This is the process route diagram for step c in Example 1.
[0030] Figure 3 This is a schematic diagram of the process of embedding the green body in step d of Example 1.
[0031] Figure 4 This is a schematic diagram of the green body after embedding in step d of Example 1.
[0032] Figure 5 This is a schematic diagram of the green body firing in step d of Example 1.
[0033] Figure 6 This is a microscopic schematic diagram of the green body firing process in step d of Example 1.
[0034] Figure 7 This is a microscopic schematic diagram of the green body firing process in step d of Example 1.
[0035] Figure 8 This is a schematic diagram of the green blank after sintering in step e of Example 1.
[0036] Figure 9 This is a schematic diagram illustrating the sintering process of the green blank in Example 1.
[0037] Figure 10 This is a schematic diagram of the green blank in Example 6.
[0038] Figure 11 This is a process route diagram for step d of Example 6, which involves repeated slurry application and spraying of ceramic sand.
[0039] The labels in the attached diagram are: 1-part, 2-shrinkage structure, 3-mold. DETAILED DESCRIPTION
[0040] The present invention will be further described below with reference to the accompanying drawings and embodiments, but this should not be construed as limiting the present invention.
[0041] Example 1. A hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, comprising the following sequential steps:
[0042] a. Design the feeding structure 2 (riser) according to the shape of part 1. Part 1 in Example 1 is a skin lattice structure. Based on the porosity, wall thickness distribution and metal solidification sequence of the part printed by metal powder binder jetting 3D printing, determine the size, quantity and position of the feeding structure 2 on the part to obtain the design drawing. In the design drawing, the part is scaled down according to the specific material shrinkage rate of the metal powder.
[0043] The total volume v' of the compensation structure is calculated using this formula: v' = 0.101v, where v is the volume of the part. This formula is an empirical formula derived by quantifying the shrinkage rate of metal casting and the porosity of metal powder binder spraying. The significance of this formula is to reduce the trial production cycle and cost for non-standard prototypes using this process route.
[0044] b. Based on the design drawings, using a metal powder binder jet 3D printing process, the following is obtained: Figure 1 The green blank of part 1 shown has multiple shrinkage compensation structures 2 integrally formed on it.
[0045] c. For example Figure 2 As shown, first, any loosely bonded metal powder on the green blank is cleaned, then the green blank is impregnated with wax, and finally excess wax is removed to improve the surface finish of the green blank and prevent the castable from penetrating the surface of the green blank during the embedding process in step d. Because the metal powder binds to create a porous surface on the green blank, if directly embedded, these pores would be filled with castable, causing the castable to penetrate the original surface of the green blank. However, after wax impregnation, the green blank surface is isolated from the castable by the wax, resulting in a high surface finish on the final part.
[0046] d. For example Figure 3 and Figure 4 As shown, the green body is placed in a box-shaped mold 3 with vent holes. Castable refractory is poured into the mold 3 to embed the green body in the castable refractory. The castable refractory is a wet material of gypsum or clay. In order to facilitate the filling and compaction of the castable refractory, vibration compaction can be performed after the castable refractory is poured into the mold 3, or a highly fluid castable refractory, such as self-leveling gypsum slurry, can be used.
[0047] When the parts are made of aluminum alloy, it is preferable to add an appropriate amount of reducing agent to the casting material (such as gypsum slurry or ceramic slurry). The role of the reducing agent is that, during the subsequent firing of the gypsum mold, the reducing agent reacts rapidly with the oxygen-containing substances in the gypsum after heating, reducing the oxide content in the gypsum and preventing oxygen from reacting with aluminum to form aluminum oxide in later steps. Aluminum oxide reduces the strength of the aluminum alloy casting, causing failure. If it is not added, the subsequent heating process will inevitably accelerate the oxidation reaction between oxygen and aluminum alloy, which is unavoidable.
[0048] like Figure 5 As shown, after the castable solidifies, the mold is fired in a furnace according to the existing and corresponding temperature curve. This removes excess moisture from the mold, hardens the castable inside mold 3, and vaporizes the binder in the green blank, forming a shell enveloping the green blank. The firing method is microwave heating, natural gas heating, or electric heating. The firing temperature is lower than the melting point of the metal powder but higher than the vaporization temperature of the binder. Heating according to the temperature curve can optimize the expansion and deformation of the castable, which is beneficial for controlling the dimensional accuracy of the parts.
[0049] e. With the mold and casting material retained, after the mold cools to 300-400°C, place the green blank according to the shrinkage direction of the shrinkage structure, with the shrinkage direction downwards. Sinter the green blank, raising the temperature above the melting point of the metal powder. The metal powder melts, forming a dense metal blank (containing part of the shrinkage structure) in the mold cavity occupied by the green blank. The green blank is composed of metal powder particles bonded together by a binder, with a wax layer on the surface. This means that there are metal particles, polymer binder, wax layer, and pores in the green blank mold cavity. After firing in step d, the binder vaporizes and escapes, and the fired green blank exhibits a structure where metal particles agglomerate and pores coexist. During the sintering process, the metal powder melts, and under the action of gravity, the metal of the shrinkage structure melts and flows out, filling the gaps between the metal powder particles in the mold cavity, thereby forming a dense metal part. As the temperature decreases, the metal solidifies sequentially, first the metal part solidifies, then the shrinkage structure (riser) partially solidifies, finally obtaining the desired dense part and some residual shrinkage structure. Remove the mold and casting material from the outside of the green blank, and machine the shrinkage compensation structure 2 on the green blank to obtain the finished part.
[0050] In step e, the sintering of the green blank must be carried out using electromagnetic induction heating, and the melting process of the green blank should be conducted in a vacuum or protective gas environment. In step e, if the mold temperature is too low, that is, the shell temperature is low, the metal will solidify immediately after melting and cannot flow sufficiently. Sintering must be done using electromagnetic induction. If traditional heating methods are used, it is difficult to heat the metal above its melting point due to the thermal conductivity of the shell. Electromagnetic induction utilizes the physical properties of metals, and the shell is non-metallic and cannot be heated during the sintering process. Therefore, the shell must be kept at a certain temperature.
[0051] Example 2. Compared with Example 1, the difference is that in step e, the mold 3 is placed in a centrifugal device for sintering, and at this time, the feeding direction is the direction of centrifugal force.
[0052] Example 3. Compared with Example 1, the difference is that in step e, the roasting method is any two or three combinations of microwave heating, natural gas heating and electric heating.
[0053] Example 4. Compared with Example 1, the difference is that in step e, after removing the mold and retaining the casting material, the green blank is placed in a vacuum or protective gas-filled environment for sintering.
[0054] Example 5. Compared with Example 1, in step c, the green blank does not undergo wax impregnation and dewaxing, which is suitable for the production of parts with low requirements for surface roughness.
[0055] Example 6. Unlike Example 1, the shape of part 1 in step a is different; in step d, the green blank is repeatedly coated with slurry and sprayed with ceramic sand, so that the cured ceramic sand forms a shell enveloping the green blank. If the green blank is made of aluminum alloy, an appropriate reducing agent is added to the slurry.
[0056] The main innovation of this invention is as follows: In existing processes, 3D-formed green blanks are directly sintered at a temperature generally around 90% of the melting point of the metal powder to reduce porosity and increase the strength of the resulting parts. However, since the pore distribution of the green blank is random during printing, the sintered parts have low structural strength and poor consistency in strength performance. Furthermore, during sintering, since the green blank is not supported, the sintering temperature must be below the metal melting point to avoid collapse. During sintering, the temperature field, temperature curve, and the internal void distribution of the green blank all affect the deformation of the green blank. However, all three are difficult to control or predict. Relying solely on design and advance calculation cannot effectively avoid deformation, resulting in large deformation of the parts. This invention creates a hard and fixed shell on the outside of the green blank before sintering. This allows the sintering temperature of the green blank to be increased above the melting point of the metal, allowing the green blank to melt and fill the cavity. The resulting part is essentially free of pores, has high structural strength and good consistency in strength performance. Furthermore, after the green blank melts and solidifies, the part is constrained by the shell and receives sufficient shrinkage compensation during solidification. The temperature field, temperature curve, and internal void distribution of the green blank do not affect the deformation of the part, eliminating unstable factors and resulting in minimal deformation of the final part.
Claims
1. A hybrid 3D printing process combining metal powder bonding 3D printing and precision casting, characterized by: The following steps are included: a. Design the feeding structure according to the shape of the part, determine the size, quantity and position of the feeding structure according to the porosity, wall thickness distribution and metal solidification sequence of the part printed by metal powder binder jet 3D printing, and obtain the design drawing; b. According to the design drawing, the metal powder adhesive jet 3D printing process is used to obtain the green body of the part, on which the shrinkage-feeding structure is integrally formed. d. A high temperature resistant shell is arranged on the outside of the green body. e. Place the green body according to the feeding direction of the feeding structure, sinter the green body so that the temperature of the green body reaches above the melting point of the metal powder, and the density of the green body is improved. After the green body is cooled, take it out and arrange it to obtain a finished product.
2. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 1, characterized in that: In the step d, the green body is placed in a mold with a vent hole, a casting material is poured into the mold, the green body is embedded in the casting material, and after the casting material solidifies, the mold is fired to remove excess water in the mold, the casting material in the mold is hardened, the binder in the green body is vaporized, and the hardened casting material forms a shell that wraps the green body. Alternatively, the green body is repeatedly slurried and sprayed with ceramic sand, so that the solidified ceramic sand forms a shell that wraps the green body.
3. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 1, characterized in that: In the step a, the total volume of the feeding structure is 0.101 times the volume of the part.
4. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 1, characterized in that: There is a step c between step b and step d. In step c, the metal powder that is not firmly bonded on the green body is first cleaned, the green body is dipped in wax, and then the excess wax is removed to improve the surface finish of the green body.
5. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 2, characterized in that: In the step d, the mold is box-shaped.
6. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 2, characterized in that: In the step d, the mold is fired in a furnace according to a corresponding temperature curve.
7. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 4, characterized in that: In the step e, the sintering method is electromagnetic induction heating.
8. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 2, characterized in that: In the step d, the roasting method is any one of microwave heating, natural gas heating and electric heating, or a combination of two or more of them.
9. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 2, characterized in that: In the step e, the mold outside the green body is first removed, and then the green body together with the solidified casting material is placed in a vacuum or protective gas environment for sintering, and electromagnetic induction heating is used during sintering.
10. The hybrid 3D printing process of metal powder bonding 3D printing combined with precision casting according to claim 2, characterized in that: In the step d, when the green body is embedded in the casting material, if the green body is made of aluminum alloy, the casting material contains a reducing agent; Alternatively, when the green body is repeatedly slurried and sprayed with ceramic sand, if the green body is made of aluminum alloy, the slurry contains a reducing agent.