Welding method and application of stainless steel pipeline

Through the gapless assembly and argon gas shielded bottom welding method, combined with the cover welding of manual arc welding, the welding deformation and forming quality problems of stainless steel pipelines are solved, and efficient and defect-free welding results are achieved.

CN118720342APending Publication Date: 2024-10-01SHENYANG TURBO MASCH CORP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410574790.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing stainless steel pipeline welding technology, the backside forming quality is greatly affected by the technical level of the welder, and the large thermal expansion coefficient of stainless steel causes serious welding deformation, affecting product dimensional accuracy and assembly quality.

Method used

The backing welding method without gap pairing is adopted, and the welding current intensity and rotation speed are controlled by internal argon gas protection to make the molten pool sink to the back of the weld to achieve the formation of the back weld, and manual arc welding is used during cover welding. to improve weld quality.

Benefits of technology

Reduce welding deformation, uniform weld formation, high internal quality, radiographic flaw detection can reach 100% first-level defect-free, improve welding efficiency, and increase work efficiency by more than 3 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720342A_ABST
    Figure CN118720342A_ABST
Patent Text Reader

Abstract

The invention discloses a stainless steel pipeline welding method and application thereof. The welding method comprises the steps of backing welding of the stainless steel pipeline and cosmetic welding of the stainless steel pipeline. Wherein backing welding of the stainless steel pipelines comprises the steps that the stainless steel pipelines are subjected to gapless assembly; the assembled stainless steel pipelines are subjected to positioned welding; argon is filled into the stainless steel pipeline subjected to positioned welding for protection, manual argon tungsten-arc welding is adopted for backing welding on the front face of the stainless steel pipeline subjected to positioned welding, the welding current intensity and the rotating speed of the stainless steel pipeline are controlled, a molten pool sinks to the back face of a welding seam, and then the welding seam on the back face of the stainless steel pipeline is formed. The welding method of the stainless steel pipeline is used for welding the stainless steel pipeline of the compressor. The welding method of the stainless steel pipeline has the advantages of being small in welding deformation, good in welding seam forming, high in welding seam internal quality and high in welding efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular to a welding method and application of a stainless steel pipeline. Background Art

[0002] The centrifugal compressor pipelines are all made of 304 or 316 stainless steel. In the traditional welding process, when the pipelines are assembled after processing the groove, a gap of 2 to 3 mm is required, and then the positioning welding is fixed. During welding, the back is filled with argon gas for protection, and the front is welded by manual tungsten inert gas arc welding. The welding method of molten hole breakdown is adopted at the root of the groove to achieve the purpose of single-sided welding and double-sided forming. This operation method is a common welding method specified by the welding process. However, in the prior art, the forming quality of the back of the pipeline is greatly affected by the technical level of the welder, and because the thermal expansion coefficient of stainless steel is large, the gap welding of the pipeline assembly will cause a large welding deformation, which affects the product dimensional accuracy and assembly quality. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a welding method for a stainless steel pipeline, aiming to form a high-quality weld through simple operation and reduce welding deformation.

[0004] To this end, a first aspect of the present invention provides a welding method for a stainless steel pipeline, including a bottom welding of a stainless steel pipeline and a cover welding of a stainless steel pipeline; wherein the bottom welding of the stainless steel pipeline includes:

[0005] Assemble stainless steel pipes without gaps;

[0006] Perform positioning welding on the assembled stainless steel pipes;

[0007] The interior of the stainless steel pipeline after positioning welding is filled with argon gas for protection, and manual tungsten inert gas welding is used to perform base welding on the front of the stainless steel pipeline after positioning welding. The welding current intensity and the rotation speed of the stainless steel pipeline are controlled to make the molten pool sink to the back of the weld, thereby achieving the formation of the weld on the back of the stainless steel pipeline.

[0008] Furthermore, the gap between the gapless pairs is 0 to 0.5 mm.

[0009] Furthermore, the method for protecting the interior of the stainless steel pipeline after positioning welding by filling argon gas is as follows:

[0010] The flow rate of argon gas continuously filled in the stainless steel pipeline is selected according to the diameter and length of the stainless steel pipeline, specifically,

[0011] The diameter of the stainless steel pipeline is ≤89mm, the length of the stainless steel pipeline is ≤6m, the flow rate of argon gas filled inside the stainless steel pipeline is 5-10L / min, and the stainless steel pipeline can be welded after the argon gas is filled inside for 5-10 minutes;

[0012] The diameter of the stainless steel pipeline is greater than 89mm, the length of the stainless steel pipeline is greater than 6m, the flow rate of argon gas filled inside the stainless steel pipeline is 10-15L / min, and welding can be carried out only after the stainless steel pipeline is filled with argon gas for 5-10 minutes.

[0013] Furthermore, the control method of the welding current intensity is: during welding, the welding current intensity is selected according to the thickness and diameter of the stainless steel pipe, specifically:

[0014] When the thickness of stainless steel pipe is ≤3.5mm and the diameter of stainless steel pipe is ≤5mm, and the welding current intensity is 110~135A;

[0015] When the thickness of the stainless steel pipe is 5mm<10mm, and the diameter of the stainless steel pipe is 60mm<114mm, the welding current intensity is 130~165A.

[0016] Furthermore, the control method of the welding current intensity is: the calculation formula of the welding current intensity value is: 1 / 2(D+H)+100; wherein D is the diameter of the stainless steel pipe, H is the thickness of the stainless steel pipe, and 100 is the coefficient.

[0017] Furthermore, the method for controlling the rotation speed of the stainless steel pipeline is as follows: preheat the manual tungsten inert gas arc welding after the arc is started, start rotating after the molten pool sinks, control the rotation speed of the stainless steel pipeline so that the molten pool sinks to the back of the weld, and adjust the rotation speed according to the molten pool temperature. If the molten pool temperature is high, the rotation speed of the stainless steel pipeline needs to be accelerated, and if the molten pool temperature is low, the rotation speed of the stainless steel pipeline needs to be slowed down.

[0018] Furthermore, the method for controlling the rotation speed of the stainless steel pipeline also includes: when the gap between the stainless steel pipeline pairs meets the requirement of 0 to 0.5 mm, the molten pool position is maintained between 12 o'clock and 2 o'clock, and clockwise rotation uphill welding is adopted; when the gap between the stainless steel pipeline pairs is greater than 0.5 mm, the welding molten pool position of the gap greater than 0.5 mm is maintained between 12 o'clock and 11 o'clock, and counterclockwise rotation downhill welding is adopted.

[0019] Furthermore, it also includes: when the thickness of the stainless steel pipeline is ≥2mm, the stainless steel pipeline is beveled before welding, the bevel angle is 60±2 degrees, the single-side bevel angle is 30±1 degrees, and the blunt edge is 0-0.5mm.

[0020] Furthermore, the cap welding method is manual arc welding, the current intensity of the manual arc welding is 65-80A, and the diameter of the welding rod is 3.2mm.

[0021] A second aspect of the present invention provides an application of a stainless steel pipeline welding method, wherein the stainless steel pipeline welding method is used for welding stainless steel pipelines of compressors.

[0022] Beneficial Effects

[0023] The welding method of the stainless steel pipeline provided by the present invention has the following advantages by performing gapless group bottom welding on the stainless steel pipeline: 1) reducing the shrinkage of the pipeline welding and reducing the deformation of the welding; 2) the weld is well formed, the back of the weld is formed evenly, the excess height is generally 0.5-1.5mm, and the excess height difference is small, which is very beautiful; 3) the internal quality of the weld is high, and the weld can be 100% defect-free in the first level by radiographic inspection; 4) the welding efficiency is improved, and the horizontal rotation welding is adopted, which is more than 3 times more efficient than the full-position welding method. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of a stainless steel pipeline assembly according to a method for welding a stainless steel pipeline provided in an embodiment of the present application.

[0025] Figure 2 A welding position clock diagram of a welding method for a stainless steel pipeline provided in an embodiment of the present application. DETAILED DESCRIPTION

[0026] In order to better understand the above technical solution, the technical solution of the present invention is described in detail below through specific embodiments.

[0027] A first aspect of an embodiment of the present invention provides a welding method for a stainless steel pipeline, including base welding of a stainless steel pipeline and cover welding of a stainless steel pipeline; wherein the base welding of the stainless steel pipeline includes:

[0028] Assemble stainless steel pipes without gaps;

[0029] Perform positioning welding on the assembled stainless steel pipes;

[0030] The interior of the stainless steel pipeline after positioning welding is filled with argon gas for protection, and manual tungsten inert gas welding is used to perform base welding on the front of the stainless steel pipeline after positioning welding. The welding current intensity and the rotation speed of the stainless steel pipeline are controlled to make the molten pool sink to the back of the weld, thereby achieving the formation of the weld on the back of the stainless steel pipeline.

[0031] The welding method of stainless steel pipeline provided by the embodiment of the present invention, wherein the backing welding of stainless steel pipeline is to perform gapless grouping of stainless steel pipeline, and the temperature of the molten pool and the slow thermal conductivity of stainless steel are used to make the molten pool produce a collapsed state, so that the molten pool sinks to the back of the weld, thereby realizing the backing welding method of single-sided welding and double-sided forming. The advantages of the backing welding operation method of gapless single-sided welding and double-sided forming of stainless steel pipeline in the embodiment of the present invention are as follows: 1) Reduce deformation. Because stainless steel has a large thermal expansion coefficient and is particularly easy to deform, the larger the gap, the greater the deformation. The gapless grouping greatly reduces the shrinkage of pipeline welding, thereby reducing the deformation of welding. 2) Good weld formation. The pipeline welded by this method has uniform back forming, the excess height is generally 0.5 to 1.5 mm, and the excess height difference is small, which is very beautiful. 3) High internal quality. The radiographic flaw detection of the pipeline welded by this method can reach 100% first-level defect-free. 4) Improve efficiency. The horizontal rotation welding is more efficient than the full-position welding method, which can improve work efficiency by more than 3 times. 5) In particular, in the welding process of thin-walled pipes below 10 mm and ultra-thin-walled pipes of about 2 mm, it is more difficult to control the size of the molten hole using conventional welding methods. The gapless base welding method of the embodiment of the present invention utilizes the heat of the molten pool to directly melt through the parent material to form a weld on the back side during the welding process, without a pinhole effect. It is superior to conventional welding methods in terms of both forming and deformation control.

[0032] In some embodiments, the gap between the gapless pairs is 0-0.5 mm.

[0033] In this technical solution, the stainless steel pipes are paired without gaps, which means that the gap is 0-0.5mm, that is, there is no gap or a very small gap. In addition, the stainless steel pipes are paired to avoid misalignment, and the positioning welding spot should not be too large, otherwise it will affect the back weld formation at that location.

[0034] In some embodiments, the method for protecting the interior of the stainless steel pipe after positioning welding by filling argon gas is as follows:

[0035] The flow rate of argon gas continuously filled in the stainless steel pipeline is selected according to the diameter and length of the stainless steel pipeline, specifically,

[0036] The diameter of the stainless steel pipeline is ≤89mm, the length of the stainless steel pipeline is ≤6m, the flow rate of argon gas filled inside the stainless steel pipeline is 5-10L / min, and the stainless steel pipeline can be welded after the argon gas is filled inside for 5-10 minutes;

[0037] The diameter of the stainless steel pipeline is greater than 89mm, the length of the stainless steel pipeline is greater than 6m, the flow rate of argon gas filled inside the stainless steel pipeline is 10-15L / min, and welding can be carried out only after the stainless steel pipeline is filled with argon gas for 5-10 minutes.

[0038] In this technical solution, the high temperature during the welding process of the gapless stainless steel pipe will cause the metallographic structure of the stainless steel to change, which is easy to oxidize. We have explored and optimized the process parameters of the internal argon protection of the stainless steel pipe, and found that the flow rate of the argon gas filled inside the stainless steel pipe should be selected according to the diameter and length of the stainless steel pipe, as mentioned above.

[0039] It is understandable that if argon protection is not performed on the back of the weld, the weld may rust in later use. The purpose of filling the back of the weld with argon protection is to prevent the high-temperature molten pool from oxidizing in the air, because argon is an inert gas that can effectively isolate oxygen and water vapor in the air, reduce oxidation and burnout on the back of the weld, and thus improve the quality and corrosion resistance of the welded joint. During the argon filling process, the flow of argon should be controlled. The appropriate argon flow can ensure that the weld is fully protected. Too small a flow may lead to insufficient protection, while too large a flow may cause defects such as concave weld root. During the welding process, argon should be filled to the back of the weld continuously until the welding is completed before the argon hose is unplugged to ensure that the weld is continuously protected. The time of argon filling should be controlled before welding. If the time is too short, the argon replacement is not complete, and air will remain in the pipeline, causing oxidation of the weld and even welding defects; if the time is too long, it will cause waste of argon and increase production costs.

[0040] In some embodiments, the control method of welding current intensity is: during welding, the welding current intensity is selected according to the thickness and diameter of the stainless steel pipe, specifically:

[0041] When the thickness of stainless steel pipe is ≤3.5mm and the diameter of stainless steel pipe is ≤5mm, and the welding current intensity is 110~135A;

[0042] When the thickness of the stainless steel pipe is 5mm<10mm, and the diameter of the stainless steel pipe is 60mm<114mm, the welding current intensity is 130~165A.

[0043] Preferably, the control method of the welding current intensity is: the calculation formula of the welding current intensity value is: 1 / 2(D+H)+100; wherein D is the diameter of the stainless steel pipe, H is the thickness of the stainless steel pipe, and 100 is the coefficient.

[0044] In this technical solution, the diameter and thickness of the stainless steel pipe are proportional to the welding current intensity. The larger the diameter of the stainless steel pipe, the greater the welding current. The welding current increases with the thickness of the stainless steel pipe, and vice versa. During the welding process of stainless steel pipes with large diameter and / or thickness, more heat is required to melt the metal to form a weld. A larger current can provide a stronger arc and generate more heat, which helps to melt more metal faster. A larger current can increase the depth of penetration to ensure that the weld can completely penetrate the parent material, forming a molten pool sinking and avoiding defects such as incomplete penetration. During the welding process of pipes with small diameter and / or small thickness, because heat concentration is particularly prone to occur, a correspondingly smaller current is required for welding to avoid defects such as burn-through and weld nodules caused by large currents.

[0045] In some embodiments, the method for controlling the rotation speed of the stainless steel pipeline is: preheating is performed after the arc is started by manual tungsten inert gas welding, and rotation begins after the molten pool sinks. The rotation speed of the stainless steel pipeline is controlled so that the molten pool sinks to the back of the weld, and the rotation speed is adjusted according to the molten pool temperature. If the molten pool temperature is high, the rotation speed of the stainless steel pipeline needs to be accelerated, and if the molten pool temperature is low, the rotation speed of the stainless steel pipeline needs to be slowed down.

[0046] Furthermore, the method for controlling the rotation speed of the stainless steel pipeline also includes: when the gap between the stainless steel pipeline pairs meets the requirement of 0 to 0.5 mm, the molten pool position is maintained between 12 o'clock and 2 o'clock, and clockwise rotation uphill welding is adopted; when the gap between the stainless steel pipeline pairs is greater than 0.5 mm, the welding molten pool position of the gap greater than 0.5 mm is maintained between 12 o'clock and 11 o'clock, and counterclockwise rotation downhill welding is adopted.

[0047] In this technical solution, the rotation speed of the stainless steel pipeline is the welding speed. The control method of the rotation speed of the stainless steel pipeline is: preheating after the manual tungsten inert gas arc welding is used, and the rotation starts after the molten pool sinks. The rotation speed is selected according to the temperature of the molten pool. The high temperature of the molten pool accelerates the rotation speed, and the low temperature of the molten pool slows down the rotation speed. It is generally necessary to stay for about 3 seconds after the arc is struck, mainly for preheating. When the temperature of the molten pool rises, the color of the molten pool changes from dark to bright, and the molten pool begins to sink, it can start to rotate. Otherwise, the temperature of the molten pool is low, and the back of the weld will not be fused. At the same time, you should always pay attention to the change of the molten pool temperature and select the rotation speed according to the temperature of the molten pool. If the molten pool is found to be white and shiny, it means that the molten pool temperature is too high, which will cause the excess height on the back of the weld to be too high, or even burn through. At this time, the rotation speed should be accelerated. If the color of the molten pool is found to be dark and the molten pool does not sink, it means that the molten pool temperature is low and the rotation speed should be slowed down. It is worth noting that this method is not suitable when the diameter of the stainless steel pipeline exceeds 114mm or the thickness of the stainless steel pipeline exceeds 10mm.

[0048] In some embodiments, it also includes: when the thickness of the stainless steel pipeline is ≥2mm, the stainless steel pipeline is beveled before welding, the bevel angle is 60±2 degrees, the single-side bevel angle is 30±1 degrees, and the blunt edge is 0-0.5mm.

[0049] In this technical solution, in actual application, our method of gapless backing welding of stainless steel pipes is mainly used for welding of 3.5-10mm stainless steel thin-walled pipes of centrifugal compressors. The welding effect is also very ideal for stainless steel pipes below 3.5mm, and even ultra-thin-walled pipes below 2mm. When the thickness of the stainless steel pipe is ≥2mm, it is necessary to process the groove, the groove angle is 60±2 degrees, the single-side groove angle is 30±1 degrees, and the blunt edge is 0-0.5mm. The purpose of processing the groove is to ensure full penetration and avoid defects such as lack of fusion and lack of penetration.

[0050] In some embodiments, the cap welding method is manual arc welding, the current intensity of the manual arc welding is 65-80A, and the electrode diameter is 3.2mm.

[0051] In this technical solution, manual arc welding is required for cap welding, because the base welding adopts the welding method of self-melting of the base material without adding welding wire, so the thickness of the base welding is relatively thin. If manual tungsten inert gas arc welding is used to continue welding, it will cause serious oxidation of the back weld. Manual arc welding with smaller welding parameters is required, and the current intensity of 3.2mm diameter welding rod is selected at 65~80A. Due to the small heat input, the stainless steel weld stays in the high temperature area for a shorter time, effectively avoiding intergranular corrosion and improving the performance of the weld.

[0052] A second aspect of an embodiment of the present invention provides an application of a stainless steel pipeline welding method, wherein the stainless steel pipeline welding method is used for welding stainless steel pipelines of compressors.

[0053] In summary, the welding method of the stainless steel pipeline of the present invention is to obtain the welding process parameters for the gapless pairing of the stainless steel pipelines after multiple tests and explorations, including welding current intensity, rotation speed, etc., so that the welding method has the following advantages:

[0054] 1. Reduce deformation. Stainless steel has a large thermal expansion coefficient and is particularly prone to deformation. The larger the gap, the greater the deformation. Gapless assembly greatly reduces the shrinkage of pipeline welding, thereby reducing the deformation of welding.

[0055] 2. Good weld formation. The back of the pipe welded by this method is evenly formed, the excess height is generally 0.5-1.5mm, and the excess height difference is small, which is very beautiful.

[0056] 3. High internal quality. The stainless steel pipes welded by this method can reach 100% first-class defect-free in the radiographic inspection.

[0057] 4. Improve performance. Cover welding needs to use manual arc welding, which shortens the time that the stainless steel pipeline weld stays in the high temperature area, effectively avoids intergranular corrosion, and improves the performance of the weld.

[0058] 5. Improve efficiency. Horizontal rotation welding is more efficient than full-position welding and can improve work efficiency by more than 3 times.

[0059] 6. Especially in the welding process of thin-walled pipes, it is more difficult to control the size of the molten hole with conventional welding methods. The method of the present invention is superior to conventional welding methods in terms of both forming and deformation control.

[0060] The welding method of stainless steel pipelines of the present invention has been successfully used in the manufacture of engineering pipelines of more than 1,000 large centrifugal compressors. The technology is mature and the quality is safe and stable. It is applied to many national key projects including million tons of ethylene, long-distance pipelines, and 100,000 air separation compressors. The first pass rate of radiographic flaw detection of centrifugal compressor pipelines has been increased from the original 80% to more than 96% overall. Among them, the radiographic flaw detection welds of stainless steel pipelines welded by the welding method of the present invention can reach 100% of the first-level defect-free, saving more than 5.4 million yuan for the enterprise every year.

[0061] Example 1 A welding method for stainless steel pipeline

[0062] A welding method for a stainless steel pipeline specifically comprises the following steps:

[0063] Step 1: Preparation before welding

[0064] The thickness of the stainless steel pipe in Example 1 is 5 mm, and a groove needs to be processed. The groove angle of the pipe is 60 degrees, the single-side groove angle is 30 degrees, there is no blunt edge or the blunt edge is less than 0.5 mm, and the burrs on the inner wall of the pipe are cleaned.

[0065] Step 2: Stainless steel pipe assembly

[0066] like Figure 1 As shown, perform gapless assembly, leaving no gap or very small gap, generally 0-0.5mm. Pay attention to avoid misalignment during pipeline assembly, and the positioning welding spot should not be too large, otherwise it will affect the back weld formation at this location.

[0067] Step 3: Soldering

[0068] (1) When welding, select the uninterrupted argon filling flow rate on the back according to the diameter and length of the pipeline. Generally, for diameters ≤89mm and lengths ≤6m, the argon filling flow rate is 5-10L / min, and welding can be carried out after 5-10 minutes. For diameters greater than 89mm and lengths greater than 6m, the argon filling flow rate is 10-15L / min, and welding can be carried out after 10-15 minutes.

[0069] (2) Select the current intensity according to the thickness and diameter of the pipeline. When the pipeline thickness is 3.5mm≤≤5mm, and the pipeline diameter is 33mm≤≤60mm, the welding current intensity should be 110~135A. When the pipeline thickness is 5mm<≤10mm, and the pipeline diameter is 60mm<≤114mm, the welding current intensity should be 130~165A.

[0070] (3) The welding speed is controlled at 6-10cm / min. After the arc is struck, it is generally necessary to stay for about 3 seconds. When the temperature of the molten pool rises, the color of the molten pool changes from dark to light, and the molten pool begins to sink, it is time to start rotating clockwise and use horizontal rotation welding. The position of the molten pool is kept between 12 o'clock and 2 o'clock (such as Figure 2 As shown), use uphill welding, pay attention to the temperature change of the molten pool at all times, and select the rotation speed according to the molten pool temperature.

[0071] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. Welding method of stainless steel pipes, It is characterized in that It includes the bottom welding of stainless steel pipeline and the cover welding of stainless steel pipeline; wherein, the bottom welding of stainless steel pipeline includes: Assemble stainless steel pipes without gaps; Perform positioning welding on the assembled stainless steel pipes; The interior of the stainless steel pipeline after positioning welding is filled with argon gas for protection, and manual tungsten inert gas welding is used to perform base welding on the front of the stainless steel pipeline after positioning welding. The welding current intensity and the rotation speed of the stainless steel pipeline are controlled to make the molten pool sink to the back of the weld, thereby achieving the formation of the weld on the back of the stainless steel pipeline.

2. The welding method for stainless steel pipeline according to claim 1, It is characterized in that The gap between the gapless pairs is 0 to 0.5 mm.

3. The welding method for stainless steel pipeline according to claim 1, It is characterized in that The method for protecting the interior of the stainless steel pipeline after positioning welding by filling argon gas is as follows: The flow rate of argon gas continuously filled in the stainless steel pipeline is selected according to the diameter and length of the stainless steel pipeline, specifically, The diameter of the stainless steel pipeline is ≤89mm, the length of the stainless steel pipeline is ≤6m, the flow rate of argon gas inside the stainless steel pipeline is 5-10L / min, and the stainless steel pipeline can be welded after the argon gas is filled inside for 5-10 minutes; The diameter of the stainless steel pipeline is greater than 89mm, the length of the stainless steel pipeline is greater than 6m, the flow rate of argon gas filled inside the stainless steel pipeline is 10-15L / min, and welding can be carried out only after the stainless steel pipeline is filled with argon gas for 5-10 minutes.

4. The welding method for stainless steel pipeline according to claim 1, It is characterized in that The control method of welding current intensity is: when welding, the welding current intensity is selected according to the thickness and diameter of the stainless steel pipe, specifically: When the thickness of stainless steel pipe is ≤3.5mm and the diameter of stainless steel pipe is ≤5mm, and the welding current intensity is 110~135A; When the thickness of the stainless steel pipe is 5mm<10mm, and the diameter of the stainless steel pipe is 60mm<114mm, the welding current intensity is 130~165A.

5. The welding method for stainless steel pipeline according to claim 4, It is characterized in that The control method of welding current intensity is: the calculation formula of welding current intensity value is: 1 / 2(D+H)+100; Where D is the diameter of the stainless steel pipe, H is the thickness of the stainless steel pipe, and 100 is the coefficient.

6. The method for welding a stainless steel pipeline according to claim 4, It is characterized in that The method for controlling the rotation speed of the stainless steel pipeline is as follows: preheat the manual tungsten inert gas arc welding after the arc is started, start rotating after the molten pool sinks, control the rotation speed of the stainless steel pipeline to make the molten pool sink to the back of the weld, and adjust the rotation speed according to the molten pool temperature. If the molten pool temperature is high, the rotation speed of the stainless steel pipeline needs to be accelerated, and if the molten pool temperature is low, the rotation speed of the stainless steel pipeline needs to be slowed down.

7. The method for welding a stainless steel pipeline according to claim 6, It is characterized in that The method for controlling the rotation speed of the stainless steel pipeline also includes: when the gap between the stainless steel pipeline pairs meets the requirement of 0-0.5 mm, the molten pool position is maintained between 12 o'clock and 2 o'clock, and clockwise rotation uphill welding is adopted; when the gap between the stainless steel pipeline pairs is greater than 0.5 mm, the welding molten pool position of the gap greater than 0.5 mm is maintained between 12 o'clock and 11 o'clock, and counterclockwise rotation downhill welding is adopted.

8. The gapless bottom welding method for stainless steel pipeline according to claim 1, It is characterized in that Also includes: When the thickness of the stainless steel pipe is ≥2mm, the stainless steel pipe shall be grooved before welding. The groove angle is 60±2 degrees, the single-side groove angle is 30±1 degrees, and the blunt edge is 0~0.5mm.

9. The method for welding a stainless steel pipeline according to claim 1, It is characterized in that The cap welding method is manual arc welding, the current intensity of the manual arc welding is 65-80A, and the diameter of the welding rod is 3.2mm.

10. Application of a welding method for stainless steel pipelines, It is characterized in that The stainless steel pipeline welding method according to any one of claims 1 to 9 is used for welding stainless steel pipelines of compressors.

Citation Information

Cited By

  • Full penetration welding method for austenitic stainless steel zero-clearance K-type joint

    CN119681390A

  • Composite welding method for low-nickel austenitic stainless steel low-temperature pipeline

    CN121245139A