By targeting the electromagnetic pulse energy on the metal construction interface, combined with vacuum sealing and electromagnetic impact treatment, the problem of metal interface healing and connection under low temperature and small deformation conditions is solved, and the healing performance and mechanical properties of the metal construction interface are improved. Effect.

CN118720645APending Publication Date: 2024-10-01WUHAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410797650.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing metal construction and forming technology achieves interface connection under high temperature and large deformation conditions, which limits the scope of engineering application of construction and forming technology. How to achieve interface healing and connection of metal components under conditions of lower temperature, small deformation or even no plastic deformation. , has become an urgent problem to be solved.

Method used

By targeting the electromagnetic pulse energy to the metal construction interface to promote pre-melting, migration and healing of the interface, vacuum sealing and electromagnetic shock treatment are used to control the electrode movement mode and pulse current parameters to achieve interface connection and avoid large plastic deformation and Significant temperature rise.

Benefits of technology

Under the conditions of no large plastic deformation and no significant temperature rise, the electromagnetic pulse energy causes Joule heating and electromagnetic vibration effects, causing the interface atomic vibration to become unstable, achieving local melting and connection of the metal interface, improving the healing performance of the metal construction interface, and improving the construction Mechanical properties of formed metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720645A_ABST
    Figure CN118720645A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the healing performance of a metal construction interface. The method comprises the steps that the construction interface of a metal element is ground and polished; the metal elements are combined and then subjected to vacuum seal welding along the outer contour of the construction interface, and a seal welding metal blank is obtained; carrying out electromagnetic impact treatment on the vacuum seal welding surface until the metal construction interface is completely healed; electromagnetic pulse energy acts on a metal construction interface in a targeted manner, and on the premise of no severe plastic deformation and no remarkable temperature rise, vibration instability or shear instability of atoms on the surface layer of the construction interface is caused by the Joule heating effect caused by coupling pulse current and the electromagnetic vibration effect caused by a pulse electromagnetic field, so that the metal construction interface is subjected to mechanical deformation or mechanical deformation. And under the auxiliary action of the magnetic compression effect, healing or connection of the metal construction interface is achieved, and the purpose of improving the healing performance of the metal construction interface is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material technology, and in particular relates to a method for improving the healing performance of a metal construction interface. Background Art

[0002] Metal components are widely used in aviation, aerospace, wind power, nuclear power, engineering machinery and other fields. They are the core components of major equipment and are indispensable in national security and national economic engineering applications. At present, such large metal components are often made of 100-ton ingots. Due to the size effect of the metal solidification process, defects such as macro segregation, shrinkage and looseness often exist inside the large ingots, which seriously affect the quality of the components and have become a global problem.

[0003] Metal building forming is a new process that obtains homogeneous large forgings by vacuum building and sealing multiple high-quality small ingots and then subjecting them to high-temperature large deformation. It uses multiple small-sized homogenized slabs as the basic elements, and through surface activation, vacuum packaging, high-temperature deformation and other means, the structure and performance of the building interface are completely consistent with the matrix, thereby obtaining the homogenized parent material required for large forgings, realizing a new manufacturing method of "making large from small". The main technical problem in the construction and forming of large forgings is how to ensure seamless connection of the interface, and the main scientific problem is the deformation and connection problem of the interface. At present, high temperature deformation (CN 105618506B, 2019; CN 113695502 B, 2023) and electric shock assisted high temperature deformation (CN 113579451A, 2021; CN 113579452 A, 2021) methods are mainly used for the construction and forming of large forgings to promote the healing of the construction interface (CN 106653629 A) and achieve the purpose of interface connection, thereby ensuring the mechanical properties of the constructed metal forgings.

[0004] However, the above-mentioned technical methods for promoting the construction of interface connection of large metal forgings all require high temperature and large deformation, that is, the current metal construction forming technology achieves solid-state connection through repeated large deformation during the free forging process. The solid-state connection conditions of the construction forming process are high temperature, high vacuum, and large plastic deformation conditions, which seriously limits the engineering application scope of the construction forming technology.

[0005] How to make the interface of large metal components heal and connect under conditions of low temperature, small deformation or even no plastic deformation, while ensuring the mechanical properties of the constructed metal components, has become an urgent problem to be solved. Summary of the invention

[0006] The purpose of the present invention is to provide a method for improving the healing performance of metal construction interfaces, by targeting electromagnetic pulse energy to the metal construction interface, promoting pre-melting of the metal construction interface, promoting interface migration, bridging and healing, improving the connection state of the metal construction interface, and improving the mechanical properties of the constructed metal components.

[0007] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0008] The method for improving the healing performance of metal structure interface comprises the following steps:

[0009] S1) grinding and polishing the construction interface of the metal element;

[0010] S2) combining the metal elements and performing vacuum sealing along the outer contour of the construction interface to obtain a sealed metal blank;

[0011] S3) The vacuum-sealed surface is subjected to electromagnetic impact treatment until the metal construction interface is completely healed.

[0012] According to the above scheme, the metal element in step S1 has at least one planar construction interface.

[0013] According to the above scheme, the vacuum sealing in step S2 adopts vacuum electron beam welding or vacuum laser welding, and the weld penetration is controlled to be 5-10% of the minimum thickness of the sealing metal blank.

[0014] According to the above scheme, when the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, the single moving distance of the electrode is controlled to be smaller than the radius of the circular cross section of the sharp electrode used.

[0015] According to the above scheme, during the electromagnetic impact treatment in step S3, the maximum surface temperature T of the metal blank is controlled max ≤kT m , T m It represents the melting point of the metal element being processed, and the value range of k is 0.05 to 0.25.

[0016] According to the above scheme, when the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, the electrode connection and movement method includes the following steps:

[0017] The electrodes are connected facing each other on the vacuum sealing surface, and then moved in the opposite direction along the outer contour of the vacuum sealing surface until the connection line of the electrode covers the entire vacuum sealing surface.

[0018] According to the above scheme, when the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, in the case where the vacuum sealing surface is rectangular, the electrode connection and movement method includes the following steps:

[0019] (1) First, connect the electrodes at two adjacent corners of the rectangular vacuum sealing surface, and then move parallel to the outer contour of the vacuum sealing surface until the connection line of the electrode covers the entire vacuum sealing surface;

[0020] (2) Then, electrodes are connected at two opposite corners of the rectangular vacuum sealing surface, and moved in the opposite direction along the outer contour of the vacuum sealing surface until the connection line of the electrodes covers the entire vacuum sealing surface.

[0021] According to the above scheme, during the electromagnetic impact treatment in step S3, the peak current density of the pulse current is controlled to be in the range of 50 to 300 A / mm 2 , the pulse current frequency range is 20 to 300 Hz, and the pulse duty cycle is 10 to 40%.

[0022] According to the above scheme, the electromagnetic shock treatment process in step S3 includes a high power mode:

[0023] The peak current density of the pulse current ranges from 50 to 300 A / mm 2 , the pulse current frequency range is 50~300Hz, the pulse duty cycle is 10~25%, and the k value range is 0.10~0.25.

[0024] According to the above scheme, the electromagnetic shock treatment process in step S3 includes a low power mode:

[0025] The peak current density of the pulse current ranges from 50 to 200 A / mm 2 , the pulse current frequency range is 20 to 200 Hz, the pulse duty cycle is 25 to 40%, and the k value range is 0.05 to 0.15.

[0026] According to the above scheme, in step S3, the electromagnetic shock treatment uses repeated switching between high and low power modes to achieve a better healing effect on the constructed interface.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention introduces electromagnetic pulse energy into the metal interface sealing welding area in the form of pulse current, that is, when the electromagnetic impact treatment is performed on the metal interface sealing welding area, on the one hand, the electromagnetic oscillation (or oscillating electromagnetic field) generated by the intermittent electromagnetic pulse will generate cyclic dynamic stress (or electromagnetic force) on the surface atoms of the interface, and at the same time, the pulse current will generate Joule heat when it circulates inside the alloy. Under the condition of reasonable control of Joule heat, the interface atoms undergo a certain degree of thermal activation, and under the action of cyclic compressive stress and shear stress caused by electromagnetic vibration, the coupling thermal activation and cyclic compressive stress and shear stress action, it is easy to cause the vibration instability or shear instability of the interface atoms, resulting in the metal interface starting to melt, thereby promoting the melting of the metal interface from nanometer scale to micrometer scale, causing the construction of the metal interface to melt locally, which is conducive to the connection of the metal interface; on the other hand, the electromagnetic pulse energy is targeted to the construction interface area through the electrode, which is conducive to the connection of the metal interface under the action of the magnetic compression effect, thereby achieving the purpose of the construction interface connection without large plastic deformation and significant temperature rise.

[0029] The present invention targets electromagnetic pulse energy at the metal construction interface, and under the premise of no large plastic deformation and no significant temperature rise, causes vibration instability or shear instability of the surface atoms of the construction interface through the Joule heating effect caused by the coupling pulse current and the electromagnetic vibration effect caused by the pulse electromagnetic field, that is, the interface is pre-melted or even partially melted, and with the assistance of the magnetic compression effect, the metal construction interface is healed or connected, thereby achieving the purpose of improving the healing performance of the metal construction interface. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 : Schematic diagram of the electromagnetic impact method for improving the healing performance of metal construction interfaces according to the present invention.

[0031] Figure 2 :Diagram of electromagnetic impact process of TC11 titanium alloy construction interface.

[0032] Figure 3 : Interface state diagram of TC11 titanium alloy element after sealing welding.

[0033] Figure 4 : Local connection diagram of the interface constructed by TC11 titanium alloy after electromagnetic shock treatment.

[0034] Figure 5 :Diagram of electromagnetic impact process of 6082 aluminum alloy construction interface.

[0035] Figure 6 : Interface state diagram of 6082 aluminum alloy element after sealing welding.

[0036] Figure 7 : Local connection diagram of 6082 aluminum alloy construction interface after electromagnetic shock treatment. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0038] Example 1

[0039] Taking TC11 titanium alloy as an example, the dimensions of the TC11 titanium alloy construction unit sample are: L = 55mm (X direction), W = 10mm (Y direction), H = 5mm (Z direction). The two TC11 titanium alloy construction units are sealed and connected by vacuum welding, and then the TC11 titanium alloy interface sample is treated by electromagnetic impact. The process method is shown in the figure. Figure 1 As shown, the specific process is as follows:

[0040] S1) grinding and polishing the construction interface of the rectangular TC11 titanium alloy unit;

[0041] S2) combining the TC11 titanium alloy primitives and performing vacuum sealing welding along the outer contour of the constructed interface to obtain a sealing metal blank;

[0042] S3) Perform electromagnetic impact treatment on the vacuum sealing surface until the metal construction interface is completely healed; control the maximum surface temperature T of the metal blank max ≤kT m ; When the rectangular vacuum sealing surface is subjected to electromagnetic impact treatment, the electrode connection and movement method is as follows:

[0043] First, the electrodes are connected at two adjacent corners of the rectangular vacuum-sealed surface, and then moved parallel to the outer contour of the vacuum-sealed surface until the connection line of the electrode covers the entire vacuum-sealed surface; at the same time, the electromagnetic shock treatment is performed in high-power mode; then the electrodes are connected at two opposite corners of the rectangular vacuum-sealed surface, and moved in the opposite direction along the outer contour of the vacuum-sealed surface until the connection line of the electrode covers the entire vacuum-sealed surface; at the same time, the electromagnetic shock treatment is performed in low-power mode. The action parameters of the electromagnetic shock process are shown in Table 1.

[0044] Table 1

[0045]

[0046] The electromagnetic impact process of the interface of TC11 titanium alloy is treated by the above method. Figure 2 As shown in Figure 2, the interface connection of TC11 titanium alloy before electromagnetic shock treatment is as follows: Figure 3 As shown in Figure 2, the interface connection of TC11 titanium alloy after electromagnetic shock treatment is observed. Figure 4 As shown, the effect of improving the healing performance of the construction interface is achieved.

[0047] Example 2

[0048] Taking 6082 aluminum alloy as an example, the dimensions of the 6082 aluminum alloy construction unit sample are: L = 60mm (X direction), W = 20mm (Y direction), H = 5mm (Z direction). The two TC11 titanium alloy construction units are sealed and connected by vacuum welding, and then the 6082 aluminum alloy interface sample is treated by electromagnetic impact. The process method is shown in the figure. Figure 1 As shown, the specific process is as follows:

[0049] S1) grinding and polishing the construction interface of the rectangular 6082 aluminum alloy primitive;

[0050] S2) combining the 6082 aluminum alloy elements and performing vacuum sealing along the outer contour of the construction interface to obtain a sealed metal blank;

[0051] S3) Perform electromagnetic impact treatment on the vacuum sealing surface until the metal construction interface is completely healed; control the maximum surface temperature T of the metal blankmax ≤kT m ; When the rectangular vacuum sealing surface is subjected to electromagnetic impact treatment, the electrode connection and movement method is as follows:

[0052] First, the electrodes are connected at two adjacent corners of the rectangular vacuum-sealed surface, and then moved parallel to the outer contour of the vacuum-sealed surface until the connection line of the electrode covers the entire vacuum-sealed surface; at the same time, the electromagnetic shock treatment is performed in high-power mode; then the electrodes are connected at two opposite corners of the rectangular vacuum-sealed surface, and moved in the opposite direction along the outer contour of the vacuum-sealed surface until the connection line of the electrode covers the entire vacuum-sealed surface; at the same time, the electromagnetic shock treatment is performed in low-power mode. The action parameters of the electromagnetic shock process are shown in Table 2.

[0053] Table 2

[0054]

[0055] The electromagnetic impact process of the interface of 6082 aluminum alloy is treated by the above method. Figure 5 As shown in the figure, the interface connection of 6082 aluminum alloy before electromagnetic shock treatment is as follows Figure 6 As shown in the figure, the interface connection of 6082 aluminum alloy after electromagnetic shock treatment is observed as follows Figure 7 As shown, the effect of improving the healing performance of the construction interface is achieved.

[0056] In summary, the present invention uses a specific process method to introduce suitable electromagnetic pulse energy in the form of pulse current into the metal interface sealing connection area, causing local melting of the metal interface, and promoting the connection of the metal interface under the action of the magnetic compression effect, thereby achieving the purpose of constructing the interface connection without large plastic deformation and without significant temperature rise, thereby achieving the purpose of improving the mechanical properties and service performance of the constructed metal.

[0057] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.

Claims

1. A method for improving the healing performance of metal construction interfaces, characterized in that The following steps are involved: S1) grinding and polishing the construction interface of the metal element; S2) combining the metal elements and performing vacuum sealing along the outer contour of the construction interface to obtain a sealed metal blank; S3) The vacuum-sealed surface is subjected to electromagnetic impact treatment until the metal construction interface is completely healed.

2. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that In step S1, the metal element has at least one planar construction interface.

3. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that The vacuum sealing in step S2 adopts vacuum electron beam welding or vacuum laser welding, and the weld penetration is controlled to be 5-10% of the minimum thickness of the sealing metal blank.

4. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that When the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, the single moving distance of the electrode is controlled to be smaller than the radius of the circular cross section of the sharp electrode used.

5. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that Step S3: During the electromagnetic impact treatment, the maximum surface temperature T of the metal blank is controlled. max ≤kT m , T m It represents the melting point of the metal element being processed, and the value range of k is 0.05 to 0.

25.

6. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that When the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, the electrode connection and movement method includes the following steps: The electrodes are connected facing each other on the vacuum sealing surface, and then the electrodes are moved in the opposite direction along the outer contour of the vacuum sealing surface until the connection line of the electrodes covers the entire vacuum sealing surface.

7. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that During the electromagnetic shock treatment in step S3, the peak current density of the pulse current is controlled to be in the range of 50 to 300 A / mm 2 , the pulse current frequency range is 20 to 300 Hz, and the pulse duty cycle is 10 to 40%.

8. The method for improving the healing performance of metal construction interfaces according to claim 1, characterized in that When the vacuum sealing surface is subjected to electromagnetic impact treatment in step S3, in the case where the vacuum sealing surface is rectangular, the electrode connection and movement method includes the following steps: (1) First, connect electrodes at two adjacent corners of the rectangular vacuum-sealed surface, and then move the electrodes parallel to the outer contour of the vacuum-sealed surface until the connecting line of the electrodes covers the entire vacuum-sealed surface; at the same time, use a high-power mode to perform electromagnetic impact treatment; (2) Then, electrodes are connected to two opposite corners of the rectangular vacuum-sealed surface, and the electrodes are moved in the opposite direction along the outer contour of the vacuum-sealed surface until the connecting line of the electrodes covers the entire vacuum-sealed surface; at the same time, electromagnetic shock treatment is performed in a low-power mode.

9. The method for improving the healing performance of metal construction interfaces according to claim 8, characterized in that The high power mode: The peak current density of the pulse current ranges from 50 to 300 A / mm 2 , the pulse current frequency range is 50~300Hz, and the pulse duty cycle is 10~25%.

10. The method for improving the healing performance of metal construction interfaces according to claim 8, characterized in that The low power mode: The peak current density of the pulse current ranges from 50 to 200 A / mm 2 , the pulse current frequency range is 20 to 200 Hz, and the pulse duty cycle is 25 to 40%.

Citation Information

Patent Citations

  • High-energy filtering protector

    CN104578071A

  • Electromagnetic pulse welding assembly

    CN114769831A

  • Method for improving interface connectivity and interface feature distribution of solid metal

    CN115058561A

  • Pulse electromagnetic method for water treatment and dedicated equipment

    CN1686849A

  • Vacuum electromagnetic contactor

    JP1990288036A