Method for regulating and controlling confinement space by using external pressure and application of method in construction of three-dimensional micro-nano structure

By controlling the confined space and special micro-templates through external pressure, the problem of difficulty in controlling the height of the assembly pattern of three-dimensional functional materials is solved, and the precise construction and performance improvement of three-dimensional micro-nano structures are achieved.

CN118723914APending Publication Date: 2024-10-01INST OF CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410716242.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing functional material patterning processing methods are difficult to accurately control the height of the assembly pattern in three-dimensional space, resulting in limited material performance.

Method used

By using external pressure to regulate the confined space, combined with a bubble generation system and a special "Y"-shaped micro-template, the assembly process of nanomaterials is controlled to achieve the precise construction of three-dimensional micro-nano structures. Specific steps include filling the bubble generation system with nanomaterial assembly liquid, applying pressure to form a patterned two-dimensional bubble array, and evaporating the solvent to assemble the nanomaterials to form a highly controllable microstructure array.

Benefits of technology

It achieves precise control of the assembly pattern height and improves the performance of functional materials, especially in the fields of optoelectronic devices and perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723914A_ABST
    Figure CN118723914A_ABST
Patent Text Reader

Abstract

The invention provides a method for regulating and controlling a confinement space by using external pressure and application of the method in construction of a three-dimensional micro-nano structure. According to the invention, uniform pressure can be applied by using an external weight in the bubble-assisted assembly process through the microstructure template, so that the three-dimensional height of the obtained pattern can be effectively controlled. According to the method, the problem that the height is difficult to control in the micro-template printing process can be solved, and more choices are provided for device application of a pattern array of subsequent micro-template printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of micro-nano processing and functional material assembly and patterning technology, and relates to a method for regulating a confined space by utilizing external pressure and its application in the construction of three-dimensional micro-nano structures, and specifically to a method for regulating the morphology of a liquid confined space in an assembly process by utilizing external pressure and controlling the height of an obtained assembly pattern. Background Art

[0002] In the process of patterning and preparing functional materials, the three-dimensional morphology of the processed pattern will significantly affect the material properties. For example, the three-dimensional stacking structure and morphology of nanoparticles will significantly affect the carrier transport channel and performance inside them; the pattern processing accuracy of conductive polymer materials will also significantly affect their quantum confinement effect, resulting in different electrical and thermal conductivity properties.

[0003] With the continuous advancement of micro-nano processing technology, a variety of solution processing methods have been used to achieve patterned processing and preparation of functional materials, such as inkjet printing, nanoimprinting, capillary bridge induction, dip pen printing and solution scraping, etc. The core of these processing methods to prepare micro-nano patterns is to control the wetting evolution behavior of droplets or solutions in micro-nano scale space, so as to accurately control the position and morphology of functional materials, thereby obtaining the corresponding functional material pattern.

[0004] However, the current patterning preparation methods focus on controlling the liquid behavior on a two-dimensional scale of functional materials. Although the above methods can obtain two-dimensional patterns of various functional materials, it is difficult to accurately control the height size of the assembled pattern in three-dimensional space. Summary of the invention

[0005] In order to improve the above technical problems, the present invention provides a method for regulating a confined space by using external pressure, comprising the following steps:

[0006] 1) The micro-template and the substrate with a flat surface are used as the lower substrate and the upper substrate respectively to form a bubble generation system;

[0007] 2) filling the bubble generation system with a nanomaterial assembly liquid containing tiny bubbles, and applying pressure on the upper substrate to form a patterned two-dimensional bubble array on the upper substrate through fusion of the tiny bubbles;

[0008] 3) removing the solvent in the nanomaterial assembly solution, and assembling the nanomaterial on the upper substrate using the patterned two-dimensional bubble array as a template to obtain a microstructure array (and the height of the pattern depends on the magnitude of the applied pressure).

[0009] According to an embodiment of the present invention, in step 2), the pressure applied is 40-4500 Pa, exemplified by 44.4 Pa, 444.4 Pa, 888.8 Pa, 1333.3 Pa, 1777.8 Pa, 2222.2 Pa, 2666.7 Pa, 3111.1 Pa, 3555.6 Pa, 4000.0 Pa, 4444.4 Pa. For example, the pressure may be applied by attaching a weight of a certain mass to the upper substrate, preferably to the center of the upper substrate, to ensure uniformity of the pressure on the entire upper substrate.

[0010] According to an embodiment of the present invention, the mass of the weight applying pressure can be 1-100g, preferably 10-50g, and exemplified by 1g, 10g, 20g, 30g, 40g, 50g, 60g, 70g, 80g, 90g, and 100g.

[0011] According to an embodiment of the present invention, the duration of externally applied pressure needs to cover the entire bubble assembly process. For example, the duration of applied pressure is about 2 to 10 hours. After the nanomaterial assembly liquid is completely dried, the pressure is stopped (the weight is removed), and the upper substrate is separated from the lower substrate so that a grid of assembly materials of a specific height can be obtained on the upper substrate.

[0012] According to an embodiment of the present invention, in step 3), the height of the microstructure array obtained is 50 to 1500 nm, preferably 200 to 500 nm, and exemplarily is 50 nm, 100 nm, 150 nm, 200 nm, 220 nm, 280 nm, 300 nm, 440 nm, 470 nm, 490 nm, 500 nm, 600 nm, 650 nm, 800 nm, 1000 nm, and 1500 nm.

[0013] According to an embodiment of the present invention, the micro-template is preferably a "Y"-shaped micro-template. In the present invention, the "Y"-shaped micro-template is defined as a two-dimensional array composed of the structural units shown in Figure 1 (a), that is, the structural units protrude from the template surface in a "Y" shape. Preferably, the array assembled from the "Y"-shaped micro-template includes but is not limited to a rectangular array, a hexagonal array, a triangular array, a parallelogram array, and other two-dimensional pattern arrays.

[0014] According to the embodiment of the present invention, the three angles in the structural unit of the "Y"-shaped micro-template are all 120°, and the length L and width D of each branch of the "Y"-shaped micro-template structural unit can be appropriately changed. For example: L can range from 1 to 100 μm (such as 15 μm); D can range from 1 to 100 μm (such as 5 μm). Generally speaking, L needs to be greater than D, but it can be adjusted according to specific needs.

[0015] According to an embodiment of the present invention, the periodic size of the structural unit array of the "Y"-shaped micro-template (in the present invention, the periodic size is defined as the center distance between two "Y"-shaped structural units) can be 1 to 1000 μm, for example, 50 μm.

[0016] According to an embodiment of the present invention, the height of the "Y"-shaped micro-template structure unit array is 1 to 100 μm (eg, 20 μm).

[0017] According to an embodiment of the present invention, in order to stably form a patterned two-dimensional bubble array, the volume fraction of bubbles in the nanomaterial assembly liquid containing tiny bubbles is 40-90%, preferably 60-85%. The size of the tiny bubbles is not particularly limited. Preferably, the diameter of the tiny bubbles is 100nm-100μm, preferably 2-100μm, and more preferably 10-60μm. Here, the volume fraction of bubbles in the nanomaterial assembly liquid containing tiny bubbles refers to the ratio of the gas volume to the total volume of the gas and the nanomaterial assembly liquid under the conditions of 25°C and 1 standard atmospheric pressure. In the physical method of generating tiny bubbles, the gas volume here refers to the volume of gas injected by physical methods; in the chemical method of generating tiny bubbles, the gas volume here refers to the volume of gas generated by chemical reactions. When calculating the volume fraction of bubbles, it is assumed that the solubility of the gas in the nanomaterial assembly liquid is zero.

[0018] In the present invention, the fusion of bubbles, which can also be referred to as the growth and evolution of bubbles, refers to the process in which small bubbles are gradually merged by large bubbles due to their different sizes, different interface curvature radii, different internal pressures, and different internal gas solubilities.

[0019] According to an embodiment of the present invention, the speed of the fusion process of the microbubbles can be controlled by temperature. The specific temperature can be appropriately selected according to needs, and can be specifically 5-50°C, preferably 10-30°C.

[0020] In the present invention, the process of removing the solvent from the nanomaterial assembly liquid refers to the process of removing the solvent from the bubble generation system by volatilization or the like. The nanomaterial assembly on the lower substrate using the patterned two-dimensional bubble array as a template refers to the process in which the nanomaterial precipitates and is deposited and assembled between bubbles as the solvent evaporates. The speed of the assembly process can be controlled by temperature, and the specific temperature can be appropriately selected as needed, specifically 5-50°C, preferably 20-30°C.

[0021] According to an embodiment of the present invention, the nanomaterial assembly liquid containing tiny bubbles is produced by a physical method or a chemical method.

[0022] According to an exemplary embodiment of the present invention, the physical method is one of ultrasonic bubbling, microporous plate bubbling, solution decompression to separate out air, and the like.

[0023] According to an exemplary embodiment of the present invention, the chemical method is a chemical reaction method capable of generating gas. For example, the chemical method is one or more selected from the group consisting of hydrolysis of borohydride (such as the method of generating bubbles by the reaction of sodium borohydride with acid), catalytic decomposition of hydrogen peroxide or urea peroxide (such as metal-catalyzed hydrogen peroxide), dimethylhydrazine, sodium azide foaming, and the like.

[0024] According to an embodiment of the present invention, for nanoparticles that can stably exist under acidic conditions, a hydrolysis reaction of borohydride (such as a method of generating bubbles by reacting sodium borohydride with acid) is suitable for generating bubbles.

[0025] According to an exemplary embodiment of the present invention, step 2) specifically includes the following steps:

[0026] a) dropping a sodium borohydride solution onto the surface of the Y-shaped micro-template on the lower substrate and then drying it;

[0027] b) dropping a solution containing acid and nanoparticles onto the surface of the upper substrate, and attaching the upper substrate to the lower substrate to generate bubbles through a rapid chemical reaction.

[0028] According to an embodiment of the present invention, in step a), the sodium borohydride solution is preferably an ethanol solution of sodium borohydride, and the concentration of the sodium borohydride solution is 0.1wt% to 0.6wt%, such as 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%.

[0029] According to an embodiment of the present invention, in step b), the acid can be selected from common acids such as hydrochloric acid and sulfuric acid. + ) has a concentration of 0.001 mol / L to 1.0 mol / L, exemplified by 0.001 mol / L, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, and 1 mol / L.

[0030] According to an embodiment of the present invention, in step b), the lamination may be performed by placing the upper substrate on the surface of the lower substrate, or by placing the lower substrate on the surface of the upper substrate.

[0031] According to an exemplary embodiment of the present invention, in step b), after lamination, sodium borohydride reacts with acid as follows to achieve rapid generation of bubbles: NaBH4+HCl+3H2O=B(OH)3+NaCl+4H2.

[0032] According to an embodiment of the present invention, in step b), the solution containing the acid and the nanoparticles further comprises a surfactant. The introduction of the surfactant can maintain the stability of the bubbles.

[0033] According to an embodiment of the present invention, for a nanoparticle system that cannot stably exist under acidic conditions, the catalytic decomposition of hydrogen peroxide or urea peroxide (such as metal-catalyzed hydrogen peroxide) is used to generate bubbles.

[0034] According to an exemplary embodiment of the present invention, step 1) specifically includes the following steps:

[0035] a') forming a metal layer on the surface of the Y-shaped micro-template of the lower substrate;

[0036] b') dropping a solution containing hydrogen peroxide and nanoparticles onto the surface of the upper substrate, and attaching the lower substrate to the upper substrate before the solution containing hydrogen peroxide and nanoparticles dries, thereby generating bubbles through a rapid chemical reaction.

[0037] According to an embodiment of the present invention, in step a'), a metal layer can be formed by spraying on the surface of the Y-shaped micro-template of the lower substrate by sputtering. Preferably, the metal is a metal that catalyzes the decomposition of hydrogen peroxide, such as Pt, Au or Pd.

[0038] In one embodiment of the present invention, the metal sputtering is performed using a SCD500 metal sputtering apparatus, the spraying time is 500 s, and the thickness of the metal layer is about 20 nm.

[0039] According to an embodiment of the present invention, in step b'), the mass fraction of hydrogen peroxide in the solution containing hydrogen peroxide and nanoparticles is 0.3% to 1.0%, exemplified by 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%.

[0040] According to an embodiment of the present invention, in step b'), the solution containing hydrogen peroxide and nanoparticles further comprises a surfactant.

[0041] According to an embodiment of the present invention, the selection of the surfactant needs to be based on the specific organic functional molecules. Generally, a surfactant with the same electrical properties as the nanoparticles is selected: when the nanoparticles are positively charged substances, a cationic surfactant needs to be selected, including but not limited to at least one of hexadecyltrimethylammonium bromide (CTAB) and triethylamine; when the nanoparticles are negatively charged substances, an anionic surfactant needs to be selected, including but not limited to at least one of sodium dodecyl sulfate (SDS) and sodium dodecylbenzene sulfonate.

[0042] According to an embodiment of the present invention, the concentration range of the surfactant is 0.05% to 0.5%, optimized to 0.1% to 0.2%, and exemplified by 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, and 0.5%.

[0043] According to an embodiment of the present invention, after the bubbles in the bubble generation system are generated, they need to be transferred to a low humidity environment (RH less than 10%) for dry assembly. For example, the duration of the dry assembly is about 2 to 10 hours (e.g., 5 hours), which may vary depending on the system.

[0044] According to the embodiment of the present invention, the substrate with a flat surface can be at least one of various common glass sheets (such as silicon sheets / silicon dioxide sheets), quartz, indium tin oxide glass (ITO glass), fluorine-doped tin oxide glass (FTO glass), ITO / polyethylene terephthalate (PET) film, ITO / polyethylene naphthalate (PEN) film or various polymer material substrates such as PET (polyethylene terephthalate), PI (polyimide), PDMS (polydimethylsiloxane), etc. It can be flexibly selected according to the substrate required for assembly printing.

[0045] According to an embodiment of the present invention, the material of the "Y"-shaped micro-template can be a silicon wafer, a silicon dioxide wafer, a metal wafer or PDMS (polydimethylsiloxane) with a microstructure.

[0046] According to an embodiment of the present invention, the nanomaterial assembly solution comprises nanomaterials and a solvent.

[0047] In order to better complete the assembly of the nanomaterial, the concentration of the nanomaterial in the assembly solution may be 10 to 100 mg / mL, and 100 mg / mL is exemplary.

[0048] According to the embodiment of the present invention, the type of the nanomaterial is not particularly limited and can be appropriately selected as needed. For example, the nanomaterial can be an electron transport material (such as titanium dioxide (TiO2), tin dioxide (SnO2), zinc oxide (ZnO), fullerene and [6,6]-phenyl C61 butyric acid methyl ester (PC61BM), etc.), a hole transport material (such as poly 3,4-ethylenedioxythiophene (PEDOT), poly 3,4-ethylenedioxythiophene / polystyrene sulfonate (PEDOT:PSS), poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (PTAA), poly (3 -hexylthiophene-2,5-diyl) (P3HT), [N,N-bis(4-methoxyphenyl)amino]spirobifluorene (Spiro-MeOTAD), phthalocyanine blue (CuPc), nickel oxide, molybdenum trioxide, cuprous iodide, etc., preferably poly 3,4-ethylenedioxythiophene / polystyrene sulfonate (PEDOT:PSS)) and other water-soluble organic functional molecules (such as water-soluble porphyrin molecules, water-soluble perylene diimide molecules, water-soluble azo molecules and partially water-soluble polymers) and the like at least one.

[0049] According to an embodiment of the present invention, the solvent can be various solvents conventionally used in the art. Preferably, the solvent is selected from one or more of water, methanol, ethanol, acetone, ethylene glycol, isopropanol, diethylene glycol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, ethylene glycol phenyl ether, ethylene glycol benzyl ether, furfuryl alcohol, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, triethylene glycol methyl ether, diacetone alcohol, tridecanol, tetradecanol, dioctyl phthalate, ethyl acetate, butyl acetate, cyclohexanone, xylene, bicyclohexane, cyclohexane, n-butanol, butanone, dimethyl phthalate and sorbitol.

[0050] The present invention also provides application of the above method in constructing three-dimensional micro-nano structures.

[0051] The invention also provides nanomaterials prepared by the method.

[0052] According to an embodiment of the present invention, the nanomaterial is in a three-dimensional micro-nano grid structure array. Preferably, the height of the three-dimensional micro-nano grid structure array is 50 to 1500 nm, preferably 200 to 500 nm, and exemplarily 50 nm, 100 nm, 150 nm, 200 nm, 220 nm, 280 nm, 300 nm, 440 nm, 470 nm, 490 nm, 500 nm, 600 nm, 650 nm, 800 nm, 1000 nm, and 1500 nm.

[0053] The present invention also provides the use of the nano material prepared by the above method in the preparation of transparent conductive films, perovskite solar cells and microfluidic chips.

[0054] The present invention also provides a method for preparing a perovskite solar cell, which includes the above-mentioned method of regulating the confined space by utilizing external pressure.

[0055] The present invention also provides a perovskite solar cell, wherein the electron transport layer and / or the hole transport layer are prepared by the above method.

[0056] According to an embodiment of the present invention, the perovskite solar cell structure includes an electron transport layer, an organic-inorganic composite perovskite thin film light absorption layer, a hole transport layer and a top electrode.

[0057] According to an embodiment of the present invention, the material of the organic-inorganic hybrid perovskite light-absorbing layer includes MAPbI3, MAPb(I x Cl 1-x )3.MAPb(I x Br 1-x )3.MAPb(I x Br y Cl 1-x-y 3. MA x FA 1-x PbI3 MA x FA 1-x Pb(I y Cl 1-y 3. MA x FA 1-x Pb(I x Br 1-x 3. MA x FA 1-x Pb(I x Br y Cl 1-x-y )3, one or more of FAPbI3, wherein: MA is methylamine cation, FA is formamidine cation, 0 <x<1,0<y<1,0<x+y<1。

[0058] According to an embodiment of the present invention, the top electrode may be a work function matching material, including but not limited to gold, silver, copper, calcium, barium, chromium, and the like.

[0059] In the present invention, the preparation process of the perovskite solar cell device: the selected layers can be coated layer by layer according to the device structure of substrate / hole transport layer / perovskite / electron transport layer / top electrode or substrate / electron transport layer / perovskite / hole transport layer / top electrode by using spin coating, scraping, spraying, wire rod coating, slit coating, screen printing, chemical vapor deposition, physical vapor deposition and the like; wherein the electron transport layer or hole transport layer in contact with the substrate is prepared according to the above method provided by the present invention.

[0060] The present invention also provides a method for preparing a transparent conductive film, which includes the above-mentioned method of regulating the confined space by utilizing external pressure.

[0061] The present invention also provides a transparent conductive film, which comprises the nano material prepared by the above method.

[0062] The present invention also provides a method for preparing a microfluidic chip, which includes the above-mentioned method of regulating the confined space by utilizing external pressure.

[0063] The present invention also provides a microfluidic chip, which comprises the nano material prepared by the above method.

[0064] Beneficial effects of the present invention:

[0065] (1) The present invention discloses a method for regulating the height of confined space and pattern assembly by using external pressure, so as to accurately control the height of the assembly pattern to be obtained, and help improve the performance of the device prepared by the assembly pattern. At the same time, based on the lattice micro-template, the present invention proposes a new micro-template pattern design strategy through reasonable geometric shape design, which can be applied to the bubble-assisted assembly process, and can evenly disperse the external pressure, which is conducive to controlling the shape of the confined space in the bubble-assisted assembly process, thereby regulating the height of the obtained assembly pattern, and finally obtaining an assembly pattern with controllable three-dimensional size.

[0066] (2) The present invention provides a method for regulating the height of confined space and pattern assembly by using external pressure. By using a specially designed new template array, the external pressure applied in the micro-template printing process can be effectively dispersed, and the height range of the obtained printed pattern can be effectively regulated, so as to solve the technical problem that it is difficult to accurately control the height of the obtained pattern or it is impossible to regulate the height of the pattern in the existing micro-template imprinting assembly and bubble printing process. The printed pattern with controllable height range prepared by the present invention can improve the application performance of subsequent devices.

[0067] (3) The method of the present invention can be used to prepare grid arrays of various electron transport materials (such as tin dioxide) and conductive polymer materials (such as PEDOT (polyethylene dioxythiophene-polystyrene sulfonate)) of different heights for application in the preparation of optoelectronic devices and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 (a) shows the schematic diagram of the structure of the micro-template "Y"-shaped structural unit; Figure 1 (b) shows the structure of the "Y"-shaped micro-template array, scale bar: 50μm; Figure 1(c) and (d) are schematic diagrams of the structure in which external pressure is applied during the assembly process and the relationship between the height of the tin dioxide grid array obtained in Example 2 and the applied pressure, respectively.

[0069] Figure 2 This is an optical photograph of bubble-assisted assembly using a "Y"-shaped micro-template. Figure 2 (a) Uniform bubble array obtained using a “Y”-shaped micro-template, scale bar: 50 μm; Figure 2 (b) shows the grid array in the “Y”-shaped micro-template after the solution has dried, scale bar: 50 μm.

[0070] Figure 3 It is a tin dioxide grid array obtained by bubble-assisted assembly using a "Y"-shaped micro-template. Among them: Figure 3 (a) is an optical microscope photo of a tin dioxide grid array, scale bar: 200 μm; Figure 3 (b) is a scanning electron micrograph of a tin dioxide grid, scale bar: 20 μm.

[0071] Figure 4 (a), (b), and (c) are atomic force microscopy characterization results of samples of different heights obtained by bubble-assisted assembly using a "Y"-shaped micro-template in Example 1.

[0072] Figure 5 (a) and (b) are conductive PEDOT grids of different heights obtained after applying different pressures of 5g and 20g during the bubble assembly process in Example 3, respectively.

[0073] Figure 6 The current-voltage curves of the perovskite solar cells prepared in Example 4 and Comparative Example 1. DETAILED DESCRIPTION

[0074] The present invention will be described in further detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0075] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0076] Example 1

[0077] A method for regulating a confined space by utilizing external pressure comprises the following steps:

[0078] (1) ITO glass was selected as the substrate for grid assembly. Before use, the ITO glass substrate was hydrophilized using a UV-ozone surface treatment device (SmartPlasma2 Pro, Plasma Technology, Germany) (treatment conditions: 100% power for 10 seconds).

[0079] (2) Add 20 μL of 0.1 mol / L hydrochloric acid and 8 μL of 50 mg / mL sodium dodecyl sulfate (SDS) solution to 160 μL of 150 mg / mL aqueous solution of tin dioxide nanoparticles (purchased from Thermo Fisher Scientific, catalog number MFCD0001124), add ultrapure water to a solution volume of 200 μL, and finally prepare a tin dioxide mixed assembly solution. The concentration of tin dioxide particles in the mixed assembly solution is 120 mg / mL, the concentration of hydrochloric acid is 0.01 mol / L, and the concentration of SDS is 2 mg / mL.

[0080] Take another 3.0 mg of sodium borohydride solid powder, add ethanol to 1.0 g, and perform ultrasonic treatment for 10 minutes to completely dissolve it, to obtain a sodium borohydride ethanol solution with a mass fraction of 0.3 wt%. Filter the solution with a 0.45 μm organic filter membrane before use.

[0081] Apply 5 μL of the prepared sodium borohydride ethanol solution on Figure 1 In the "Y"-shaped micro-template shown in the figure (purchased from the School of Information Science and Technology of Peking University, made of silicon wafers processed by photolithography technology, D is 5μm, L is 15μm), 5μl of the tin dioxide mixed assembly solution is dropped on the ITO substrate. After the sodium borohydride solution is completely dried, the ITO substrate is contacted with the "Y"-shaped micro-template, and bubbles are generated by the reaction of sodium borohydride and dilute hydrochloric acid to deposit tin dioxide nanoparticles on the ITO substrate in a patterned manner.

[0082] (3) After the cover sheet is foamed, different pressures are applied to different assembled samples by weights of 30 g, 40 g, and 50 g in sequence on the top of the ITO substrate (e.g. Figure 1 (as shown in (c)).

[0083] (4) Leave it to stand for 6 hours in an environment with a humidity of less than 10% until the solvent evaporates completely, then remove the template to obtain the following Figure 3 The tin dioxide micro-nanostructure array shown (during the bubble assembly process, the assembly solution will be squeezed to the boundary of the "Y"-shaped micro-template and build a connected stable liquid bridge between the two "Y"-shaped micro-templates; therefore, a continuous hexagonal grid array can be obtained after drying).

[0084] The height of the SnO2 micro-nanostructure array prepared in this embodiment was tested using an atomic force microscope (Bruker). The results are as follows: Figure 4 It can be seen from the figure that: using a 30g weight to apply pressure corresponds to a 470nm high tin dioxide array, using a 40g weight to apply pressure corresponds to a 300nm high tin dioxide array, and using a 50g weight to apply pressure corresponds to a 220nm high tin dioxide array.

[0085] Example 2

[0086] A method for regulating a confined space by utilizing external pressure comprises the following steps:

[0087] (1) ITO glass was selected as the substrate for grid assembly. Before use, the ITO glass substrate was hydrophilized using a UV-ozone surface treatment device (SmartPlasma2 Pro, Plasma Technology, Germany) (treatment conditions: 100% power for 10 seconds).

[0088] (2) Add 4 μL of 30 wt% hydrogen peroxide (H2O2) solution and 8 μL of 50 mg / mL sodium dodecyl sulfate (SDS) solution to 160 μL of 150 mg / mL aqueous solution of tin dioxide nanoparticles (purchased from Thermo Fisher Scientific, catalog number MFCD0001124), and add ultrapure water to a total volume of 200 μL to prepare a tin dioxide mixed assembly solution. The concentration of tin dioxide particles in the mixed assembly solution is 120 mg / mL, the concentration of hydrogen peroxide is 0.6 wt%, and the concentration of SDS is 2 mg / mL.

[0089] Using SCD500 metal sputtering instrument Figure 1 A metal Pt layer is sprayed on the surface of the micro-template shown in the figure. The spraying time is 500s and the thickness is about 20nm.

[0090] 5 μl of the tin dioxide mixed assembly solution was dropped onto the ITO substrate. The ITO substrate was placed in contact with a "Y"-shaped micro-template, and the decomposition reaction of hydrogen peroxide was catalyzed by platinum metal to generate bubbles, and the tin dioxide nanoparticles were patterned and deposited on the ITO substrate.

[0091] (3) After the cover sheet is foamed, different pressures are applied to different assembled samples by weights of 20 g, 30 g, 40 g, and 50 g on the top of the template in sequence.

[0092] (4) Standing for 6 hours in an environment with a humidity of less than 10% and after the solvent is completely evaporated, removing the template to obtain a tin dioxide micro-nanostructure array.

[0093] The height of the SnO2 micro-nano structure array obtained in this embodiment was tested using a step profiler. The heights of the SnO2 micro-nano structure array obtained under different applied pressures are shown in FIG. Figure 1 As shown in (d). It can be seen from the figure that the height of the tin dioxide micro-nanostructure array obtained without applying pressure with a weight is about 1.588μm (0g); the tin dioxide micro-nanostructure array with an average height of about 650nm is obtained under the pressure applied by a 20g weight; the tin dioxide micro-nanostructure array with an average height of about 490nm is obtained under the pressure applied by a 30g weight; the tin dioxide micro-nanostructure array with an average height of about 440nm is obtained under the pressure applied by a 40g weight; and the tin dioxide micro-nanostructure array with an average height of about 280nm is obtained under the pressure applied by a 50g weight.

[0094] Example 3

[0095] A method for regulating a confined space by utilizing external pressure comprises the following steps:

[0096] (1) Ordinary glass substrates are selected as assembly substrates. Before use, they need to be ultrasonically cleaned with acetone, water, and isopropanol. Then, they are blown dry with high-purity nitrogen.

[0097] (2) Weigh 3.0 mg of sodium borohydride (NaBH4) powder, add ethanol to 1.0 g, and dissolve it by ultrasonication to obtain a sodium borohydride ethanol solution with a mass fraction of 0.3 wt%. Filter the solution with a 0.45 μm organic filter membrane before use.

[0098] Sodium dodecyl sulfate (SDS) solution was added to PEDOT:PSS solution (purchased from Heraeus, model: Clevios PH1000) to prepare PEDOT assembly solution. The concentration of PEDOT:PSS in the assembly solution was 8 mg / mL, and the concentration of SDS was 2 mg / mL.

[0099] Use a pipette to take 3 μL of the prepared sodium borohydride ethanol solution and apply it dropwise to the Figure 1 The template shown in (purchased from the School of Information Science and Technology, Peking University, made of silicon wafers processed by photolithography technology, D is 5μm, L is 15μm) was placed on the glass substrate, and then 3μL of the prepared PEDOT assembly solution was dropped on the glass substrate using a pipette. The glass substrate was carefully turned over and placed on the template with sodium borohydride droplets to form a sandwich foaming assembly structure.

[0100] (3) Place 5g and 20g weights on top of the sandwich structure, and keep the ambient humidity stable below 10% RH for dry assembly. After the entire assembly structure is completely dry (about 6 hours), remove the weights and carefully separate the substrate and the assembly template to obtain PEDOT grids of different heights.

[0101] The height of the PEDOT micro-nano structure array obtained in this embodiment was tested using a step profiler. The heights of the PEDOT micro-nano structure array obtained under different applied pressures are shown in FIG. Figure 5 It can be seen from the figure that when the external pressure is 5g weight, the height of the PEDOT grid is about 460nm; when the external pressure is 20g weight, the height of the PEDOT grid is about 320nm.

[0102] Example 4

[0103] The preparation method of perovskite solar cell comprises the following steps:

[0104] ITO glass was selected as the substrate: the ITO substrate was cleaned in a UV-ozone cleaning machine for 30 minutes. Then 10 μL of 100 mg / ml tin dioxide nanoparticle aqueous solution (purchased from Thermo Fisher Scientific, catalog number MFCD0001124) was added with hydrochloric acid until the hydrogen ion concentration was 0.01 mol / L, and the solution was dripped onto the cleaned ITO substrate. Figure 1 The template shown is pre-coated with 0.3wt% sodium borohydride ethanol solution. After the template is covered on the substrate with tin dioxide solution, the bubbles generated by the reaction of sodium borohydride and dilute hydrochloric acid are used to deposit tin dioxide nanoparticles on the ITO substrate in a patterned manner. Different pressures are applied on the top of the template by weights of 30g, 40g, and 50g in sequence, and tin dioxide micro-nanostructure arrays with different heights can be obtained. After that, wait for 6 hours in an environment with a humidity of less than 10%. After the solvent is completely evaporated, remove the template to obtain the following Figure 3 The tin dioxide micro-nanostructure array shown. The obtained array was annealed at 150°C for two hours. After annealing, wait for cooling to room temperature, spin coat 50μL of 1.5mol / L MAPbI3 solution (solvent DMF:DMSO=8:2) (spin coating speed is 5000 rpm, time is 30 seconds) on the tin dioxide micro-nanostructure array, and then annealed at 100°C for 15 minutes. After cooling to room temperature, 20μL of 20mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) chlorobenzene solution was spin coated at 5000 rpm for 30 seconds on top of the perovskite layer. Finally, the perovskite layer was prepared by physical vapor deposition method (vacuum degree less than 10 -5In an environment of Pa, 100 nm thick gold was deposited on the PTAA layer to obtain the desired perovskite solar cell.

[0105] Comparative Example 1

[0106] The method for preparing a perovskite solar cell is different from that of Example 4 in that the tin dioxide micro-nanostructure array is replaced by a tin dioxide film.

[0107] Wherein: the tin dioxide film is prepared by spin coating 30 μL of a 50 mg / mL aqueous solution of tin dioxide nanoparticles (purchased from Thermo Fisher Scientific, catalog number 44592) on an ITO substrate at a speed of 4000 rpm for 30 seconds, and annealing the obtained film at 150°C for two hours. After the annealing is completed, the film is cooled to room temperature to obtain a tin dioxide film.

[0108] The preparation methods of the remaining layers are the same as those in Example 4.

[0109] The current-voltage curves of the perovskite solar cells prepared in Example 4 and Comparative Example 1 are as follows: Figure 6 As shown. From the results in the figure, it can be seen that compared with the tin dioxide film without micro-nano structure as the electron transport layer (Comparative Example 1), the photoelectric conversion efficiency of the perovskite solar cell is increased from 21.20% to 22.40% after using the electron transport layer of the 220nm high micro-nano structure tin dioxide array; the photoelectric conversion efficiency of the perovskite solar cell is increased to 23.24% after using the 300nm high micro-nano structure tin dioxide array electron transport layer; after using the 470nm high micro-nano structure tin dioxide array electron transport layer, due to the leakage effect caused by the excessively high height of the tin dioxide array, the photoelectric conversion efficiency of the perovskite solar cell drops to 18.63%.

[0110] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for regulating a confined space by using external pressure, characterized in that: The steps include: 1) The micro-template and the substrate with a flat surface are used as the lower substrate and the upper substrate respectively to form a bubble generation system; 2) filling the bubble generation system with a nanomaterial assembly liquid containing tiny bubbles, and applying pressure on the upper substrate to form a patterned two-dimensional bubble array on the upper substrate through fusion of the tiny bubbles; 3) removing the solvent in the nanomaterial assembly solution, and assembling the nanomaterial on the upper substrate using the patterned two-dimensional bubble array as a template to obtain a microstructure array.

2. The method according to claim 1, characterized in that In step 2), the pressure applied is 40 to 4500 Pa. Preferably, the pressure is applied by adhering a weight of a certain mass to the upper substrate, preferably at the center of the upper substrate. Preferably, the mass of the weight applying the pressure is 1 to 100 g, preferably 10 to 50 g. Preferably, in step 3), the height of the microstructure array is 50 to 1500 nm, preferably 200 to 500 nm. Preferably, the micro-template is preferably a "Y"-shaped micro-template. Preferably, the arrays assembled from the "Y"-shaped micro-templates include but are not limited to rectangular arrays, hexagonal arrays, triangular arrays, parallelogram arrays, and other two-dimensional pattern arrays. Preferably, the three angles in the structural unit of the "Y"-shaped micro-template are all 120°, the structural length L may be in the range of 1 to 100 μm, and the width D may be in the range of 1 to 100 μm. Preferably, the height of the "Y"-shaped micro-template structure unit array is 1 to 100 μm.

3. Application of the method according to any one of claims 1 to 2 in the construction of three-dimensional micro-nano structures.

4. A nanomaterial prepared by the method according to any one of claims 1 to 2. Preferably, the nanomaterial is in a three-dimensional micro-nano grid structure array. Preferably, the height of the three-dimensional micro-nano grid structure array is 50 to 1500 nm, preferably 200 to 500 nm.

5. Application of the nanomaterial prepared by the method according to any one of claims 1 to 2 in the preparation of transparent conductive films, perovskite solar cells, and microfluidic chips.

6. A method for preparing a perovskite solar cell, characterized in that: It includes the method for regulating a confined space by utilizing external pressure as described in any one of claims 1-2.

7. A perovskite solar cell, characterized in that: The electron transport layer and / or hole transport layer is prepared by the method described in any one of claims 1-2. Preferably, the perovskite solar cell structure includes an electron transport layer, an organic-inorganic composite perovskite thin film light absorption layer, a hole transport layer and a top electrode.

8. A method for preparing a transparent conductive film, characterized in that: It includes the method for regulating a confined space by utilizing external pressure as described in any one of claims 1-2.

9. A transparent conductive film, characterized in that: The transparent conductive film comprises a nanomaterial prepared by the method according to any one of claims 1 to 2.

10. A microfluidic chip, characterized in that: The microfluidic chip comprises nanomaterials prepared by the method according to any one of claims 1-2.

Citation Information

Cited By

  • Quantum dot-based light-emitting micro device and transient emulsion method sequential preparation method thereof

    CN119546145A