Seed layer structure for enabling HF to penetrate thin silicon layer to etch SiO2 and preparation method of seed layer structure
By using custom patterned metal layers and HF dry etching technology in MEMS technology, the problem of traditional SiO2 etching requiring through-hole etching is solved, and SiO2 etching under thin layers of silicon is achieved without damaging the integrity and sealing It improves product performance and test accuracy.
Patent Information
- Application Number
- CN202410909035.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional MEMS technology requires etching through holes when etching SiO2 under a thin layer of silicon, which affects the integrity and sealing of the thin layer of silicon and increases the difficulty of the process.
Using a seed layer structure of an upper metal layer, a lower metal layer, a thin layer of silicon and a SiO2 layer arranged in sequence from top to bottom, a custom patterned metal layer is formed through the MEMS etching process, and is subjected to high-temperature annealing treatment, combined with HF dry etching. Etching technology is used to form an etching cavity to achieve SiO2 etching, avoiding the need to etch through holes.
It realizes the SiO2 etching under the thin layer of silicon without etching through holes, ensuring the integrity of the thin layer of silicon and the sealing of the etching cavity, improving the performance reliability and test accuracy of the product, and the process flow It is simple, easy to operate and has good application prospects.
Smart Images

Figure CN118723919A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the MEMS technical field and particularly relates to a SiO 2 Etching technology, specifically a method for HF to penetrate thin silicon layers to etch SiO 2 A seed layer structure and a preparation method thereof. Background Art
[0002] Currently, SiO2 is commonly used in the field of MEMS technology. 2 Etching techniques include wet etching, dry etching, laser etching, etc. Wet etching mainly uses HF-containing liquid to 2 The components undergo corrosion reaction; dry etching mainly includes reactive ion etching (RIE), ion beam etching (IBE), and HF gas etching; laser etching mainly uses laser to interact with the target material through quartz glass to generate plasma to etch the bottom surface of the glass. Among the above methods, HF gas etching is an isotropic glass etching process with equal etching speed in each direction and a smooth interface.
[0003] In traditional MEMS technology, SiO2 under thin silicon layer 2 When etching, it is usually necessary to make SiO 2 Exposure to etchants usually destroys the integrity of thin silicon layers. Some structures that require sealed chambers usually need to be sealed again after etching. These complex processes increase the difficulty of the overall process and affect the final results. Summary of the invention
[0004] The purpose of this invention is to solve the problem of traditional MEMS technology on SiO2 under thin silicon layer. 2 The problem of etching through holes during etching is solved, and a method for HF to penetrate thin silicon layer to etch SiO 2 The seed layer structure and preparation method thereof. The seed layer structure can be customized in shape and does not require etching of through holes to complete the SiO 2 Etching.
[0005] The present invention is achieved through the following technical solutions: A method for HF to penetrate thin silicon layers and etch SiO 2 The seed layer structure includes an upper metal layer, a lower metal layer, a thin layer of silicon and SiO 2 The upper metal layer and the lower metal layer are custom pattern metal layers formed by MEMS etching process, the shapes of the two are consistent, and they are processed by high temperature annealing process; the thin layer of silicon is ion doped by MEMS diffusion process; SiO 2An etching cavity is formed on the layer by HF dry etching technology, and the position of the etching cavity corresponds to the positions of the upper metal layer and the lower metal layer, and the shape is also consistent.
[0006] As a preferred technical solution, the upper metal layer is a gold layer, and the lower metal layer is a chromium layer.
[0007] As a preferred technical solution, the thickness of the gold layer is 100-500 nm, and the thickness of the chromium layer is 10-100 nm.
[0008] As a preferred technical solution, the thickness of the gold layer is 300 nm, and the thickness of the chromium layer is 30 nm.
[0009] As a preferred technical solution, the thin layer of silicon is doped with boron ions through a MEMS diffusion process.
[0010] Furthermore, the above-mentioned HF is used to penetrate the thin silicon layer to etch SiO 2 The method for preparing a seed layer structure comprises the following steps: 1) Take the upper layer as a thin layer of silicon and the lower layer as SiO 2 The devices in the layer are reserved.
[0011] 2) Boron ion doping of the device's thin silicon layer is performed through the MEMS diffusion process.
[0012] 3) Magnetron sputtering is performed on the upper surface of the thin silicon layer through a MEMS coating process to form a metal layer with a chromium layer at the bottom and a gold layer at the top.
[0013] 4) Coat a layer of photoresist on the metal layer, use photolithography technology to transfer the mask pattern to the photoresist, use the photoresist pattern as a mask, and use MEMS etching process to etch the unmasked area of the metal layer to form a custom pattern metal layer.
[0014] 5) Perform high temperature annealing process on the custom graphic metal layer.
[0015] 6) HF dry etching technology is used to etch SiO through the custom pattern metal layer and thin layer silicon 2 The layer is dry-etched and finally the SiO 2 An etched cavity is formed on the layer.
[0016] As a preferred technical solution, in the above preparation method, when boron ions are doped, the doping temperature is 400° C. and the doping time is 30 minutes.
[0017] As a preferred technical solution, in the above preparation method, during high temperature annealing, the high temperature annealing temperature is 400° C. and the high temperature annealing time is 30 minutes.
[0018] The seed layer structure of the present invention realizes the SiO2 When etching, there is no need to etch through holes, and SiO 2 Etching is carried out to ensure the integrity of the thin layer of silicon and the sealing of the etching chamber, and the shape of the etching chamber is customized according to actual requirements, which greatly improves the performance reliability and test accuracy of the product.
[0019] The seed layer structure and preparation method of the present invention are scientific and reasonable, the process flow is simple, easy to operate, the manufacturing process has excellent consistency, and high integration can be achieved. At the same time, the cost is relatively low and it is easy to mass produce. Compared with the existing technology, the present invention is more attractive and has broad and good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 Schematic diagram of the seed layer structure of the present invention.
[0022] Figure 2 The figure is a flow chart of the preparation process of the seed layer structure of the present invention.
[0023] In the figure: 1-upper metal layer, 2-lower metal layer, 3-thin layer of silicon, 4-SiO 2 Layer, 5-etching cavity. DETAILED DESCRIPTION
[0024] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0025] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. Example 1
[0026] This embodiment provides a method for HF to penetrate a thin silicon layer and etch SiO 2 The seed layer structure, such as Figure 1 As shown, it includes an upper metal layer 1, a lower metal layer 2, a thin layer of silicon 3 and SiO 2 Layer 4; wherein the upper metal layer 1 and the lower metal layer 2 are custom pattern metal layers formed by MEMS etching process, the shapes of the two are consistent, and they are processed by high temperature annealing process; the thin layer silicon 3 is ion doped by MEMS diffusion process; SiO 2 An etching cavity 5 is formed on the layer 4 by HF dry etching technology. The position of the etching cavity 5 corresponds to the positions of the upper metal layer 1 and the lower metal layer 2 and the shapes are also consistent.
[0027] Specifically, the upper metal layer 1 is a gold layer, and the lower metal layer 2 is a chromium layer; the thickness of the gold layer is 100-500nm, and preferably 300nm; the thickness of the chromium layer is 10-100nm, and preferably 30nm.
[0028] Specifically, the thin silicon layer 3 is doped with boron ions through a MEMS diffusion process. Example 2
[0029] This embodiment provides the method for HF to penetrate thin silicon layer and etch SiO 2 The method for preparing a seed layer structure comprises the following steps: 1) Take the upper layer as a thin layer of silicon 3 and the lower layer as SiO 2 Layer 4 devices are reserved, such as Figure 2 As shown in A.
[0030] 2) Boron ion doping is performed on the thin silicon 3 of the device through the MEMS diffusion process, the doping temperature is 400°C, and the doping time is 30 minutes. Figure 2 As shown in B.
[0031] 3) magnetron sputtering is performed on the upper surface of the thin silicon layer 3 through a MEMS coating process to form a metal layer with a lower layer of chromium and an upper layer of gold.
[0032] 4) Coat a layer of photoresist on the metal layer, transfer the mask pattern to the photoresist using photolithography technology, use the photoresist pattern as a mask, and use the MEMS etching process to etch the unmasked area of the metal layer to form a custom pattern metal layer, such as Figure 2 As shown in C.
[0033] 5) The custom graphic metal layer is subjected to a high temperature annealing process, the high temperature annealing temperature is 400°C, and the high temperature annealing time is 30 minutes.
[0034] 6) Through the HF dry etching technology, the custom pattern metal layer and thin layer of silicon 3 to SiO 2 Layer 4 is dry-etched, and finally the SiO 2 An etching cavity 5 is formed on the layer 4, such as Figure 2 As shown in D.
[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A seed layer structure for HF penetrating thin silicon layer to etch SiO2, characterized in that: It includes an upper metal layer, a lower metal layer, a thin layer of silicon and a SiO2 layer arranged in sequence from top to bottom; wherein the upper metal layer and the lower metal layer are custom pattern metal layers formed by a MEMS etching process, the shapes of the two are consistent, and they have been processed by a high-temperature annealing process; the thin layer of silicon has been ion-doped by a MEMS diffusion process; an etching cavity is formed on the SiO2 layer by HF dry etching technology, and the position of the etching cavity corresponds to the positions of the upper metal layer and the lower metal layer and the shape is also consistent.
2. The seed layer structure for etching SiO2 by HF penetrating thin silicon layer according to claim 1, characterized in that: The upper metal layer is a gold layer, and the lower metal layer is a chromium layer.
3. The seed layer structure for etching SiO2 by HF penetrating thin silicon layer according to claim 2, characterized in that: The thickness of the gold layer is 100-500 nm, and the thickness of the chromium layer is 10-100 nm.
4. The seed layer structure for etching SiO2 by HF penetrating thin silicon layer according to claim 3, characterized in that: The thickness of the gold layer is 300 nm and the thickness of the chromium layer is 30 nm.
5. The seed layer structure for etching SiO2 by HF penetrating thin silicon layer according to claim 4, characterized in that: The thin silicon layer is doped with boron ions through a MEMS diffusion process.
6. The method for preparing a seed layer structure for etching SiO2 by HF penetrating a thin silicon layer as claimed in claim 5, characterized in that: The steps include: 1) Take the device with a thin silicon layer on the upper layer and a SiO2 layer on the lower layer for later use; 2) Boron ion doping of thin silicon layers of the device through MEMS diffusion process; 3) magnetron sputtering is performed on the upper surface of the thin silicon layer through a MEMS coating process to form a metal layer with a chromium layer at the bottom and a gold layer at the top; 4) Coat a layer of photoresist on the metal layer, transfer the mask pattern to the photoresist using photolithography technology, use the photoresist pattern as a mask, and use the MEMS etching process to etch the unmasked area of the metal layer to form a custom pattern metal layer; 5) Perform high temperature annealing process on the custom graphic metal layer; 6) The SiO2 layer is dry-etched through the custom patterned metal layer and the thin layer of silicon by HF dry etching technology, and finally an etching cavity is formed on the SiO2 layer.
7. The method for preparing a seed layer structure for etching SiO2 by HF penetrating a thin silicon layer according to claim 6, characterized in that: When boron ions are doped, the doping temperature is 400°C and the doping time is 30 minutes.
8. The method for preparing a seed layer structure for etching SiO2 by HF penetrating a thin silicon layer according to claim 6, characterized in that: During high temperature annealing, the high temperature annealing temperature is 400°C and the high temperature annealing time is 30 minutes.