Brazing process of diamond saw blade

By using mechanical and chemical cleaning, argon cooling and metal activation treatment in the diamond saw blade brazing process, the problems of poor flux fluidity and difficult cooling control are solved, and high-quality welding effects and saw blade stability are achieved.

CN118720310AInactive Publication Date: 2024-10-01HUBEI WANKE DIAMOND TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411018756.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing diamond saw blade brazing process, the poor fluidity of the flux leads to the risk of voids and incomplete penetration, and the air cooling method is difficult to control the welding temperature, which can easily lead to saw blade deformation.

Method used

Mechanical and chemical methods are used to clean the welding surface, high-purity argon gas cooling and a vacuum furnace are used for brazing, phosphorus is added to improve flux fluidity, and diamond particles are subjected to metal activation treatment to improve bonding strength.

Benefits of technology

It reduces the risk of voids and incomplete penetration, improves welding quality and strength, reduces the possibility of saw blade deformation, and ensures purity and efficient cooling of the welding area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720310A_ABST
    Figure CN118720310A_ABST
Patent Text Reader

Abstract

The invention discloses a brazing process for a diamond saw blade, and relates to the technical field of brazing processes, and the brazing process comprises the following steps: S1, cleaning a welding surface; s2, welding and assembling; s3, brazing in a vacuum furnace; s4, detecting a welding seam; according to the brazing process of the diamond saw blade, the fluidity of the brazing filler metal can be improved through the phosphorus element of the brazing flux, so that the brazing flux for brazing can easily flow and be filled after being heated, it is guaranteed that soldering tin can be evenly distributed in a welding area, the risks of cavities and incomplete penetration are reduced, and the welding quality is improved. And meanwhile, the diamond can be quickly spread to the whole welding area, so that the welding process is simplified and is simpler, more convenient and quicker, and meanwhile, the diamond surface is subjected to metal activation treatment, so that the surface has metalloid performance, and combination between the diamond and metal brazing filler metal is more facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of brazing technology, in particular to a brazing technology for a diamond saw blade. Background Art

[0002] In order to make the diamond particles firmly adhere to the saw blade substrate during processing, brazing is usually used for welding. After searching, the Chinese patent publication number CN102319934B discloses a brazing process for diamond saw blades. Although the diamond saw blades prepared by this process have low porosity, strong bonding between diamond and substrate, and high quality and stable yield, the brazing flux has poor fluidity, which leads to the risk of voids and incomplete penetration during welding. At the same time, the existing brazing cooling method uses air cooling as the cooling method, which makes the welding temperature difficult to control, and thus there is a risk of saw blade deformation. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a brazing process for diamond saw blades, which solves the problem in the background art that the brazing flux has poor fluidity, which easily leads to the risk of voids and incomplete penetration, and that air cooling is used as a cooling method, which easily leads to the risk of saw blade deformation.

[0004] To achieve the above objectives, the present invention is implemented by the following technical scheme: a brazing process for a diamond saw blade, S1: cleaning the welding surface; using mechanical methods and chemical methods to clean the oxide film, grease or other attachments in the area to be welded of diamond particles and knife grooves; the brazing area after surface cleaning should be kept clean, and when moving diamond particles, the operator should wear gloves, and it is forbidden to touch the area to be brazed of the metal substrate with oily dirt or bare hands, and use a clean cloth dipped in anhydrous ethanol or acetone to wipe the area to be brazed of the metal substrate;

[0005] S2: Welding assembly; then apply paste flux in the knife groove of the cutter body, place the brazing material and diamond particles in sequence, and apply another layer of flux between the brazing material and the diamond particles, place it in a high-frequency sound wave environment, select a vacuum furnace for brazing, and use induction heating fuzzy control and synchronous data acquisition system to control the heating temperature;

[0006] S3: Brazing in a vacuum furnace; using argon cooling, the purity of argon should be >99.9%; and the principle is to avoid cracks and minimize the internal stress of the brazed joint and the deformation of the metal matrix;

[0007] S4: Inspect the weld; after welding, measure the weld thickness with a stereo microscope, observe the weld microstructure with a JEOL JSM6360LV scanning electron microscope, and then test the shear strength on a shear strength measuring device.

[0008] Preferably, when brazing is performed in a vacuum furnace in S2, the vacuum furnace equipment is out of service for more than one month and needs to be dried. The drying furnace process parameters are: vacuuming to below 5x103Pa, heating for 60min-120min and heating to 1000°C-1200°C;

[0009] Preferably, after the temperature in the vacuum furnace stabilizes at the set temperature, it is kept warm for 5 minutes to 10 minutes, and then cooled to room temperature with the furnace. When the thickness of the diamond particle matrix is ​​large, the vacuum brazing furnace is heated to 20°C to 100°C below the melting temperature of the brazing material for insulation, and then heated to the brazing temperature for brazing after the temperature is uniform.

[0010] Preferably, the mechanical method in S1 is to sandblast or grind the weld, and the surface roughness of the weld after sandblasting or grinding is Ra6.5.

[0011] Preferably, the flux composition in the S2 is as follows: Ag 60-65%, Cu 20-25%, Ti 0.5%-1.5%, Si 5%-7%, P 1%-5%.

[0012] Preferably, the chemical cleaning method in S1 is to place the diamond particle substrate in an alkaline aqueous solution of 8-15wt% NaOH, 5-10wt% Na2CO3, 5-10wt% Na2SiO3 and 3-5wt% Na3PO4, at a cleaning temperature of 50-85°C for 10-20 minutes to remove the oil film on the surface, and then place the diamond particle substrate in an aqueous solution of 3-5wt% hydrochloric acid and 0.5-1.2wt% thiourea for pickling for 5-10 minutes to remove the oxide layer on the surface of the substrate.

[0013] Preferably, before welding in S2, the process further includes performing metal activation treatment on the surface of the diamond particles, and the method is as follows:

[0014] a: subjecting the diamond particles to chemical plating treatment, so that the surface of the diamond particles is evenly coated with a chemical plating layer, wherein the chemical plating layer is a Ni-MP composite layer;

[0015] b: hydrolyzing ferric chloride to prepare a stable Fe2O3 sol, impregnating the diamond particles coated with a chemical plating layer in step a with the Fe2O3 sol, drying and then calcining to uniformly coat the surface of the diamond particles with a layer of Fe2O3 film, thereby obtaining diamond particles with the surface coated with both the Fe2O3 film and the chemical plating layer;

[0016] c: subjecting the diamond particles coated with both Fe2O3 film and chemical plating layer in step b to microwave heating treatment under vacuum of 3Pa, with a microwave heating temperature of 500-800°C, a time of 5-20min, and a microwave power of 600-1000W to obtain diamond particles with metallized surface.

[0017] Preferably, the high-frequency sound waves in S2 have a frequency greater than 20 kHz, a wavelength of 0.01 to 10 cm, and a power density greater than 0.3 w / cm 2 , forming "cavitation bubbles".

[0018] Preferably, the welding in S2 further includes adding a flux, and the flux is one or more combinations of boron, sodium fluoride, potassium chloride, borax, sodium chloride, gluconic acid, oxalic acid, succinic acid, immonium chloride, and zinc chloride.

[0019] The present invention provides a brazing process for a diamond saw blade, which has the following beneficial effects:

[0020] The brazing process of a diamond saw blade, wherein the phosphorus element of the brazing flux can improve the fluidity of the brazing material, thereby facilitating the brazing flux to flow and fill easily after being heated, thereby ensuring that the solder can be evenly distributed in the welding area, thereby reducing the risk of voids and incomplete penetration, and can quickly spread to the entire welding area, which not only simplifies the welding process, making it simpler and faster, but also activates the diamond surface to give the surface metal-like properties, which is more conducive to the combination between the diamond and the metal brazing material, and adopts argon cooling, which has good thermal conductivity and can quickly cool the weld, which helps to quickly cool the welding area, reduce the size of the heat-affected zone, and thus reduce the possibility of deformation. This cooling effect helps to control the welding temperature, reduce the risk of thermal deformation, prevent the weld and molten metal from reacting with oxygen, nitrogen, etc. in the air, thereby avoiding adverse effects such as oxidation and nitridation, and helps to maintain the purity of the welding area and improve the quality and strength of the weld. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a flow chart of the present invention. Figure 2 This is a graph showing the relationship between shear strength and brazing temperature of the present invention. Figure 3 This is a graph showing the relationship between shear strength and pressure of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] A brazing process for a diamond saw blade, S1: cleaning the welding surface; using mechanical and chemical methods to clean the oxide film, grease or other attachments on the diamond particles and the blade groove to be welded; the brazing area after surface cleaning should be kept clean, and when moving diamond particles, the operator should wear gloves, and it is forbidden to touch the metal substrate to be brazed with oily dirt or bare hands, and the metal substrate to be brazed is wiped clean with a clean cloth dipped in anhydrous ethanol or acetone;

[0025] S2: welding assembly; then apply paste flux in the knife groove of the cutter body, place the brazing material and diamond particles in sequence, and apply another layer of flux between the brazing material and the diamond particles. The flux composition is as follows: Ag60%, Cu20%, Ti0.5%, Si5%, P1%, and the remainder is impurities; place it in a high-frequency sound wave environment and select a vacuum furnace for brazing, and use induction heating fuzzy control and synchronous data acquisition system for heating temperature control;

[0026] S3: Brazing in a vacuum furnace; using argon cooling, the purity of argon should be >99.9%; and the principle is to avoid cracks and minimize the internal stress of the brazed joint and the deformation of the metal matrix;

[0027] S4: Inspect the weld; after welding, measure the weld thickness with a stereo microscope, observe the weld microstructure with a JEOL JSM6360LV scanning electron microscope, and then test the shear strength on a shear strength measuring device.

[0028] When brazing in a vacuum furnace is used in S2, the vacuum furnace equipment is out of service for more than 1 month and needs to be dried. The furnace drying process parameters are: evacuate to below 5x103Pa, heat to 1000℃ for 60min-120min, keep warm for 5min after the temperature in the vacuum furnace stabilizes at the set temperature, and cool to room temperature with the furnace. When the thickness of the diamond particle matrix is ​​large, the vacuum brazing furnace is heated to 20℃ below the melting temperature of the brazing material for insulation, and then heated to the brazing temperature for brazing after the temperature is uniform. Figure 3 It can be seen that before the brazing pressure reaches 3.911 MPa, the shear strength gradually increases with the increase of the brazing pressure.

[0029] The chemical cleaning method in S1 is to place the diamond particle matrix in an alkaline aqueous solution of 8wt% NaOH, 5wt% Na2CO3, 5wt% Na2SiO3 and 3wt% Na3PO4, with a cleaning temperature of 50°C and a cleaning time of 10 minutes to remove the oil film on the surface, and then place the diamond particle matrix in an aqueous solution of 3wt% hydrochloric acid and 0.5wt% thiourea for a pickling time of 5 minutes to remove the oxide layer on the surface of the matrix.

[0030] S2 also includes metal activation treatment on the surface of diamond particles before welding, and the method is as follows:

[0031] a: subjecting diamond particles to chemical plating treatment so that the surface of the diamond particles is uniformly coated with a layer of chemical plating, wherein the chemical plating layer is a Ni-MP composite layer; b: hydrolyzing ferric chloride to prepare a stable Fe2O3 sol, impregnating the diamond particles with the chemical plating layer on the surface in step a with the Fe2O3 sol, drying and then calcining so that the surface of the diamond particles is uniformly coated with a layer of Fe2O3 film, thereby obtaining diamond particles with the surface simultaneously coated with the Fe2O3 film and the chemical plating layer; c: subjecting the diamond particles with the Fe2O3 film and the chemical plating layer on the surface in step b to microwave heating treatment under a vacuum degree of 3Pa, wherein the microwave heating treatment temperature is 500°C, the time is 5min, and the microwave power is 600W, thereby obtaining diamond particles with surface metallization.

[0032] The soldering in S2 also includes adding a flux, which is one or more combinations of boron, sodium fluoride, potassium chloride, borax, sodium chloride, gluconic acid, oxalic acid, succinic acid, immonium chloride, and zinc chloride.

[0033] Embodiment 2:

[0034] A brazing process for a diamond saw blade, S1: cleaning the welding surface; using mechanical and chemical methods to clean the oxide film, grease or other attachments on the diamond particles and the blade groove to be welded; the brazing area after surface cleaning should be kept clean, and when moving diamond particles, the operator should wear gloves, and it is forbidden to touch the metal substrate to be brazed with oily dirt or bare hands, and the metal substrate to be brazed is wiped clean with a clean cloth dipped in anhydrous ethanol or acetone;

[0035] S2: welding assembly; then apply paste flux in the knife groove of the cutter body, place the brazing material and diamond particles in sequence, and apply another layer of flux between the brazing material and the diamond particles. The flux composition is as follows: Ag65%, Cu20-25%, Ti1.5%, Si7%, P5%, and the remainder is impurities; place it in a high-frequency sound wave environment and select a vacuum furnace for brazing, and use induction heating fuzzy control and synchronous data acquisition system for heating temperature control;

[0036] S3: Brazing in a vacuum furnace; using argon cooling, the purity of argon should be >99.9%; and the principle is to avoid cracks and minimize the internal stress of the brazed joint and the deformation of the metal matrix;

[0037] S4: Inspect the weld; after welding, measure the weld thickness with a stereo microscope, observe the weld microstructure with a JEOL JSM6360LV scanning electron microscope, and then test the shear strength on a shear strength measuring device.

[0038] When brazing in a vacuum furnace is used in S2, the vacuum furnace equipment is out of service for more than one month and needs to be dried. The furnace drying process parameters are: evacuate to below 5x103Pa, heat to 1200℃ for 120min, keep warm for 10min after the temperature in the vacuum furnace stabilizes at the set temperature, and cool to room temperature with the furnace. When the thickness of the diamond particle matrix is ​​large, the vacuum brazing furnace is heated to 100℃ below the melting temperature of the brazing material for insulation, and then heated to the brazing temperature for brazing after the temperature is uniform. Figure 2 The figure shows the relationship between the brazing temperature and the weld shear strength when the brazing pressure is 7.661MPa. Figure 2It can be seen that with the increase of brazing temperature, the shear strength increases; this is the same as the general brazing law, from which it is known that with the increase of brazing temperature, the wetting angle of the brazing material to the cemented carbide gradually decreases, and the wetting performance is improved; at the same time, the fluidity of the brazing metal is enhanced, and the molten brazing material can fully fill the pits on the surface of the parent material, thereby increasing the effective contact area of ​​the brazing interface; in addition, the higher the welding temperature, the easier it is for the atoms to activate, the greater the diffusion coefficient, the more sufficient the mutual diffusion of atoms between the interfaces, the greater the thickness of the diffusion layer, and the better the bonding strength of the interface. The chemical cleaning method in S1 is to place the diamond particle matrix in an alkaline aqueous solution of 15wt% NaOH, 10wt% Na2CO3, 10wt% Na2SiO3 and 5wt% Na3PO4, the cleaning temperature is 85℃, the time is 20 minutes, remove the oil film on the surface, and then place the diamond particle matrix in a 5wt% hydrochloric acid, 1.2wt% thiourea aqueous solution, the pickling time is 10 minutes, to remove the oxide layer on the surface of the matrix. Before welding, S2 also includes metal activation treatment on the surface of diamond particles, and the method is as follows: a: chemically plate the diamond particles so that the surface is evenly coated with a layer of chemical plating, and the chemical plating layer is a Ni-MP composite layer; b: hydrolyze ferric chloride to prepare a stable Fe2O3 sol, and use the Fe2O3 sol to impregnate the diamond particles with the chemical plating layer on the surface in step a, dry and then roast, so that the surface is evenly coated with a layer of Fe2O3 film, so as to obtain diamond particles with the Fe2O3 film and the chemical plating layer on the surface at the same time; c: perform microwave heating treatment on the diamond particles with the Fe2O3 film and the chemical plating layer on the surface in step b under the condition of a vacuum degree of 3Pa, the microwave heating temperature is 800°C, the time is 20min, and the microwave power is 1000W, so as to obtain diamond particles with metallized surface.

[0039] The soldering in S2 also includes adding a flux, which is one or more combinations of boron, sodium fluoride, potassium chloride, borax, sodium chloride, gluconic acid, oxalic acid, succinic acid, immonium chloride, and zinc chloride.

[0040] Embodiment 3:

[0041] A brazing process for a diamond saw blade, S1: cleaning the welding surface; using mechanical and chemical methods to clean the oxide film, grease or other attachments on the diamond particles and the blade groove to be welded; the brazing area after surface cleaning should be kept clean, and when moving diamond particles, the operator should wear gloves, and it is forbidden to touch the metal substrate to be brazed with oily dirt or bare hands, and the metal substrate to be brazed is wiped clean with a clean cloth dipped in anhydrous ethanol or acetone;

[0042] S2: Welding assembly; then apply paste flux in the knife groove of the cutter body, place the brazing material and diamond particles in sequence, and apply another layer of flux between the brazing material and the diamond particles. The flux composition is as follows: Ag62%, Cu22%, Ti1%, Si6%, P3%, and the remainder is impurities; place it in a high-frequency sound wave environment and select a vacuum furnace for brazing, and use induction heating fuzzy control and synchronous data acquisition system for heating temperature control;

[0043] S3: Brazing in a vacuum furnace; using argon cooling, the purity of argon should be >99.9%; and the principle is to avoid cracks and minimize the internal stress of the brazed joint and the deformation of the metal matrix;

[0044] S4: Inspect the weld; after welding, measure the weld thickness with a stereo microscope, observe the weld microstructure with a JEOL JSM6360LV scanning electron microscope, and then test the shear strength on a shear strength measuring device.

[0045] When brazing in a vacuum furnace is adopted in S2, the vacuum furnace equipment is stopped for more than 1 month, and the furnace needs to be baked. The furnace baking process parameters are: evacuate to below 5x103Pa, heat to 1100℃ for 100min, keep warm for 8min after the temperature in the vacuum furnace stabilizes at the set temperature, cool to room temperature with the furnace, and when the thickness of the diamond particle matrix is ​​large, the vacuum brazing furnace is heated to 50℃ below the melting temperature of the brazing material for insulation, and then heated to the brazing temperature for brazing after the temperature is uniform. The chemical cleaning method in S1 is to place the diamond particle matrix in an alkaline aqueous solution of 12wt% NaOH, 8wt% Na2CO3, 8wt% Na2SiO3 and 4wt% Na3PO4, the cleaning temperature is 60℃, the time is 15 minutes, remove the oil film on the surface, and then place the diamond particle matrix in a 4wt% hydrochloric acid, 0.8wt% thiourea aqueous solution, the pickling time is 8 minutes, to remove the oxide layer on the surface of the matrix.

[0046] S2 also includes metal activation treatment on the surface of diamond particles before welding, and the method is as follows:

[0047] a: subjecting diamond particles to chemical plating treatment so that the surface of the diamond particles is uniformly coated with a chemical plating layer, wherein the chemical plating layer is a Ni-MP composite layer; b: hydrolyzing ferric chloride to prepare a stable Fe2O3 sol, impregnating the diamond particles coated with the chemical plating layer in step a with the Fe2O3 sol, drying and then calcining so that the surface of the diamond particles is uniformly coated with a Fe2O3 film, thereby obtaining diamond particles with the surface simultaneously coated with the Fe2O3 film and the chemical plating layer; c: subjecting the diamond particles with the surface simultaneously coated with the Fe2O3 film and the chemical plating layer in step b to microwave heating treatment under the condition of a vacuum degree of 3Pa, the microwave heating treatment temperature is 600°C, the time is 15min, and the microwave power is 800W, thereby obtaining diamond particles with metallized surface. S2 also includes adding flux during welding, wherein the flux is one or more combinations of boron, sodium fluoride, potassium chloride, borax, sodium chloride, gluconic acid, oxalic acid, succinic acid, immonium chloride, and zinc chloride.

[0048] Comparative Example 1:

[0049] The difference between Comparative Example 1 and Example 1 is that the phosphorus element is not added to the flux;

[0050] Comparative Example 2:

[0051] The difference between Comparative Example 2 and Example 1 is that: Comparative Example 2 adopts air cooling;

[0052]

[0053] As shown in Table 1, the phosphorus element in the brazing flux in this solution can improve the fluidity of the brazing material, thereby facilitating the brazing flux to flow and fill easily after being heated, thereby ensuring that the solder can be evenly distributed in the welding area, thereby reducing the risk of voids and incomplete penetration;

[0054] By using argon cooling, argon has good thermal conductivity and can quickly cool the weld, which helps to quickly cool the welding area and reduce the size of the heat-affected zone, thereby reducing the possibility of deformation. This cooling effect helps to control the welding temperature, reduce the risk of thermal deformation, and prevent the weld and molten metal from reacting with oxygen, nitrogen, etc. in the air, thereby avoiding adverse effects such as oxidation and nitridation, helping to maintain the purity of the welding area and improve the quality and strength of the weld.

[0055] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0056] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A brazing process for a diamond saw blade, characterized in that: The method steps are as follows: S1: Clean the welding surface; use mechanical and chemical methods to clean the oxide film, grease or other attachments on the diamond particles and the groove to be welded; the brazing area should be kept clean after surface cleaning; S2: Welding assembly; then apply paste flux in the knife groove of the cutter body, place the brazing material and diamond particles in sequence, and apply another layer of flux between the brazing material and the diamond particles, place it in a high-frequency sound wave environment, select a vacuum furnace for brazing, and use induction heating fuzzy control and synchronous data acquisition system to control the heating temperature; S3: Brazing in a vacuum furnace; using argon cooling, the purity of argon should be >99.9%; and the principle is to avoid cracks and minimize the internal stress of the brazed joint and the deformation of the metal matrix; S4: Inspect the weld; after welding, measure the weld thickness with a stereo microscope, and then test the shear strength on a shear strength measuring device.

2. A brazing process for a diamond saw blade according to claim 1, characterized in that: When brazing is performed in a vacuum furnace in S2, the vacuum furnace equipment is out of service for more than one month and needs to be baked. The baking furnace process parameters are: evacuating to below 5x103Pa, heating to 1000℃-1200℃ for 60min-120min.

3. A brazing process for a diamond saw blade according to claim 2, characterized in that: After the temperature in the vacuum furnace stabilizes at the set temperature, keep it warm for 5-10 minutes, and cool it to room temperature with the furnace. When the thickness of the diamond particle matrix is ​​large, the vacuum brazing furnace is heated to 20℃-100℃ lower than the melting temperature of the brazing material for insulation, and then heated to the brazing temperature for brazing after the temperature is uniform.

4. A brazing process for a diamond saw blade according to claim 1, characterized in that: The mechanical method in S1 is to perform sandblasting or grinding on the welding point, and the surface roughness of the welding point after grinding is Ra6.

5.

5. The brazing process of a diamond saw blade according to claim 1, characterized in that: The solder composition in the S2 is as follows: Ag 60-65%, Cu 20-25%, Ti 0.5%-1.5%, Si 5%-7%, P 1%-5%.

6. A brazing process for a diamond saw blade according to claim 1, characterized in that: The chemical cleaning method in S1 is to place the diamond particle matrix in an alkaline aqueous solution of 8-15wt% NaOH, 5-10wt% Na2CO3, 5-10wt% Na2SiO3 and 3-5wt% Na3PO4, at a cleaning temperature of 50-85°C for 10-20 minutes to remove the oil film on the surface, and then place the diamond particle matrix in an aqueous solution of 3-5wt% hydrochloric acid and 0.5-1.2wt% thiourea for pickling for 5-10 minutes to remove the oxide layer on the surface of the matrix.

7. A brazing process for a diamond saw blade according to claim 1, characterized in that: The S2 also includes performing metal activation treatment on the surface of the diamond particles before welding, and the method is as follows: a: subjecting the diamond particles to chemical plating treatment, so that the surface of the diamond particles is evenly coated with a chemical plating layer, wherein the chemical plating layer is a Ni-MP composite layer; b: hydrolyzing ferric chloride to prepare a stable Fe2O3 sol, impregnating the diamond particles coated with a chemical plating layer in step a with the Fe2O3 sol, drying and then calcining to uniformly coat the surface of the diamond particles with a layer of Fe2O3 film, thereby obtaining diamond particles with the surface coated with both the Fe2O3 film and the chemical plating layer; c: subjecting the diamond particles coated with both Fe2O3 film and chemical plating layer in step b to microwave heating treatment under vacuum condition of 3Pa, with microwave heating treatment temperature of 500-800℃, time of 5-20min, microwave power of 600-1000W, to obtain surface diamond particles.

8. The brazing process of a diamond saw blade according to claim 1, characterized in that: The high-frequency sound waves in S2 have a frequency greater than 20kHz, a wavelength of 0.01 to 10cm, and a power density greater than 0.3w / cm 2 .

9. A brazing process for a diamond saw blade according to claim 1, characterized in that: The welding in S2 also includes adding a flux, and the flux is one or more combinations of boron, sodium fluoride, potassium chloride, borax, sodium chloride, gluconic acid, oxalic acid, succinic acid, immonium chloride, and zinc chloride.

Citation Information

Patent Citations

  • Glass and metal vacuum brazing technique

    CN101708964A

  • A method for metallizing diamond surfaces

    CN102286742A

  • Brazing process of diamond saw blade

    CN102319934A

  • Copper / aluminum ultrasonic liquid-phase diffusion brazing process and brazing device

    CN102513635A

  • Self-fluxing silver solder containing neodymium, zirconium and gallium

    CN102513727A