Copper-aluminum composite sheet and preparation method thereof
By combining explosive welding and rolling processing in the preparation of copper-aluminum composite panels, the problems of thickness limitation and warping deformation of the composite panels are solved, and copper-aluminum composite thin sheets with excellent mechanical properties are efficiently prepared, which are suitable for new energy materials.
Patent Information
- Application Number
- CN202411022842.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing preparation process of copper-aluminum composite panels, the explosion welding method has problems such as limited thickness of the cladding material and low production efficiency. The rolling method causes the plate to warp and deform due to inconsistent extension of copper and aluminum, affecting process stability and efficiency.
After using the explosive welding method to obtain the copper-aluminum composite plate blank, it is cut to the same specifications and combined with back-to-back welding, and then cold-rolled in the rolling equipment. The copper surface is centered to offset the extensional plastic deformation and avoid warpage. Deformation.
It achieves the preparation of high-quality copper-aluminum composite sheets, avoids warping deformation, improves production efficiency, and is suitable for the field of new energy materials.
Smart Images

Figure CN118720657A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of layered metal composite material processing, and specifically relates to a copper-aluminum composite sheet and a preparation method thereof. Background Art
[0002] Dissimilar metal composite materials are made of different types of metals through special processes and have unique properties and advantages. This material has broad application prospects in new energy and other fields. With the improvement of material performance requirements in new energy vehicles and other fields, the demand for copper-aluminum composite plates in the new energy vehicle industry is increasing rapidly. At present, the main preparation processes of copper-aluminum composite plates include explosive welding and rolling.
[0003] Explosive welding is a method that uses the instantaneous high temperature and high pressure generated by the explosion of explosives to cause metal plates to collide with each other, generate a high-speed jet during the collision, remove impurities on the surface between the two metal plates, and achieve metallurgical bonding of the plates under extremely high pressure. It is particularly suitable for surface bonding between dissimilar layered metal materials. However, this method has a technical bottleneck in the thickness of the composite material. Usually, the thickness of the composite metal in one explosion welding should be 3 to 15 mm. The composite material should not be too thick or too thin. It is generally suitable for the composite preparation of composite medium and thick plates, but not for the composite preparation of thin plates. In addition, based on its working principle, the current production process of the explosive composite process is still mainly manual, making it difficult to achieve full mechanization and automation, and the production efficiency is relatively low.
[0004] The rolling method is a pressure processing method in which a metal billet passes through the gap (of various shapes) between a pair of rotating rollers. Due to the compression of the rollers, the cross-section of the material is reduced and the length is increased. This process is stable, efficient, and suitable for mass production. However, during the rolling process of a single copper-aluminum composite plate, due to the inconsistent extension of copper and aluminum, the aluminum layer flows faster under pressure, while the copper layer flows slower under pressure, which can easily cause the plate to show "C-shaped" warping deformation, thereby affecting the normal rolling process, and in severe cases, causing the process to be interrupted.
[0005] Therefore, how to prepare a high-quality copper-aluminum composite sheet with excellent comprehensive mechanical properties is an urgent problem to be solved. Summary of the invention
[0006] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art and provide a method for preparing a high-performance copper-aluminum composite sheet. The method first obtains a copper-aluminum composite sheet blank by explosion welding, then cuts and processes two composite sheets with exactly the same size and specifications for back-to-back welding and assembly, and uses a copper surface centering method. Finally, the assembled composite sheet is cold-rolled under suitable rolling mill equipment, which can effectively overcome the warping deformation problem that often occurs during the rolling process of a single copper-aluminum composite sheet and achieve high-quality copper-aluminum composite. The copper-aluminum composite sheet prepared by this method has excellent comprehensive mechanical properties and is suitable for the field of new energy materials, especially for use in products such as poles in the new energy industry.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a copper-aluminum composite sheet, comprising the following steps:
[0009] S1. Using explosive welding technology to perform explosive welding composite processing on aluminum plates and copper plates to obtain copper-aluminum composite blanks, and then leveling, testing, and cutting the copper-aluminum composite blanks to obtain qualified copper-aluminum composite plates;
[0010] S2. Using the principle of rolling processing technology, the copper-aluminum composite plate obtained in step S1 is subjected to rolling and thinning treatment to obtain the desired copper-aluminum composite thin plate. The specific process is as follows:
[0011] 1) Cold-cut the copper-aluminum composite plate, and then combine the two copper-aluminum composite plates of the same size and specifications back to back. The combination requires the copper side to be in the middle and the aluminum side to face outward, and the two copper sides to be close together. Then weld the edges around the outer side of the copper material in the middle, intermittently weld along the length direction, and fully weld in the width direction. All welds must be welded firmly and reliably;
[0012] 2) The copper-aluminum composite plate assembled in step 1) is rolled according to set rolling process parameters. After rolling is completed, the weld is removed to obtain the copper-aluminum composite sheet.
[0013] Furthermore, in step S1, the material of the aluminum plate is pure aluminum or aluminum alloy, and the material of the copper plate is pure copper or copper alloy.
[0014] In some specific implementations, in step S1, the material of the aluminum plate is 1060 pure aluminum, and the material of the copper plate is T2 red copper.
[0015] In some specific implementations, in step S1, the aluminum plate is the base layer with a thickness of ≥7 mm; the copper plate is the cladding layer with a thickness of 3-8 mm.
[0016] In some specific implementations, in step S1, the length of the aluminum plate and the copper plate are both 800-1500 mm, and the width is both 300-600 mm.
[0017] Furthermore, step S1 specifically includes the following steps:
[0018] The surfaces of the aluminum plate and copper plate to be welded are pre-polished and cleaned to meet the requirements of the explosive composite process;
[0019] The pretreated aluminum plate is placed horizontally on a flat foundation, and gap columns for explosive welding are evenly arranged along the edge and middle of the aluminum plate surface, and then the pretreated copper plate is placed on the gap columns, wherein the polished surface of the aluminum plate faces upward and the polished surface of the copper plate faces downward, and finally a protective layer is laid on the copper plate, and an explosive layer is laid on the protective layer and detonated by a detonator, and the explosion residue and the protective layer are removed to obtain a copper-aluminum composite billet;
[0020] The prepared copper-aluminum composite billet is first leveled, and then an ultrasonic flaw detector is used to detect the bonding condition of the composite interface, and the poor bonding area is marked. The copper-aluminum composite sheet that passes the inspection is cut through mechanical cold working.
[0021] In some specific embodiments, the spacing between the gap columns for explosion welding is 100-150 mm, and the protective layer is a 1-2 mm thin wood board.
[0022] In some specific embodiments, in step 1), the copper-aluminum composite plate is cold-cut into strips, and the specific specifications are determined according to the capacity of the rolling equipment.
[0023] It should be noted that when two copper-aluminum composite panels of the same size and specifications are assembled back to back in step 1), if the panel surfaces are uneven, they need to be leveled first.
[0024] In some specific embodiments, in step 1), conventional arc welding MAG welding is used to weld the outer edges of the middle copper material, and the welding process parameters are: current 220-250A, voltage 29-30V, welding speed 12-15cm / min, shielding gas flow rate 15-20L / min, welding 100mm every 100mm along the length direction, and full welding in the width direction.
[0025] In some specific embodiments, in step 2), the rolling is multiple small-pressure rolling, and the rolling process parameters are: the maximum pressure of a single pass is controlled to be 5%-20% of the thickness of the copper-aluminum composite plate, the total deformation is controlled to be less than 80%, and the rolling processing speed is controlled within 20m / min.
[0026] The present invention combines and welds two copper-aluminum composite plates and then rolls them, which can restrain the extension plastic deformation of the copper and aluminum during the rolling process. The centering of the copper surface can offset the warping deformation, thereby achieving consistent extension of the copper and aluminum, thereby avoiding warping deformation of the plate.
[0027] A copper-aluminum composite sheet is prepared according to the preparation method.
[0028] The copper-aluminum composite thin plate adopts a layered composite connection structure and has a thickness of 3-8 mm, wherein the thickness of the copper plate is 1-3 mm and the thickness of the aluminum plate is 2-6 mm.
[0029] Beneficial effects of the present invention:
[0030] The method for preparing copper-aluminum composite thin plates provided by the present invention fully utilizes and combines the principle advantages of explosion welding and rolling processing, and adopts advanced combined welding technology to successfully avoid the problem of "C-shaped" warping deformation of the copper-aluminum composite plate due to the inconsistent extension of copper and aluminum during the rolling process. Through the combination and optimization of the "explosion + rolling" process, not only can the preparation of copper-aluminum composite thin plates be successfully realized, but the method also has mature process technology, simple operation process, high production efficiency, and is easy to realize mass production.
[0031] The copper-aluminum composite thin plate prepared by the method of the present invention has a good appearance, no microcracks or warping deformation on the surface, and has excellent mechanical properties. It is suitable for the field of new energy materials, especially for use in products such as poles in the new energy industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Schematic diagram of the copper-aluminum composite plate rolling billet assembly. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.
[0034] The aluminum plate used in the following embodiments and comparative examples is a 1060 pure aluminum plate, and the copper plate is a T2 copper plate.
[0035] Example 1
[0036] 1) Obtain an aluminum plate with a length of 1500 mm, a width of 450 mm, and a thickness of 7 mm and a copper plate with a length of 1500 mm, a width of 450 mm, and a thickness of 6 mm, and perform surface polishing and pre-cleaning treatment on their surfaces to be welded to meet the requirements of the explosive composite process;
[0037] 2) Place the pretreated aluminum plate horizontally on a flat foundation, evenly arrange gap columns for explosive welding along the edge and middle of the aluminum plate surface, with a spacing of 150 mm between the gap columns, then place a copper plate (polished surface facing downward) on the gap columns, and finally lay a 1.5 mm thin wood board on the copper plate, lay an explosive layer on the thin wood board and detonate it through a detonator, remove the explosion residue and the thin wood board to obtain a copper-aluminum composite billet;
[0038] 3) The prepared copper-aluminum composite blank is first leveled, and then an ultrasonic flaw detector is used to detect the bonding condition of the composite interface, and the poor bonding area is marked, and a qualified copper-aluminum composite plate workpiece is cut and processed by mechanical cold working;
[0039] 4) Cold cutting the copper-aluminum composite plate-shaped workpiece into a strip-shaped copper-aluminum composite plate with a specification of 250*400mm;
[0040] 5) Combine two copper-aluminum composite plates of the same size and specifications after cutting back to back (if the plate surface is uneven, it needs to be leveled first), with the copper side in the middle and the aluminum side facing outward (the two copper sides are required to be close together with almost no gap), and then weld the outer edge of the copper material in the middle using traditional arc welding MAG welding. The welding process parameters are: current 230A, voltage 30V, welding speed 15cm / min, shielding gas flow 18L / min, welding 100mm every 100mm along the length direction, full welding in the width direction, and all welds must be welded firmly and reliably;
[0041] 6) The assembled copper-aluminum composite plate is rolled 8 times on a rolling mill. The specific rolling process parameters are as follows: the maximum pressing amount of a single rolling pass is controlled to be 9.8% of the plate thickness, the total deformation is controlled to be 63%, and the rolling processing speed is controlled to be 5 m / min. After rolling is completed, the weld is removed to obtain the final finished copper-aluminum composite sheet.
[0042] The copper-aluminum composite thin plate prepared in this embodiment has a copper plate thickness of 2.2 mm and an aluminum plate thickness of 2.6 mm, and has a good appearance, no microcracks on the surface, no warping or deformation, and a shear strength of 72 MPa.
[0043] Comparative Example 1
[0044] Compared with Example 1, the difference of this comparative example is that the number of rolling passes is 4, the maximum pressing amount of a single rolling pass is controlled to be 26.3% of the plate thickness, and other conditions remain unchanged. The relevant performance results of the obtained copper-aluminum composite sheet are shown in Table 1.
[0045] Example 2
[0046] A copper-aluminum composite sheet was prepared according to the method of Example 1. Compared with Example 1, the difference of this embodiment is that in step 1), the thickness of the copper sheet is 4 mm, and the thickness of the aluminum sheet is 10 mm; in step 6), the number of rolling passes is 9 times, and the maximum pressing amount of a single rolling pass is 14.6% of the sheet thickness. The relevant performance results of the prepared copper-aluminum composite sheet are shown in Table 1.
[0047] Comparative Example 2
[0048] Compared with Example 2, the main difference of this comparative example is that when the copper-aluminum composite plates are assembled, the aluminum surface is centered. The relevant performance results of the prepared copper-aluminum composite thin plates are shown in Table 1.
[0049] Example 3
[0050] A copper-aluminum composite sheet was prepared according to the method of Example 1. Compared with Example 1, the difference of this embodiment is that in step 1), the thickness of the copper sheet is 4 mm, and the thickness of the aluminum sheet is 8 mm; in step 6), the number of rolling passes is 13 times, the maximum pressing amount of a single rolling pass is 14.5% of the sheet thickness, and the rolling speed is 10 m / min. The relevant performance results of the prepared copper-aluminum composite sheet are shown in Table 1.
[0051] Comparative Example 3
[0052] Compared with Example 3, the main difference of this comparative example is that when the copper-aluminum composite plates are assembled, the aluminum surface is centered. The relevant performance results of the prepared copper-aluminum composite thin plates are shown in Table 1.
[0053] Example 4
[0054] A copper-aluminum composite sheet was prepared according to the method of Example 1. Compared with Example 1, the main differences of this embodiment are: in step 1), the thickness of the copper plate is 6 mm, and the thickness of the aluminum plate is 10 mm; in step 6), the maximum pressing amount of a single rolling pass is 19.7% of the plate thickness, and the rolling speed is 15 m / min. The relevant performance results of the prepared copper-aluminum composite sheet are shown in Table 1.
[0055] Comparative Example 4
[0056] Compared with Example 4, the difference of this comparative example is that the number of rolling passes is 5, the maximum pressing amount of a single rolling pass is controlled to be 28.6% of the plate thickness, and other conditions remain unchanged. The relevant performance results of the obtained copper-aluminum composite sheet are shown in Table 1.
[0057] Example 5
[0058] A copper-aluminum composite sheet was prepared according to the method of Example 1. Compared with Example 1, the difference of this embodiment is that in step 1), the thickness of the copper sheet is 5 mm, and the thickness of the aluminum sheet is 14 mm; in step 6), the number of rolling passes is 11 times, the maximum pressing amount of a single rolling pass is 14.8% of the sheet thickness, and the rolling speed is 20 m / min. The relevant performance results of the prepared copper-aluminum composite sheet are shown in Table 1.
[0059] Comparative Example 5
[0060] Compared with Example 5, the main difference of this comparative example is that the rolling speed is 30 m / min. The relevant performance results of the obtained copper-aluminum composite sheet are shown in Table 1.
[0061] Table 1 Preparation process parameters and performance results of copper-aluminum composite sheets
[0062]
Claims
1. A method for preparing a copper-aluminum composite sheet, comprising the following steps: S1. Using explosive welding technology to perform explosive welding composite processing on aluminum plates and copper plates to obtain copper-aluminum composite blanks, and then leveling, testing, and cutting the copper-aluminum composite blanks to obtain qualified copper-aluminum composite plates; S2. Using the principle of rolling processing technology, the copper-aluminum composite plate obtained in step S1 is subjected to rolling and thinning treatment to obtain the desired copper-aluminum composite thin plate. The specific process is as follows: 1) Cold-cut the copper-aluminum composite plate, and then combine the two copper-aluminum composite plates of the same size and specifications back to back. The combination requires the copper side to be in the middle and the aluminum side to face outward, and the two copper sides to be close together. Then weld the edges around the outer side of the copper material in the middle, intermittently weld along the length direction, and fully weld in the width direction. All welds must be welded firmly and reliably; 2) The copper-aluminum composite plate assembled in step 1) is rolled according to set rolling process parameters. After rolling is completed, the weld is removed to obtain the copper-aluminum composite sheet.
2. The preparation method according to claim 1, characterized in that: In step S1, the material of the aluminum plate is pure aluminum or aluminum alloy, and the material of the copper plate is pure copper or copper alloy.
3. The preparation method according to claim 1, characterized in that: In step S1, the material of the aluminum plate is 1060 pure aluminum, and the material of the copper plate is T2 red copper.
4. The preparation method according to claim 1, characterized in that: In step S1, the aluminum plate is the base layer with a thickness of ≥7 mm; the copper plate is the cladding layer with a thickness of 3-8 mm.
5. The preparation method according to claim 1, characterized in that: Step S1 specifically includes the following steps: The surfaces of the aluminum plate and copper plate to be welded are pre-polished and cleaned to meet the requirements of the explosive composite process; The pretreated aluminum plate is placed horizontally on a flat foundation, and gap columns for explosive welding are evenly arranged along the edge and middle of the aluminum plate surface, and then the pretreated copper plate is placed on the gap columns, wherein the polished surface of the aluminum plate faces upward and the polished surface of the copper plate faces downward, and finally a protective layer is laid on the copper plate, and an explosive layer is laid on the protective layer and detonated by a detonator, and the explosion residue and the protective layer are removed to obtain a copper-aluminum composite billet; The prepared copper-aluminum composite billet is first leveled, and then an ultrasonic flaw detector is used to detect the bonding condition of the composite interface, and the poor bonding area is marked. The copper-aluminum composite sheet that passes the inspection is cut through mechanical cold working.
6. The preparation method according to claim 1, characterized in that: In step 1), conventional arc welding MAG welding is used to weld the outer edges of the middle copper material. The welding process parameters are: current 220-250A, voltage 29-30V, welding speed 12-15cm / min, shielding gas flow rate 15-20L / min, welding 100mm every 100mm along the length direction, and full welding in the width direction.
7. The preparation method according to claim 1, characterized in that: In step 2), the rolling is multiple small pressing rollings, and the rolling process parameters are: the maximum pressing amount of a single pass is controlled to be 5%-20% of the thickness of the copper-aluminum composite plate, the total deformation is controlled to be less than 80%, and the rolling processing speed is controlled within 20m / min.
8. A copper-aluminum composite sheet obtained according to the preparation method according to any one of claims 1 to 7.
9. The copper-aluminum composite sheet according to claim 8, characterized in that: The copper-aluminum composite thin plate adopts a layered composite connection structure and has a thickness of 3-8 mm, wherein the thickness of the copper plate is 1-3 mm and the thickness of the aluminum plate is 2-6 mm.
Citation Information
Patent Citations
Copper-aluminum explosion composite plate adapter
CN104057200A
Method for rolling copper-aluminum double-layer composite plate
CN104959382A
Method for smoothing continuous ply rolling of metal-based composite plates
CN108971226A
Method for preparing ultra-thin high-performance multilayer copper / copper-aluminum intermetallic compound / aluminum composite foil
CN109174965A
Method for preparing metal composite thin strip through pack rolling technology
CN113695393A