Method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components through CMT electric arc swing pair
By using CMT arc swing technology in aluminum alloy additive manufacturing, the oxide film is removed, the problems of reduced performance and unstable connections of dissimilar alloys are solved, and the performance and stability of aluminum alloy components are improved.
Patent Information
- Application Number
- CN202410870069.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-01
AI Technical Summary
During the additive manufacturing process of aluminum alloys, the formation of oxide films leads to excessive wettability and fluidity, resulting in reduced performance of dissimilar alloys and unstable connections.
CMT arc swing technology is used to break the oxide film and improve the flexibility of the dissimilar alloy additive manufacturing process and the stability of the connection layer by setting arc swing parameters such as amplitude and frequency during the welding process.
It effectively removes the oxide film, improves the performance of the bonding layer of dissimilar alloys and the stability of the connecting layer, and enhances the overall performance of aluminum alloy components.
Smart Images

Figure CN118720330A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy utilization, and in particular to a method for additively manufacturing 2319 and 5356 dissimilar aluminum alloy components using CMT arc swing. Background Art
[0002] Aluminum alloys, due to their excellent specific strength, toughness, fatigue resistance and corrosion resistance, occupy a pivotal position in the aerospace, railway transportation and automobile manufacturing industries. However, traditional aluminum alloy processing methods have problems such as long cycle, large material waste and insufficient reliability of weld connections. These problems are particularly prominent in today's pursuit of efficient, high-precision and high-performance integrated manufacturing. 2319 aluminum alloy, as a member of the 2 series aluminum alloy, belongs to the category of hard aluminum alloys. It has excellent strength and hardness. At the same time, it also has the characteristics of heat treatment. Therefore, it is a popular material in the field of aerospace industry. Compared with other series of aluminum alloys, 5356 aluminum alloy has excellent fatigue performance and is a rust-proof aluminum alloy with good corrosion resistance. It is also more widely used in actual production.
[0003] At present, in the existing technology, an oxide film is produced during the additive manufacturing process of aluminum alloys. The oxide film will cause excessive deposition of alloy components during the additive manufacturing process, resulting in excessive wettability and fluidity, which in turn leads to reduced performance of dissimilar alloys and unstable connections.
[0004] Therefore, the prior art still needs to be improved and enhanced. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for additively manufacturing 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing, aiming to solve the problem in the prior art that an oxide film will be generated during the additive manufacturing process of aluminum alloys. The oxide film will cause excessive deposition of alloy components during the additive manufacturing process, resulting in excessive wettability and fluidity, thereby reducing the performance of the dissimilar alloys and unstable connections.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, a method for additively manufacturing 2319 and 5356 dissimilar aluminum alloy components by CMT arc swinging includes:
[0008] Step 1. Select the base material: Select 2024-T4 plate as the base material and perform pretreatment.
[0009] Step 2, parameter setting: set aluminum alloy processing parameters for related processing equipment, set aluminum alloy welding procedures and welding parameter ranges: 2319 aluminum alloy welding speed range is 30-60cm / min, wire feeding speed is 4-6m / min; 5356 aluminum alloy welding speed is 30-60cm / min, wire feeding speed is 4-6m / min, inert gas is used as shielding gas, 99.99% high-purity argon is selected, gas flow is 25L / min, and welding path is set;
[0010] Step 3, welding forming: first, 15 layers of 5356 aluminum alloy are welded on the base material 2024-T4 plate according to the welding path, and CMT arc swing is added during the welding process. After completion, 20 layers of 2319 aluminum alloy are continued to be welded thereon according to the welding path, and CMT arc swing is added during the welding process to obtain dissimilar aluminum alloy components.
[0011] Furthermore, in step 2, the welding path is set to be a single-pass multi-layer deployment of the welding robot, and the welding path is reciprocating.
[0012] Furthermore, in step 3:
[0013] The welding speed of 5356 aluminum alloy is set to 30-60cm / min, the wire feeding speed is 4-6m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min. Each time a layer is welded, the interlayer cooling time is stopped for 30s, and the forming morphology of the aluminum alloy is observed. After 30s, the next layer is welded until 15 layers of 5356 aluminum alloy are welded.
[0014] Furthermore, in step 3:
[0015] Continue to add 2319 aluminum alloy CMT arc additive manufacturing on the completed 5356 aluminum alloy component. The welding speed of 2319 aluminum alloy is 30-60cm / min, the wire feeding speed is 4-6m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min until the welding of 20 layers is completed.
[0016] Furthermore, in step 3:
[0017] Arc swing is added during the welding process, and the swing parameter range is: swing amplitude 5-7mm, frequency 3-5Hz, and the swing pattern is a Z-shaped symmetrical swing.
[0018] Furthermore, the dissimilar aluminum alloy components are 2319 and 5356 dissimilar aluminum alloy components. The 2319 and 5356 dissimilar aluminum alloy components are subjected to post-manufacturing performance tests. The performance tests show that the metallurgical bonding layer has two obvious aluminum alloy precipitation phases. A large amount of white reticular eutectic structure is distributed on the 2319 side, and there is an α-Al+θ phase, that is, Al 2 Cu phase, and some fine second phases are distributed in the crystal; the sample area on one side of 5356 is composed of α-Al matrix and β, i.e. Al 3 Mg 2 Phase composition.
[0019] The technical solution adopted by the present invention has the following beneficial effects:
[0020] In this application, CMT arc oscillation is first used to additively manufacture 5356 aluminum alloy components, and then 2319 aluminum alloy is further additively manufactured on the 5356 aluminum alloy components. The arc oscillation parameters are: amplitude of 6 mm, frequency of 4 Hz, and Z-shaped symmetrical oscillation. The additive parameters of 5356 aluminum alloy are: wire feeding speed of 4-6 m / min, welding speed of 30-60 cm / min, and interlayer cooling rate of 30s; the additive parameters of 2319 aluminum alloy are: wire feeding speed of 4-6 m / min, welding speed of 30-60 cm / min, and interlayer cooling rate of 30s. By adding a Z-shaped symmetrical oscillating oscillating arc in the process of additive manufacturing of dissimilar alloys, the oxide film generated in the manufacturing process can be broken, the flexibility of the additive manufacturing process of dissimilar alloys can be improved, the bonding layer performance of the component can be improved, and the stability of the connecting layer can be enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the additive manufacturing process designed for the present invention;
[0022] Figure 2 The macroscopic morphology of the heterogeneous aluminum alloy components;
[0023] Figure 3 Metallographic and tensile specimen location and specification diagrams for dissimilar aluminum alloy components;
[0024] Figure 4 The microstructure diagram of the heterogeneous aluminum alloy components;
[0025] Figure 5 This is the pore distribution diagram of heterogeneous aluminum alloy components;
[0026] Figure 6 It is the grain size distribution diagram of heterogeneous aluminum alloy components;
[0027] Figure 7 is the average Vickers hardness distribution curve of heterogeneous aluminum alloy components;
[0028] Figure 8 This is a scanning electron microscope image of a dissimilar aluminum alloy component. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] It should be noted that when a component is referred to as being "fixed to" or "disposed on" another component, it can be directly on the other component or indirectly on the other component. When a component is referred to as being "connected to" another component, it can be directly connected to the other component or indirectly connected to the other component.
[0031] It should also be noted that the same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right" and the like indicate directions or positional relationships based on the directions or positional relationships shown in the drawings, it is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and cannot be understood as limitations on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0033] Porosity is the most common and almost unavoidable defect in additively manufactured aluminum alloys, and has become the main factor restricting its application. Therefore, it is very important to evaluate the porosity of the formed components. Therefore, the porosity analysis of the two aluminum alloy components was carried out.
[0034] First, in this embodiment, refer to Figure 1 , a CMT arc swing method for additively manufacturing 2319 and 5356 dissimilar aluminum alloy components, comprising:
[0035] Step 1. Select the base material: Select 2024-T4 plate as the base material, because the oxide film, pollutants and moisture on the surface layer of the aluminum alloy will affect the welding effect, resulting in internal defects such as inclusions and pores, thereby affecting the material's organizational properties. In view of this, the substrate must be pretreated before the additive manufacturing test. The specific steps are: use an angle grinder to grind the area to be deposited on the substrate, remove the oxide film and impurities attached to the surface, place the treated substrate in a sodium hydroxide solution for 5 minutes, rinse with clean water and wipe thoroughly with acetone to ensure that there is no residual dirt. Finally, dry it for use.
[0036] The base material is 2024-T4 aluminum alloy, and the welding wire is 2319 and 5356. The chemical composition of the welding wire and the substrate is shown in Table 1:
[0037] Table 1 Chemical composition of welding wire and substrate (mass fraction, %)
[0038]
[0039] Step 2, parameter setting: set aluminum alloy processing parameters for related processing equipment, set aluminum alloy welding program, welding parameters, 2319 aluminum alloy welding speed is 50m / min, wire feeding speed is 4m / min; 5356 aluminum alloy welding speed is 30m / min, wire feeding speed is 4.5m / min, shielding gas is inert gas, the present invention selects 99.99% high-purity argon gas, gas flow rate is 25L / min, and set welding path, wherein the welding path is set to single-pass multi-layer expansion of the welding robot, and the welding path is reciprocating.
[0040] The welding mode during the test was manual + automatic mode. The automatic mode was programmed in the KIDE software using the AS language. In the manual mode, it is necessary to establish a welding database in advance, set the job program to be used for each layer in the teach pendant, set the arc crater filling time, extract the arc swing trajectory, and the most important Z-axis offset. The Z-axis offset was set based on preliminary experiments and experience: for the first 15 layers, the welding gun is raised 1.6mm along the Z-axis for each layer, and for the last 20 layers, the welding gun is raised 1.2mm along the Z-axis for each layer.
[0041] Step 3, welding forming: first, 15 layers of 5356 aluminum alloy are welded on the base material 2024-T4 plate according to the welding path, and CMT arc swing is added during the welding process. After completion, 20 layers of 2319 aluminum alloy are continued to be welded thereon according to the welding path, and CMT arc swing is added during the welding process to obtain dissimilar aluminum alloy components.
[0042] Among them, arc swing is added during the welding process, and the swing parameters are: swing amplitude 6mm, frequency 4Hz, swing pattern is Z-shaped symmetrical swing, and the additive manufacturing parameters are as follows: wire feeding speed range is 4-6m / min, welding speed range is 30-60cm / min, welding current range is 60-90A, and welding voltage range is 5-20V. The preferred process parameters of 2319 aluminum alloy are wire feeding speed of 4m / min and welding speed of 50cm / min. The gas flow rate is 25L / min; the process parameters of 5356 aluminum alloy are wire feeding speed of 4.5m / min and welding speed of 30cm / min. The gas flow rate is 25L / min.
[0043] In addition, in step 3, the welding speed of 5356 aluminum alloy is set to 30m / min, the wire feeding speed is 4.5m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min. Each time a welding is completed, the interlayer cooling time is stopped for 30s, the aluminum alloy forming morphology is observed, and the next layer is welded after 30s until 15 layers of 5356 aluminum alloy are welded.
[0044] In this embodiment, in step 3, CMT arc additive manufacturing of 2319 aluminum alloy is continued on the completed 5356 aluminum alloy component. The welding speed of 2319 aluminum alloy is 50m / min, the wire feeding speed is 4m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min, until the welding of 20 layers is completed.
[0045] After the dissimilar aluminum alloy components were manufactured, the post-manufacturing performance tests were carried out on the 2319 and 5356 dissimilar aluminum alloy components. The performance tests showed that the metallurgical bonding layer had two obvious aluminum alloy precipitation phases. A large amount of white eutectic structure was distributed on the 2319 side, and there was α-Al+θ(Al 2 Cu) phase, and there are also some fine second phases distributed in the crystal; the sample area on one side of 5356 is composed of α-Al matrix and β (Al 3 Mg 2 ) phase.
[0046] The technical solution of the present invention is further described below in conjunction with specific implementation:
[0047] The metal arc additive manufacturing experimental substrate used in the present invention is a 2024-T4 aluminum alloy plate with a substrate size of 250mm×50mm×4mm. The welding wires are 2319 welding wires with a diameter of 1.2mm and 1.6mm5356 welding wires. CMT cold metal transition welding is used for additive manufacturing. Aluminum alloy arc additive manufacturing experiments are carried out using aluminum alloy procedures and cold metal transition technology. The additive manufacturing system built for the experiment is a complete cold metal transition welding system consisting of a Fronius CMT TPS 4000 welding machine and a Kawasaki BA 006N six-axis welding robot.
[0048] The main implementation steps are as follows:
[0049] 1. Before the formal test, the aluminum alloy welding procedure and welding parameters were set. The welding speed of 2319 aluminum alloy was 50m / min, and the wire feeding speed was 4m / min; the welding speed of 5356 aluminum alloy was 30m / min, and the wire feeding speed was 4.5m / min. The shielding gas was 99.99% high-purity argon gas, and the gas flow rate was 25L / min.
[0050] 2. Figure 1 A schematic diagram of the additive manufacturing process designed for the present invention is shown in FIG. Figure 1 As shown, arc swing is added in the additive process, the swing trajectory is a Z-shaped symmetrical swing, the swing amplitude is 6mm, and the swing frequency is 4Hz. The welding robot is set to single-pass multi-layer expansion, and the welding path is reciprocating. The welding speed of 5356 aluminum alloy is set to 30m / min, the wire feeding speed is 4.5m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min. Each time a welding is completed, the interlayer cooling time is stopped for 30s, and the aluminum alloy forming morphology is observed. After 30s, the next layer is welded until 15 layers of 5356 aluminum alloy are welded.
[0051] 3. Continue to add 2319 aluminum alloy CMT arc additive manufacturing on the above-mentioned 5356 aluminum alloy components. The welding speed of 2319 aluminum alloy is 50m / min, the wire feeding speed is 4m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25L / min until the welding of 20 layers is completed.
[0052] 4. Continue to additively manufacture a dissimilar aluminum alloy metal component without adding arc swing using the same process parameters as above, and compare the macromorphology, microstructure and mechanical properties of the two metal components.
[0053] 5. Observe the macroscopic morphology of heterogeneous components, such as Figure 2As shown, it can be found that the two aluminum alloys can be well combined and have an obvious metallurgical bonding layer. It can be seen that there is a slight collapse phenomenon at both ends of the two components, showing a layered feature. No crack collapse is found in the metallurgical bonding layer of the two aluminum alloys, indicating that the two aluminum alloys have good metallurgical bonding. The metallurgical bonding layer and surface of the component with arc swing are better in flatness and better in forming than those without arc swing.
[0054] 6. Install the above components according to Figure 3 The metallographic samples were polished with 1000#, 1500#, and 2000# sandpapers, and then mechanically polished with gold velvet polishing cloth and diamond polishing pastes of W 2.5 and W 0.5, respectively. Keller reagent (HF:HCl:HNO 3 :H 2 O=2:3:5:190) was used to corrode 2319 aluminum alloy for 20s and 5356 aluminum alloy for 30s. After washing with deionized water and drying with compressed air, macroscopic and microscopic observations were performed.
[0055] 7. Install the above components according to Figure 3 The position size was sampled by wire cutting, and the two components were subjected to room temperature tensile tests. The tensile strength of the component with arc swing was 111.7MPa; the tensile strength of the component without arc swing was 205MPa.
[0056] 8. Image Pro Plus 6.0 software was used to perform porosity parameter statistics on the two samples.
[0057] 9. The Vickers hardness of the metallurgical bonding layer of the above sample was measured. The results are as follows: Figure 7 shown.
[0058] Comparative Example 1:
[0059] The alloy composition of the heterogeneous aluminum alloy deposition part is: 2319: Cu: 6.03wt.%; Mn: 0.38wt.%; Mg: <0.02wt.%; Si: <0.2wt.%; Zn: <0.1wt.%; Fe: 0.163wt.%; Al balance. 5356: Cu: 0.08wt.%; Mn: 0.12wt.%; Mg: 4.8wt.%; Si: 0.2wt.%; Zn: 0.08wt.%; Fe: 0.4wt.%; Al balance.
[0060] Manufacturing method: The aluminum alloy process in the cold metal transition technology is used to perform aluminum alloy arc additive manufacturing. The welding speed of 2319 aluminum alloy is 50m / min, and the wire feeding speed is 4m / min; the welding speed of 5356 aluminum alloy is 30m / min, and the wire feeding speed is 4.5m / min. The shielding gas is 99.99% high-purity argon gas, and the gas flow rate is 25L / min. No arc swing is added for additive manufacturing.
[0061] Sedimentary structure: The metallographic structure observed is as follows Figure 4 (b), it can be observed that 2319 and 5356 have obvious metallographic boundaries. The dotted line in the figure is the metallurgical bonding layer of the two aluminum alloys, the upper part is 5356 aluminum alloy, and the lower part is 2319 aluminum alloy.
[0062] Example:
[0063] The alloy composition of the heterogeneous aluminum alloy deposition part is: 2319: Cu: 6.03wt.%; Mn: 0.38wt.%; Mg: <0.02wt.%; Si: <0.2wt.%; Zn: <0.1wt.%; Fe: 0.163wt.%; Al balance. 5356: Cu: 0.08wt.%; Mn: 0.12wt.%; Mg: 4.8wt.%; Si: 0.2wt.%; Zn: 0.08wt.%; Fe: 0.4wt.%; Al balance.
[0064] Manufacturing method: The aluminum alloy process in the cold metal transition technology is used to perform aluminum alloy arc additive manufacturing. The welding speed of 2319 aluminum alloy is 50m / min, and the wire feeding speed is 4m / min; the welding speed of 5356 aluminum alloy is 30m / min, and the wire feeding speed is 4.5m / min. The shielding gas is 99.99% high-purity argon gas, and the gas flow rate is 25L / min. Arc swing is added for additive manufacturing.
[0065] Sedimentary structure: The metallographic structure observed is as follows Figure 4 (a), it can be observed that 2319 and 5356 have obvious metallographic boundaries. Compared with the components without arc swing, the components with arc swing are more obvious and the grain boundary precipitation is more obvious. Porosity is the most common and almost unavoidable defect in aluminum alloys manufactured by additive manufacturing, and has become the main factor restricting its application. Therefore, it is crucial to evaluate the porosity of formed components. The vast majority of pore defects in aluminum alloys manufactured by arc additive manufacturing are hydrogen pores. The source of hydrogen is partly the oxidation of the substrate and welding wire stored in non-dry air; the other part is the hydrous aluminum oxide film that is easily formed on aluminum alloy materials in the air. During the formation process, pores mainly go through the stages of nucleation, growth, and escape. Image Pro Plus 6.0 software was used to calculate the porosity parameters. The substrate substrate needed to be removed before statistics. The pore distribution map was obtained through threshold segmentation optimization, as shown below: Figure 5 The white area in the middle is the identified pores. And the porosity formula is used to calculate: (4.2) Where: P is the porosity; A i is the total area of pores in the sample metallographic image; A M is the total area of the sampled metallographic image. According to the above statistical method, three areas of the samples were taken from the metallurgical joints of the two components, and the average number of pores, average pore size and average porosity were statistically analyzed, and the data were shown in Table 2.
[0066] Porosity is the most common and almost unavoidable defect in aluminum alloys manufactured by additive manufacturing, and has become the main factor restricting its application. Therefore, it is crucial to evaluate the porosity of formed components. The vast majority of pore defects in aluminum alloys manufactured by arc additive manufacturing are hydrogen pores. The source of hydrogen is partly the oxidation of the substrate and welding wire stored in non-dry air; the other part is the hydrous aluminum oxide film that is easily formed on aluminum alloy materials in the air. During the formation process, pores mainly go through the stages of nucleation, growth, and escape. Image Pro Plus 6.0 software was used to calculate the porosity parameters. The substrate substrate needed to be removed before statistics. The pore distribution map was obtained through threshold segmentation optimization, as shown below: Figure 5 The white area in the middle is the identified pores. And the porosity formula is used to calculate:
[0067]
[0068] Where: P is the porosity; ∑A i A is the total area of pores in the sample metallographic image; M is the total area of the sampled metallographic image. According to the above statistical method, three areas of the samples were taken from the metallurgical joints of the two components, and the average number of pores, average pore size and average porosity were statistically analyzed, and the data were shown in Table 2.
[0069] Table 2 shows the pore statistics of two aluminum alloy components.
[0070]
[0071] The pore distribution diagram and statistical data show that the pores in the components without arc additive are larger and the porosity is higher. This is because in the additive manufacturing process, the uneven distribution of epitaxially grown columnar crystals, inclusions and solutes can serve as non-uniform nucleation points for pores. Therefore, the organizational structure of columnar crystals is conducive to the formation of pores. In addition, in the CMT mode, since the molten pool is relatively deep and narrow, the pores are not easy to escape. The smaller pores float up and combine with each other to form large pores and stay on the surface of the molten pool. The sample with arc swing has a more complicated flow of the molten pool due to the addition of Z-shaped symmetrical arc swing. Under the action of arc force and droplet impact force, the liquid metal flows along the left and right edges to the bottom of the molten pool, and the liquid metal at the bottom of the molten pool flows to the left and right sides and the upper part, thereby generating a large vortex in the cross section of the molten pool, which helps the pores to float up, break through the constraints of the coarse columnar crystals, and escape from the surface of the molten pool. Therefore, the radius of the pores inside the sample is small, and the layered porosity is also at a low level.
[0072] See Figure 6 , is the grain size distribution diagram of the two component styles. It can be seen that the internal crystal structure of the additive component shows the characteristics of different orientations and random distribution. The grain size distribution of the formed sample in the CMT mode is not uniform, and the structural characteristics of the equiaxed crystal are more obvious. After adding arc swing, the distribution of equiaxed crystals is more uniform, the proportion of equiaxed crystals increases, and the size is relatively large. The average size of the metallographic structure of the sample with arc swing is 6.67μm, and the average size of the metallographic structure of the sample without arc swing is 49.66μm. This is because under the action of arc swing, the arc residence time per unit weld length becomes longer, and the amount of melted welding wire is more. Although the heat input has increased, under the action of swinging along the Y direction, the effective width becomes larger, and the heat action range on the lower metal becomes smaller, so the driving force for the recrystallization of the lower layer is reduced, and no obvious grain growth occurs.
[0073] The Vickers hardness of the above comparative example 1 and embodiment 1 was measured. The measurement results are shown in Figure 7 The change along the X-axis direction is small, and the average hardness value of the arc swing sample is 81.57HV 0.2 The average hardness of the sample without arc swing is 80.36HV 0.2 In the Z-axis direction, it shows an increasing trend, and the average hardness value of the sample with arc swing is 82.02HV 0.2 The average hardness of the sample without arc swing is 79.87HV 0.2 In both directions, the average hardness of the samples with arc swing is slightly greater than that of the samples without arc swing. In the Z-axis direction, the maximum hardness appears in the upper middle part, while in the lower 5 series aluminum alloy, the samples without arc swing are better than those with arc swing.
[0074] Figure 8 The microstructures of the two samples were examined by scanning electron microscope. It can be seen that the metallurgical bonding layer has two obvious aluminum alloy precipitation phases. A large amount of white eutectic structure is distributed on the 2319 side, and there is α-Al+θ(Al 2 Cu) phase, and some small second phases are irregularly distributed in the crystal. The sample area on one side of 5356 is composed of α-Al matrix and β (Al 3 Mg 2 ) phase, without other impurity phases. It can be seen that black particles are dispersed on the gray matrix. And the precipitation phases of the two aluminum alloys in the arc swing sample grow more obviously towards the opposite side.
[0075] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the schemes disclosed herein. The present invention is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed in this disclosure. The description and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the claims.
Claims
1. A method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components using CMT arc swing. It is characterized in that include: Step 1. Select the base material: Select 2024-T4 plate as the base material and perform pretreatment; Step 2, parameter setting: set aluminum alloy processing parameters for related processing equipment, set aluminum alloy welding procedures and welding parameter ranges: 2319 aluminum alloy welding speed range is 30-60cm / min, wire feeding speed is 4-6 m / min; 5356 aluminum alloy welding speed is 30-60cm / min, wire feeding speed is 4-6m / min, inert gas is used as shielding gas, 99.99% high-purity argon is selected, gas flow is 25 L / min, and welding path is set; Step 3, welding forming: First, 15 layers of 5356 aluminum alloy are welded on the base material 2024-T4 plate according to the welding path, and CMT arc swing is added during the welding process. After completion, 20 layers of 2319 aluminum alloy are continued to be welded on it according to the welding path, and CMT arc swing is added during the welding process to obtain dissimilar aluminum alloy components.
2. The method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing according to claim 1, It is characterized in that In step 2, the welding path is set to be a single-pass multi-layer deployment of the welding robot, and the welding path is reciprocating.
3. The method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing according to claim 1, It is characterized in that In step 3: The welding speed of 5356 aluminum alloy was set to 30-60 cm / min, the wire feeding speed was 4-6 m / min, the shielding gas was 99.99% high-purity argon, and the gas flow rate was 25 L / min. Each time a layer was welded, the interlayer cooling time was stopped for 30 s, and the forming morphology of the aluminum alloy was observed. After 30 s, the next layer was welded until 15 layers of 5356 aluminum alloy were welded.
4. The method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing according to claim 2, It is characterized in that In step 3: Continue to add 2319 aluminum alloy CMT arc additive manufacturing on the completed 5356 aluminum alloy component. The welding speed of 2319 aluminum alloy is 30-60cm / min, the wire feeding speed is 4-6 m / min, the shielding gas is 99.99% high-purity argon, and the gas flow rate is 25 L / min until the welding of 20 layers is completed.
5. The method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing according to claim 2, It is characterized in that In step 3: Arc swing is added during the welding process, and the swing parameter range is: swing amplitude 5-7 mm, frequency 3-5 Hz, and the swing pattern is a Z-shaped symmetrical swing.
6. The method for additive manufacturing of 2319 and 5356 dissimilar aluminum alloy components by CMT arc swing according to claim 1, It is characterized in that The dissimilar aluminum alloy components are 2319 and 5356 dissimilar aluminum alloy components. The 2319 and 5356 dissimilar aluminum alloy components are subjected to post-manufacturing performance tests. The performance tests show that the metallurgical bonding layer has two obvious aluminum alloy precipitation phases. A large amount of white reticular eutectic structure is distributed on the 2319 side, and there is an α-Al + θ phase, that is, Al 2 Cu phase, and some fine second phases are distributed in the crystal; the sample area on one side of 5356 is composed of α-Al matrix and β, i.e. Al 3 Mg 2 Phase composition.